Two-component epoxy pouring sealant for capacitor pouring and bonding and preparation method thereof

By adding rubber copolymer toughening agent and composite thermal flame retardant to the capacitor potting glue, a two-component epoxy potting glue that is resistant to high and low temperatures and aging resistance is prepared, which solves the thermal conductivity and resistance of capacitor potting glue at high temperatures. The problem of insufficient combustion performance significantly reduces the risk of temperature rise and thermal runaway, and improves the service life of the capacitor.

CN118895095APending Publication Date: 2024-11-05BEIJING COMENS NEW MATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411324201.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing capacitor potting glues lack thermal conductivity and flame retardant properties at high temperatures, resulting in reduced performance of insulating materials and risk of thermal runaway control, and lack of products that are resistant to aging.

Method used

Develop a two-component epoxy potting adhesive for capacitor potting heat dissipation and flame retardant. By combining components A and components B, rubber copolymer toughening agent and composite thermal flame retardant are added to prepare high and low temperature resistance and Aging-resistant thermally conductive and flame-retardant epoxy potting adhesive.

Benefits of technology

It significantly reduces the temperature rise of the capacitor, improves the resistance to high and low temperature shock and aging resistance, and is suitable for the capacitor potting industry, extends the service life and reduces the risk of thermal runaway.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005054934100000071
    Figure BDA0005054934100000071
  • Figure BDA0005054934100000081
    Figure BDA0005054934100000081
  • Figure BDA0005054934100000082
    Figure BDA0005054934100000082
Patent Text Reader

Abstract

The invention discloses a double-component epoxy pouring sealant for potting heat dissipation and flame retardance of a capacitor and a preparation method of the double-component epoxy pouring sealant, and belongs to the field of preparation of pouring sealants. The pouring sealant comprises a component A and a component B in a mass ratio of 100: 30, wherein the component A is a main agent and comprises modified epoxy resin, a diluent, a coupling agent, a defoaming aid, a composite heat-conducting flame retardant and a rubber copolymer flexibilizer; the component B is a curing agent and comprises modified anhydride, an accelerant, a composite heat-conducting flame retardant and a rubber copolymer toughening agent. The epoxy pouring sealant has the advantages of high heat conductivity, excellent flame retardance, long room-temperature operable time, high mechanical strength and the like, and is suitable for multiple industries such as electronic and electric appliances, insulating materials, adhesives, composite materials and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of potting adhesive preparation, and in particular to a two-component epoxy potting adhesive for capacitor potting and bonding and a preparation method thereof. Background Art

[0002] As an important part of the power industry, capacitors have been developed rapidly in recent years with the strong support of national policies. They have the advantages of long cycle life, high insulation resistance, excellent frequency characteristics, and low environmental pollution. With the continuous advancement of technology, capacitors are developing in the direction of large capacity, miniaturization, high power integration, etc., and higher requirements are put forward for the heat dissipation and flame retardant performance of equipment. During the operation of capacitors, high temperature will reduce the electrical properties, mechanical properties and service life of insulating materials and easily cause thermal runaway. Therefore, the heating and combustion control of capacitors is one of the key issues that need to be solved in the development of modern capacitor technology. The development of high-performance thermal conductive / flame retardant materials can not only improve the thermal conductivity and flame retardant ability of the capacitor insulation structure, but also improve its insulation system, reduce the temperature rise and loss of capacitors, and enhance its flame retardant performance. It is one of the research hotspots of electrical systems at home and abroad today.

[0003] As an intrinsic component of the above-mentioned insulating devices, the performance of potting glue is closely related to the performance of the devices. Therefore, it is imperative to conduct relevant analysis on capacitors and develop high-quality flame-retardant thermal conductive potting glue for capacitors. At present, thermal conductive / flame-retardant potting glue can be mainly divided into two types: epoxy type and polyurethane type. Among them, although polyurethane thermal conductive / flame-retardant potting glue has the advantages of adjustable hardness, high elasticity, and high impact resistance, its mechanical strength is low, its temperature resistance is poor, and its flame retardant effect is sometimes poor; epoxy thermal conductive / flame-retardant potting glue has good double 85 resistance, high electrical performance, and excellent temperature resistance. Therefore, the use of improved epoxy thermal conductive / flame-retardant potting glue in the field of capacitors is more common. In view of the fact that there are no potting glue products with extremely reliable thermal conductive / flame-retardant / aging resistance on the market, it is very necessary to develop such products.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy and a preparation method thereof, thereby solving the above-mentioned technical problems existing in the prior art. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy and a preparation method thereof can improve thermal conductivity, flame retardancy and flexibility to meet the heat dissipation, flame retardancy and aging resistance requirements of capacitors, thereby solving the above-mentioned technical problems existing in the prior art.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] A two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy, comprising: component A and component B in a mass ratio of 100:30; wherein:

[0008] In parts by mass, the component A comprises 30 to 40 parts of modified epoxy resin, 3 to 5 parts of diluent, 1 to 2 parts of difunctional polyether polyol, 1 to 4 parts of coupling agent, 0.05 to 1 part of defoaming aid, 0.1 to 1 part of color paste, 1 to 5 parts of rubber copolymer toughening agent, and 40 to 50 parts of composite thermal conductive flame retardant;

[0009] In terms of parts by mass, the B component comprises 70 to 80 parts of modified acid anhydride, 1 to 10 parts of amine accelerator, 1 to 5 parts of rubber copolymer toughening agent, and 5 to 10 parts of composite thermal conductive flame retardant.

[0010] A method for preparing the two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to the present invention comprises the following steps:

[0011] Preparation of component A: taking the raw materials of component A according to the formula of the present invention, adding the modified epoxy resin, phenolic diluent and difunctional polyether polyol in the raw materials into a reaction kettle in sequence, stirring at medium speed for 0.5 to 1 hour at 60 to 70° C. until the solid is completely dissolved, then adding the coupling agent and defoaming aid into the reaction kettle in sequence, stirring at low speed for 0.5 to 1 hour at 60 to 70° C. to mix the liquid raw materials evenly, then adding the color paste, rubber copolymer toughening agent and composite thermal conductive flame retardant in sequence, vacuuming and stirring at high speed for 1 to 2 hours at 50 to 60° C., and thus obtaining component A with toughening, thermal conductive and flame retardant properties;

[0012] Preparation of component B: taking the raw materials of component B according to the formula of the present invention, adding the modified anhydride and amine accelerator in the raw materials into another reaction kettle in turn, stirring at medium speed at 90-100° C. for 1-1.5 hours until the solid is completely dissolved, then adding the rubber copolymer toughening agent and the composite thermal conductive flame retardant into the reaction kettle in turn, vacuuming and stirring at high speed at 70-80° C. for 1-2 hours to obtain component B with toughening, thermal conductive and flame retardant properties;

[0013] The component A and the component B prepared above are combined in a mass ratio of 100:30 to obtain a two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy.

[0014] Compared with the prior art, the two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy provided by the present invention and its preparation method have the following beneficial effects:

[0015] By adding rubber copolymer toughening agent and composite thermal conductive flame retardant to both component A and component B, a thermal conductive flame retardant epoxy potting adhesive that is resistant to high and low temperature impact and resistant to double 85 aging is made, which can well meet the requirements of capacitor potting heat dissipation and flame retardancy. Through experimental verification, it is known that in the temperature rise experiment of the 50Ah capacitor using this potting heat dissipation and flame retardant epoxy potting adhesive at a 2C cycle rate, the maximum temperature is reduced by 10°C, and the cooling effect is obvious; in the high and low temperature impact experiment at -40 to 85°C, no cracking is observed after more than 1,500 cycles, and the aging resistance effect is obvious. Due to its many advantages mentioned above, this potting adhesive is suitable for the capacitor potting industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0017] Figure 1 This is a temperature rise curve of a capacitor potted with a two-component epoxy potting adhesive provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0018] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0019] First, the terms that may be used in this article are explained as follows:

[0020] The term “and / or” means that either or both of them can be realized at the same time. For example, X and / or Y means both “X” or “Y” and “X and Y”.

[0021] The terms "include", "comprises", "contains", "has" or other descriptions with similar semantics should be interpreted as non-exclusive inclusion. For example, including certain technical feature elements (such as raw materials, components, ingredients, carriers, dosage forms, materials, dimensions, parts, components, mechanisms, devices, steps, procedures, methods, reaction conditions, processing conditions, parameters, algorithms, signals, data, products or products, etc.) should be interpreted as including not only certain technical feature elements explicitly listed, but also other technical feature elements known in the art that are not explicitly listed.

[0022] The term "consisting of..." means excluding any technical feature elements not explicitly listed. If this term is used in a claim, it will make the claim closed, so that it does not contain technical feature elements other than the technical feature elements explicitly listed, except for the conventional impurities related to them. If this term only appears in a clause of a claim, it only limits the elements explicitly listed in the clause, and the elements recorded in other clauses are not excluded from the overall claim.

[0023] The term "parts by mass" refers to the mass ratio relationship between multiple components. For example, if it is described that component X is x parts by mass and component Y is y parts by mass, then the mass ratio of component X to component Y is x:y. 1 part by mass can represent any mass, for example, 1 part by mass can be represented as 1 kg or 3.1415926 kg. The sum of the parts by mass of all components is not necessarily 100 parts, but can be greater than 100 parts, less than 100 parts or equal to 100 parts. Unless otherwise specified, the parts, proportions and percentages described herein are all measured by mass.

[0024] When concentration, temperature, pressure, size or other parameters are expressed in the form of a numerical range, the numerical range should be understood to specifically disclose all ranges formed by the pairing of any upper limit, lower limit, and preferred value in the numerical range, regardless of whether the range is explicitly stated; for example, if a numerical range of "2 to 8" is stated, the numerical range should be interpreted as including ranges such as "2 to 7", "2 to 6", "5 to 7", "3 to 4 and 6 to 7", "3 to 5 and 7", "2 and 5 to 7", etc. Unless otherwise specified, the numerical ranges stated herein include both their end values ​​and all integers and fractions within the numerical range.

[0025] The orientation or position relationship indicated by terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc. are based on the orientation or position relationship shown in the drawings and are only for the convenience and simplification of description, and do not explicitly or implicitly indicate that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation of this document.

[0026] The scheme provided by the present invention is described in detail below. The contents not described in detail in the embodiments of the present invention belong to the prior art known to professionals in the field. If the specific conditions are not specified in the embodiments of the present invention, they are carried out according to the conventional conditions in the field or the conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used in the embodiments of the present invention, they are all conventional products that can be purchased commercially.

[0027] The embodiment of the present invention provides a two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy, comprising:

[0028] A component and a component B are combined in a mass ratio of 100:30; wherein,

[0029] Measured by weight, the component A comprises 30 to 40 parts of modified epoxy resin, 3 to 5 parts of diluent, 1 to 2 parts of difunctional polyether polyol, 1 to 4 parts of coupling agent, 0.05 to 1 part of defoaming aid, 0.1 to 1 part of color paste, 1 to 5 parts of special rubber copolymer toughening agent, and 40 to 50 parts of special composite thermal conductive flame retardant;

[0030] In terms of parts by mass, the B component contains 70 to 80 parts of modified acid anhydride, 1 to 10 parts of amine accelerator, 1 to 5 parts of special rubber copolymer toughening agent, and 5 to 10 parts of special composite thermal conductive flame retardant.

[0031] Preferably, in the component A and the component B of the above-mentioned potting glue, the rubber copolymer toughening agent is prepared from the base material 1, phthalate, distilled water, sulfuric acid solution, sodium persulfate and polysulfate amine by any one of graft copolymerization, block copolymerization and aldol condensation;

[0032] The first base material is at least one of polysulfide rubber, nitrile rubber, styrene-butadiene rubber, and ABS resin.

[0033] Preferably, the rubber copolymer toughening agent is synthesized in the following manner, including:

[0034] The base material 1 and phthalate are cut into blocks, which can be cut into small blocks, and distilled water accounting for 80% of the total mass of the base material 1 is added, and a 20% sulfuric acid solution accounting for 30% of the total mass of the base material 1 is added, and the mixture is placed in a 150°C oil bath and stirred at a high speed at a speed of 800R for a constant temperature. After 2 hours, the mixture is cooled to 50°C, nitrogen is introduced, and sodium persulfate accounting for 15% of the total mass of the base material 1 is added, and then polysulfate amine with a mass fraction of 60% is placed in a constant pressure dropping funnel, and the molar ratio of the base material 1 to the polysulfate amine is 1:1-3 respectively; the dripping speed of the constant pressure dropping funnel is adjusted to one drop per 3s, and high-speed stirring is maintained after the reaction for 3 hours, and the heating is stopped and the mixture is cooled to room temperature to obtain a base material 1-polysulfate amine graft copolymer toughening agent.

[0035] If the first base material is polysulfide rubber, the obtained product is a polysulfide rubber-polysulfate amine graft copolymer toughening agent;

[0036] If the first base material is nitrile rubber, the obtained product is nitrile rubber-polysulfate amine graft copolymer toughening agent;

[0037] If the first base material is styrene-butadiene rubber, the obtained product is styrene-butadiene rubber-polysulfate amine graft copolymer toughening agent;

[0038] If the first base material is ABS resin, the obtained material is ABS resin-polysulfate amine graft copolymer toughening agent.

[0039] Preferably, the molar ratio of the base material 1 to the polysulfate ammonium is 1:1 to 3, and if the base material 1 is nitrile rubber, the molar ratio of the nitrile rubber to the polysulfate ammonium is 1:1;

[0040] If the first base material is styrene-butadiene rubber, the molar ratio of styrene-butadiene rubber to polysulfate ammonium is 1:2;

[0041] If the first base material is polysulfide rubber, the molar ratio of nitrile rubber to polysulfate amine is 1:3;

[0042] If the first base material is ABS resin, the molar ratio of ABS resin to polysulfate ammonium is 1:2.

[0043] Preferably, in the component A and the component B of the above-mentioned potting glue, the composite thermal conductive flame retardant is prepared by: the base material and the plating material are prepared by any one of the following methods: surface coating, electroplating, graft copolymerization, and block copolymerization;

[0044] The matrix material is at least one of aluminum hydroxide, aluminum oxide, expanded graphite, worm graphite, carbon fiber, carbon nanotube, spherical silicon powder, and fused silicon powder;

[0045] The plating material is at least one of boron nitride and aluminum nitride.

[0046] Preferably, the thermally conductive flame retardant filler is prepared in the following manner, including:

[0047] Using a base material as a base, the base material is prepared by sequentially performing base degreasing, cleaning, roughening, re-cleaning, electroplating, passivation, final cleaning and drying;

[0048] The plating base material and the plating material are subjected to a surface coating synthesis reaction, and sintered under high temperature and high pressure conditions to obtain a composite thermal conductive filler with super thermal conductivity.

[0049] Preferably, in the plating base material prepared by the above method, the substrate degreasing, cleaning, roughening and re-cleaning are performed by chemically degreasing the substrate with a sodium hydroxide solution and chemically treating the substrate with concentrated sulfuric acid to remove surface pollutants and increase surface roughness;

[0050] The electroplating, final cleaning and drying are performed by using the pre-treated substrate electric friction ring as the cathode and the carbon material plate as the anode, using a DC voltage-stabilized current power supply, constant voltage electroplating, and controlling the voltage to be 0.5-8V; the electroplating solution formula is: 50-100g / L CuSO4·5H2O, 55g / L LH2SO4, 50mg / L HCl, the electroplating solution is mechanically stirred at room temperature, and the plating time is 10-30min;

[0051] Passivation means that after the electroplating is completed, the substrate is washed with water until it is neutral, and then passivated with an imidazole passivator, that is, a certain temperature (100°C) is controlled, the plated substrate is immersed in the imidazole passivator for 1 hour, and then washed and dried at 100°C;

[0052] Specifically, the preparation process of the plating base material is as follows: substrate degreasing → cleaning → roughening → cleaning → electroplating → passivation → cleaning → drying to obtain the plating base material. In order to make the aluminum hydroxide or aluminum oxide substrate and the carbon-based material layer closely bonded, the substrate is chemically degreased with sodium hydroxide solution and chemically treated with concentrated sulfuric acid to remove surface pollutants, improve surface roughness, and improve the wettability of the substrate and the carbon-based material. The pretreated aluminum hydroxide or aluminum oxide substrate electric friction ring is used as the cathode, and the carbon material plate is used as the anode. The HBBS1730OSL15A DC voltage and current stabilized power supply is used for constant voltage electroplating, and the control voltage is 0.5 to 8V. The plating solution formula is: 50 to 100g / L CuSO4·5H2O, 55g / LH2SO4, 50mg / L HCl, the plating solution is mechanically stirred at room temperature, and the plating time is 10 to 30min. After electroplating, wash with water until neutral, then use imidazole passivator for passivation treatment (control a certain temperature and soak the plated sample in the imidazole passivator for a certain time), clean and dry at 100℃.

[0053] The plating base material and boron nitride are subjected to surface coating synthesis reaction and sintered under high temperature and high pressure conditions in the following manner, including:

[0054] The plated base material is used as the friction material, the friction component is selected as aluminum nitride or boron nitride as the plated material, the lubricating component is carbon fiber and expanded graphite respectively, the carbon fiber and expanded graphite are prepared by spark plasma sintering technology, the material sintering temperature is 900-1000°C, the sintering pressure is 50MPa, and the vacuum degree in the furnace is controlled below 1-10Pa during sintering.

[0055] Preferably, in the component A of the epoxy potting glue, the modified epoxy resin is one or more of glycidyl ethers, glycidyl esters, glycidyl amines, and alicyclic epoxy resins; epoxy resin is the most basic component of the potting glue and can be selected according to different viscosity and performance requirements;

[0056] The diluent is one or two of p-tert-butylphenol, 4-methoxyphenol, 2,6-di-tert-butylphenol, 1,4-butanediol diglycidyl ether, benzyl glycidyl ether, carbonyl glycidyl ether, neopentyl glycol diglycidyl ether, and cardanol glycidyl ether;

[0057] The coupling agent is one or more of vinyl trichlorosilane, vinyl triethoxysilane, vinyl tri(2-methoxyethoxy)silane, γ-chloropropane trichlorosilane, γ-chloropropane triethoxysilane, aniline methyl trimethoxysilane, and γ-urea propyl triethoxysilane;

[0058] The defoaming aid is one or more of SH5500, A535, BYK996, BYK966, animal and plant wax, palm wax, castor oil, coconut oil, tall oil, silicate, sodium bicarbonate, detergent, and polysiloxane defoaming agent;

[0059] The color paste is one or more of the following: red iron oxide, yellow iron oxide, black iron oxide, carbon black, yellow chrome oxide, red paste, black paste, green paste, purple paste, and white paste;

[0060] Preferably, in the component B of the epoxy potting glue, the modified acid anhydride is one or more of methyltetrahydrophthalic anhydride, phthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, methylhexahydrophthalic anhydride, chlorendic anhydride, benzophenone tetracarboxylic anhydride, polyazelaic anhydride, and methylcyclohexene tetracarboxylic anhydride;

[0061] The amine accelerator is one or more of N,N dimethylbenzylamine, N,N,N trimethylbenzylamine, N,N dimethyl-p-toluidine, ammonium chloride, tetramethylammonium chloride, dimethylammonium chloride, polyamide, and methacryloxypropyltrimethoxybenzylamine.

[0062] The embodiment of the present invention also provides a method for preparing the above-mentioned two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy, comprising the following steps:

[0063] Preparation of component A: Take the raw materials of component A according to the above formula, add the modified epoxy resin, phenolic diluent and difunctional polyether polyol in the raw materials into the reaction kettle in sequence, stir at medium speed for 0.5 to 1 hour at 60 to 70°C until the solid is completely dissolved, then add the coupling agent and defoaming aid into the reaction kettle in sequence, stir at low speed for 0.5 to 1 hour at 60 to 70°C to mix the liquid raw materials evenly, then add the color paste, rubber copolymer toughening agent and composite thermal conductive flame retardant in sequence, vacuum and stir at high speed for 1 to 2 hours at 50 to 60°C, and obtain component A with toughening, thermal conductivity and flame retardant properties;

[0064] Preparation of component B: Take the raw materials of component B according to the above formula, add the modified anhydride and amine accelerator in the raw materials into another reaction kettle in turn, stir at medium speed at 90-100°C for 1-1.5 hours until the solid is completely dissolved, then add the rubber copolymer toughening agent and the composite thermal conductive flame retardant into the reaction kettle in turn, vacuum and stir at high speed at 70-80°C for 1-2 hours to obtain component B with toughening, thermal conductivity and flame retardancy;

[0065] The component A and the component B prepared above are combined in a mass ratio of 100:30 to obtain a two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy.

[0066] In summary, the epoxy potting adhesive of the present invention has the advantages of high thermal conductivity, excellent flame retardancy, long room temperature operability time, high mechanical strength, etc., and is suitable for multiple industries such as electronic appliances, insulating materials, adhesives, and composite materials.

[0067] In order to more clearly demonstrate the technical solution and technical effects provided by the present invention, the solution provided by the embodiment of the present invention is described in detail with specific embodiments below.

[0068] The embodiment of the present invention provides a two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy, which is composed of component A and component B, and the mass ratio of component A to component B is 100:30; wherein component A is a main agent, and component B is a curing agent;

[0069] The present invention is described in detail below through 4 embodiments and 1 comparative example.

[0070] Example 1

[0071] In this embodiment, the modified epoxy resin of component A is E54 resin; the diluent is carbon tetradecyl glycidyl ether; the coupling agent is γ-chloropropane trichlorosilane; the defoaming agent is SH5500; the color paste is iron oxide black; the rubber copolymer toughening agent is ABS resin-polysulfate amine graft copolymer; the composite thermal conductive flame retardant is aluminum hydroxide-based composite filler, and the specific component contents are shown in Table 1.

[0072] Table 1:

[0073]

[0074]

[0075] The modified anhydride of component B is methyl hexahydrophthalic anhydride; the amine accelerator is N,N,N trimethylbenzylamine; the rubber copolymer toughening agent is ABS resin-polysulfate amine graft copolymer; the composite thermal conductive flame retardant is aluminum hydroxide-based composite filler, and the specific component contents are shown in Table 2.

[0076] Table 2:

[0077] B component raw materials Dosage (parts by mass) Methylhexahydrophthalic anhydride 80 N,N,N-trimethylbenzylamine 5 ABS resin-polysulfate amine graft copolymer 5 Aluminum hydroxide based composite filler 10

[0078] Example 2

[0079] In this embodiment, the modified epoxy resin of component A is E51 resin; the diluent is p-tert-butylphenol and 4-methoxyphenol; the coupling agent is vinyl trichlorosilane; the defoaming agent is A535; the color paste is carbon black; the rubber copolymer toughening agent is polysulfide rubber-polysulfate amine graft copolymer; the composite thermal conductive flame retardant is an alumina-based composite filler. The specific content of the raw materials of component A is shown in Table 3.

[0080] Table 3:

[0081]

[0082]

[0083] The modified acid anhydride of component B is methyltetrahydrophthalic anhydride; the amine accelerator is N,N-dimethylbenzylamine and tetramethylammonium chloride; the rubber copolymer toughening agent is polysulfide rubber-polysulfate amine graft copolymer; the thermal conductive flame retardant composite filler is an alumina-based composite filler. The specific content of the raw materials of component B is shown in Table 4.

[0084] Table 4:

[0085] B component raw materials Dosage (parts by mass) Methyltetrahydrophthalic anhydride 85 N,N-Dimethylbenzylamine 1.5 Tetramethylammonium chloride 1.5 Polysulfide rubber-polysulfate amine graft copolymer 3 Alumina-based composite fillers 9

[0086] Example 3

[0087] In this embodiment, the modified epoxy resin of component A is E51 resin; the diluent is neopentyl glycol diglycidyl ether; the coupling agent is γ-ureapropyl triethoxysilane; the defoaming agent is A535; the color paste is carbon black; the special toughening agent is nitrile rubber-polysulfate amine graft copolymer; the special thermal conductive flame retardant is an alumina-based composite filler, and the specific component contents are shown in Table 5.

[0088] Table 5:

[0089] A component raw materials Dosage (parts by mass) Epoxy resin E51 30 Neopentyl glycol diglycidyl ether 6 γ-Ureapropyltriethoxysilane 3 A535 0.5 Carbon Black 1.5 Nitrile rubber-polysulfate amine graft copolymer 12 Alumina-based composite fillers 47

[0090] The modified anhydride of component B is chlorendic anhydride; the amine accelerator is dimethyl ammonium chloride and polyamide; the rubber copolymer toughening agent is nitrile rubber-polysulfate amine graft copolymer; the composite thermal conductive flame retardant is alumina-based composite fillers and aluminum hydroxide-based composite fillers. The specific component contents are shown in Table 6

[0091] Table 6:

[0092] B component raw materials Dosage (parts by mass) Chlorendic anhydride 83 Polyamide 1 Dimethylammonium chloride 1.5 Nitrile rubber-polysulfate amine graft copolymer 5 Alumina-based composite fillers 4.5 Aluminum hydroxide based composite filler 5

[0093] Example 4

[0094] In this embodiment, the modified epoxy resin of component A is alicyclic epoxy resin TTA21P; the diluent is cardanol glycidyl ether; the coupling agent is KH560 and KH570; the defoaming agent is tall oil; the color paste is black paste; the rubber copolymer toughening agent is styrene-butadiene rubber-polysulfate amine graft copolymer; the composite thermal conductive flame retardant is a spherical silica powder-based composite filler, and the specific component contents are shown in Table 7.

[0095] Table 7:

[0096] A component raw materials Amount (parts by mass) Cycloaliphatic epoxy resin TTA21P 25 Cardanol Glycidyl Ether 10 KH560 1 KH570 1 Tall Oil 1 Black pulp 3 Styrene butadiene rubber-polysulfate amine graft copolymer 18 Spherical silica powder based composite filler 41

[0097] The modified anhydride of component B is benzophenone tetracarboxylic dianhydride; the amine accelerator is N, N-dimethylbenzylamine and polyamide; the rubber copolymer toughening agent is phthalate-polysulfate amine graft copolymer; the composite thermal conductive flame retardant is aluminum hydroxide-based composite filler, and the specific component contents are shown in Table 8

[0098] Table 8:

[0099] B component raw materials Dosage (parts by mass) Benzophenone tetracarboxylic dianhydride 83 Polyamide 1.2 N,N-Dimethylbenzylamine 1.8 Phthalate-polysulfate amine graft copolymer 4 Aluminum hydroxide based composite filler 10

[0100] The above embodiment was actually applied to large cylindrical capacitors for wind power and photovoltaic power generation, and compared with the currently commercially available product Dongrun 9005 (Z). The anti-cracking performance of the product was tested at low temperature (-50°C / several days) and high and low temperature cycles (-40-85°C, each temperature was maintained for 50 minutes, and the temperature rise and fall time was controlled to be 20 minutes). The flame retardant performance (UL94 standard) and thermal conductivity (Hot Disk method) of the product were tested. The temperature rise curve of the product in a simulated aluminum shell cylindrical capacitor with a 2C rate running for one cycle under power-on was tested using a temperature recorder, and the maximum exothermic temperature of the product and the competing products was compared (see details). Figure 1 The curves from top to bottom are competitor, Example 4, Example 3, Example 2, and Example 1); the product's double 85 aging resistance (85°C / 85RH) was tested, and the specific results are shown in Table 9.

[0101] Among them, the double 85 aging resistance, high and low temperature impact resistance, and low temperature impact resistance are all tested after simulating capacitor potting using PPS material and aluminum shell. The test is conducted at regular intervals until the surface glue cracks or the shell is obviously deformed. At this time, the product is judged to be failed.

[0102] Table 9 Comparison of relevant properties of the potting glue of the present invention and existing market products

[0103] Related performance Example 1 Example 2 Example 3 Example 4 Dongrun 9005(Z) Thermal conductivity / [W / (m·K)] 1.039 1.028 1.067 1.043 0.645 Flame retardant grade / UL94 1.5mm V0 1.5mm V0 1.5mm V0 1.5mm V0 3mm V0 Double 85 resistance performance / h 1850 1850 1800 1900 1000 Low temperature impact resistance / d 40 45 42 43 25 High and low temperature impact resistance / times 1490 1550 1680 1580 1000 Temperature rise test maximum temperature / ℃ 44 45 46 47 54

[0104] The results in the table above show that compared with the current commercial product Dongrun 9005 (Z), the formula with added special thermal conductive / flame retardant and toughening fillers has significantly improved aging resistance, and the number of cycles and time have increased by about 1 times; the thermal conductivity has increased significantly, and the maximum temperature of the temperature rise experiment has decreased by about 10°C on average, with a significant heat dissipation effect; this is of great help in alleviating the excessive heat release of large capacitors under high-rate cycles, reducing the risk of thermal runaway, and extending the service life of capacitors; the flame retardant grade has been improved to a certain extent, reaching the standard of UL94 1.5mm V-0, which greatly improves the flame retardant performance of capacitors under harsh conditions and reduces the accident rate of capacitors, which is crucial to ensure the safe use of capacitors.

[0105] Depend on Figure 1 It can be seen that the maximum heat release temperature of the capacitor product of the present invention using the composite thermal conductive flame retardant is significantly reduced compared with competing products, with the maximum reduction being about 10°C.

[0106] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.

Claims

1. A two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy, characterized in that: include: Component A and component B are combined in a mass ratio of 100:30; wherein, In parts by mass, the component A comprises 30 to 40 parts of modified epoxy resin, 3 to 5 parts of diluent, 1 to 2 parts of difunctional polyether polyol, 1 to 4 parts of coupling agent, 0.05 to 1 part of defoaming aid, 0.1 to 1 part of color paste, 1 to 5 parts of rubber copolymer toughening agent, and 40 to 50 parts of composite thermal conductive flame retardant; In terms of parts by mass, the B component comprises 70 to 80 parts of modified acid anhydride, 1 to 10 parts of amine accelerator, 1 to 5 parts of rubber copolymer toughening agent, and 5 to 10 parts of composite thermal conductive flame retardant.

2. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to claim 1, characterized in that: In the A component and the B component, the rubber copolymer toughener is prepared from the base material 1, distilled water, sulfuric acid solution, sodium persulfate and polysulfate amine as raw materials by any one of graft copolymerization, block copolymerization and aldol condensation; The first base material is at least one of polysulfide rubber, nitrile rubber, styrene-butadiene rubber, ABS resin, and phthalate.

3. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to claim 2, characterized in that: The rubber copolymer toughening agent is synthesized in the following manner, including: The base material 1 is cut into blocks, distilled water accounting for 80% of the total mass of the base material 1 is added, and a 20% sulfuric acid solution accounting for 30% of the total mass of the base material 1 is added, and the blocks are placed in an oil bath at 150°C and stirred at a high speed at a speed of 800R for a constant temperature. After 2 hours, the blocks are cooled to 50°C, nitrogen is introduced, and sodium persulfate accounting for 15% of the total mass of the base material 1 is added. Then, polysulfate amine with a mass fraction of 60% is placed in a constant pressure dropping funnel, and the molar ratio of the base material 1 to the polysulfate amine is 1:1-3 respectively; the dripping speed of the constant pressure dropping funnel is adjusted to one drop per 3s, and high-speed stirring is maintained after the reaction for 3 hours, and the heating is stopped and the blocks are cooled to room temperature to obtain a base material 1-polysulfate amine graft copolymer toughening agent.

4. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to claim 3, characterized in that: The molar ratio of the base material 1 to the polysulfate ammonium is 1:1 to 3. If the base material 1 is nitrile rubber, the molar ratio of the nitrile rubber to the polysulfate ammonium is 1:

1. If the first base material is styrene-butadiene rubber, the molar ratio of styrene-butadiene rubber to polysulfate ammonium is 1:2; If the first base material is polysulfide rubber, the molar ratio of nitrile rubber to polysulfate amine is 1:3; If the base material 1 is ABS resin, the molar ratio of ABS resin to polysulfate ammonium is 1:2; If the first base material is phthalate, the molar ratio of phthalate to polysulfate amine is 1:

3.

5. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to claim 1, characterized in that: In the A component and the B component, the composite thermal conductive flame retardant is prepared by: the base material and the plating material are prepared by any one of surface coating, electroplating, graft copolymerization and block copolymerization; The matrix material is at least one of aluminum hydroxide, aluminum oxide, expanded graphite, worm graphite, carbon fiber, carbon nanotube, spherical silicon powder, and fused silicon powder; The plating material is at least one of boron nitride and aluminum nitride.

6. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to claim 5, characterized in that: The thermally conductive flame retardant filler is prepared in the following manner, including: Using a base material as a base, the base material is prepared by sequentially performing base degreasing, cleaning, roughening, re-cleaning, electroplating, passivation, final cleaning and drying; The plating base material and the plating material are subjected to a surface coating synthesis reaction, and sintered under high temperature and high pressure conditions to obtain a composite thermal conductive filler with super thermal conductivity.

7. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to claim 6, characterized in that: In the plating base material prepared by the method, Degreasing, cleaning, roughening and re-cleaning of the substrate are carried out by chemically degreasing the substrate with sodium hydroxide solution and chemically treating the substrate with concentrated sulfuric acid to remove surface contaminants and improve surface roughness; The electroplating, final cleaning and drying are performed by using the pre-treated substrate electric friction ring as the cathode and the carbon material plate as the anode, using a DC voltage-stabilized current power supply, constant voltage electroplating, and controlling the voltage to be 0.5-8V; the electroplating solution formula is: 50-100g / L CuSO4·5H2O, 55g / L LH2SO4, 50mg / L HCl, the electroplating solution is mechanically stirred at room temperature, and the plating time is 10-30min; Passivation means that after the electroplating is completed, the surface is washed with water until it is neutral, and then passivated with an imidazole passivating agent, and then cleaned and dried at 100°C; The plating base material and the plating material are subjected to a surface coating synthesis reaction and sintered under high temperature and high pressure conditions in the following manner, including: The plated base material is used as the friction material, the friction component is selected as aluminum nitride or boron nitride as the plated material, the lubricating component is carbon fiber and expanded graphite respectively, the carbon fiber and expanded graphite are prepared by spark plasma sintering technology, the material sintering temperature is 900-1000°C, the sintering pressure is 50MPa, and the vacuum degree in the furnace is controlled below 1-10Pa during sintering.

8. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to any one of claims 1 to 7, characterized in that: In the component A, the modified epoxy resin is one or more of glycidyl ethers, glycidyl esters, glycidyl amines, and alicyclic epoxy resins; The diluent is one or two of p-tert-butylphenol, 4-methoxyphenol, 2,6-di-tert-butylphenol, 1,4-butanediol diglycidyl ether, benzyl glycidyl ether, carbonyl glycidyl ether, neopentyl glycol diglycidyl ether, and cardanol glycidyl ether; The coupling agent is one or more of vinyl trichlorosilane, vinyl triethoxysilane, vinyl tri(2-methoxyethoxy)silane, γ-chloropropane trichlorosilane, γ-chloropropane triethoxysilane, aniline methyl trimethoxysilane, and γ-urea propyl triethoxysilane; The defoaming aid is one or more of SH5500, A535, BYK996, BYK966, animal and plant wax, palm wax, castor oil, coconut oil, tall oil, silicate, sodium bicarbonate, detergent, and polysiloxane defoaming agent; The color paste is one or more than two of red iron oxide, yellow iron oxide, black iron oxide, carbon black, yellow chrome oxide, red paste, black paste, green paste, purple paste and white paste.

9. The two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to any one of claims 1 to 7, characterized in that: In the B component, the modified acid anhydride is one or more of methyltetrahydrophthalic anhydride, phthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, methylhexahydrophthalic anhydride, chlorendic anhydride, benzophenone tetracarboxylic anhydride, polyazelaic anhydride, and methylcyclohexene tetracarboxylic anhydride; The amine accelerator is one or more of N,N dimethylbenzylamine, N,N,N trimethylbenzylamine, N,N dimethyl-p-toluidine, ammonium chloride, tetramethylammonium chloride, dimethylammonium chloride, polyamide, and methacryloxypropyltrimethoxybenzylamine.

10. A method for preparing the two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy according to any one of claims 1 to 9, characterized in that: The following steps are involved: Preparation of component A: taking the raw materials of component A according to the formula described in any one of claims 1 to 9, adding the modified epoxy resin, phenolic diluent and difunctional polyether polyol in the raw materials into a reaction kettle in sequence, stirring at medium speed for 0.5 to 1 hour at 60 to 70°C until the solid is completely dissolved, then adding the coupling agent and defoaming aid into the reaction kettle in sequence, stirring at low speed for 0.5 to 1 hour at 60 to 70°C to mix the liquid raw materials evenly, then adding the color paste, rubber copolymer toughening agent and composite thermal conductive flame retardant in sequence, vacuuming and stirring at high speed for 1 to 2 hours at 50 to 60°C, and obtaining component A with toughening, thermal conductivity and flame retardant properties; Preparation of component B: taking the raw materials of component B according to the formula described in any one of claims 1 to 9, adding the modified acid anhydride and amine accelerator in the raw materials into another reaction kettle in turn, stirring at medium speed at 90 to 100° C. for 1 to 1.5 hours until the solid is completely dissolved, then adding the rubber copolymer toughening agent and the composite thermal conductive flame retardant into the reaction kettle in turn, vacuuming and stirring at high speed at 70 to 80° C. for 1 to 2 hours to obtain component B with toughening, thermal conductivity and flame retardancy; The component A and the component B prepared above are combined in a mass ratio of 100:30 to obtain a two-component epoxy potting adhesive for capacitor potting, heat dissipation and flame retardancy.

Citation Information

Cited By

  • High-thermal-conductivity bi-component flame-retardant pouring sealant and preparation method thereof

    CN121495529A