Preparation method of composite abrasive for polishing silicon carbide substrate
By preparing composite abrasives based on aluminum hydroxide powder, the problems of low polishing efficiency and short abrasive use time in the existing silicon carbide surface polishing technology are solved, and high efficiency is achieved. Widely applicable silicon carbide device polishing effect.
Patent Information
- Application Number
- CN202410933215.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
The existing silicon carbide surface polishing technology is easily affected by factors such as polishing liquid pH and oxidants. Single alumina powder, silicon oxide or cerium oxide abrasives have problems with low polishing efficiency and short effective use time, making it difficult to meet electric vehicles and high-frequency communications. The industry has high requirements for silicon carbide devices.
Using alumina powder-based composite abrasives, nano-alumina preparation, nano-alumina preparation and aluminum oxide surface-coated silicon oxide process, inducing agents, surfactants, mineralizers, citric acid and Silicate, adjusts pH value, forms a stable composite abrasive, suitable for acidic, neutral and alkaline polishing liquids.
It improves polishing efficiency, extends the use time of abrasives, has a wide range of applications, solves the problems of scratches and low processing yield of a single abrasive, and is suitable for high-precision polishing of silicon carbide devices.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite abrasives for polishing, and in particular to a method for preparing composite abrasives for polishing a silicon carbide substrate. Background Art
[0002] Silicon carbide has greater potential in power devices and radio frequency devices due to its wider bandgap, higher saturated electron migration speed, higher thermal conductivity and lower on-resistance compared to silicon-based materials. It has a broad application market in electric vehicles, charging piles, photovoltaic inverters, rail transit, 5G high-frequency communications, etc. Silicon carbide surface CMP processing is an important part of the silicon carbide device processing industry chain. Silicon carbide devices have extremely high requirements for the surface flatness of silicon carbide. So far, chemical mechanical polishing is the only technology that can achieve a smooth and defect-free surface of silicon carbide wafers, but it is easily affected by many factors such as polishing liquid pH, oxidant, polishing parameters, electrolytes, etc. Among them, abrasives and their stability are the most important influencing factors. With the explosive growth of industries such as electric vehicles and high-frequency communications, the application of silicon carbide in automotive chips is also expanding. In the next 10 years, silicon carbide semiconductors will be in a period of rising demand, and the demand for supporting polishing liquids and other auxiliary materials will also increase significantly accordingly.
[0003] At present, the mainstream technical abrasives are mainly single aluminum oxide powder, diamond powder or silicon oxide. Single abrasives have disadvantages such as high defective rate and low polishing efficiency. The composite abrasives reported in departmental literature and patents are also a small amount of aluminum oxide mixed with silicon oxide or cerium oxide. The two abrasives are simply mixed and mixed together by electrostatic adsorption. The main substances are silicon oxide or cerium oxide, which have disadvantages such as low polishing efficiency and short effective use time. Summary of the invention
[0004] Based on the problems raised in the background technology, the present invention proposes a method for preparing a composite abrasive for polishing a silicon carbide substrate.
[0005] The present invention provides a composite abrasive for polishing a silicon carbide substrate, wherein the composite abrasive comprises aluminum hydroxide powder and components in mass percentages based on the mass of the aluminum hydroxide powder:
[0006] Inducer 1%-2%,
[0007] Surfactant 1%-2%,
[0008] Mineralizer 0.5%-1.5%,
[0009] Dispersant 1%-1.5%,
[0010] Citric acid 1%-1.5%,
[0011] Silicate 2%-5%,
[0012] pH regulator adjusts the pH to 3-6;
[0013] The present invention provides a method for preparing a composite abrasive for polishing a silicon carbide substrate, comprising the following steps:
[0014] Step 1, preparation of nano-boehmite, using aluminum hydroxide with a purity of 99.99% as a raw material, adding aluminum hydroxide into a high-pressure reactor, adding 1%-1.5% of an inducer, adding a surfactant, and using one or more of hydrochloric acid, nitric acid, phosphoric acid, and citric acid to adjust the pH value to 3-6, adding high-purity water with a resistance of more than 10 megohms, making the slurry solid content 20-30%, heating the reaction, controlling the reaction temperature to 180°C-230°C, and reacting for 6-8h. The obtained product is separated and dried to obtain nano-boehmite;
[0015] Step 2, preparation of nano-alumina, adding about 1% of nano-α-phase alumina as seed crystals to the boehmite, adding 0.5%-1.5% of mineralizer, and calcining at 1050-1150°C for 4h to obtain nano-alumina powder;
[0016] Step three, preparation of composite abrasive: grind and disperse the above-mentioned nano alumina powder in a ball mill, add 1%-1.5% sodium hexametaphosphate as a dispersant, grind until the nano alumina is completely dispersed, add 1%-1.5% citric acid, continue grinding to form an alumina-citric acid suspension, control the temperature of the suspension to 25-35°C, continue stirring, and slowly add silicate. The newly added silicate molecules will react with the hydrogen ions on the surface of the alumina to form metasilicic acid, and the metasilicic acid will dehydrate and condense to form silica molecules coated on the surface of the alumina particles. Calcine the coated composite particles at 500-550°C to obtain a composite abrasive with silica coated on the alumina surface.
[0017] Preferably, the aluminum hydroxide raw material contains one or more of the three crystal phases of gibbsite, nordstrandite and gibbsite.
[0018] Preferably, the inducing agent is one or a mixture of aluminum nitrate, aluminum chloride, and aluminum isopropoxide.
[0019] Preferably, the aluminum hydroxide powder is aluminum hydroxide powder having a regular surface morphology obtained by repeated grinding, and the average particle size thereof is 300nm-500nm.
[0020] Preferably, the surfactant is one or a mixture of ethylene glycol, anhydrous ethanol, polyvinyl alcohol, polyethylene glycol.
[0021] Preferably, the silicate is one or a mixture of sodium silicate, aluminum silicate, potassium silicate and calcium silicate.
[0022] Preferably, the mineralizer is one or a mixture of boric acid, ammonium chloride and aluminum fluoride.
[0023] The beneficial effects of the present invention are:
[0024] The composite abrasive with silicon oxide coated on the surface of aluminum oxide proposed by the present invention can be applied to polishing liquids with various pH values such as acidic, neutral and alkaline. It has a wide range of applications and can solve the problem of low polishing efficiency of single silicon oxide and cerium oxide abrasives, and the problem of many scratches and low processing yield of single aluminum oxide abrasives. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.
[0026] A composite abrasive for polishing a silicon carbide substrate, the composite abrasive comprising aluminum hydroxide powder and components in mass percentages based on the mass of the aluminum hydroxide powder:
[0027] Inducer 1%-2%,
[0028] Surfactant 1%-2%,
[0029] Mineralizer 0.5%-1.5%,
[0030] Dispersant 1%-1.5%,
[0031] Citric acid 1%-1.5%,
[0032] Silicate 2%-5%,
[0033] pH regulator adjusts the pH to 3-6;
[0034] The present invention provides a method for preparing a composite abrasive for polishing a silicon carbide substrate, comprising the following steps:
[0035] Step 1, preparation of nano-boehmite, using aluminum hydroxide with a purity of 99.99% as a raw material, adding aluminum hydroxide into a high-pressure reactor, adding 1%-1.5% of an inducer, adding a surfactant, and using one or more of hydrochloric acid, nitric acid, phosphoric acid, and citric acid to adjust the pH value to 3-6, adding high-purity water with a resistance of more than 10 megohms, making the slurry solid content 20-30%, heating the reaction, controlling the reaction temperature to 180°C-230°C, and reacting for 6-8h. The obtained product is separated and dried to obtain nano-boehmite;
[0036] Step 2, preparation of nano-alumina, adding about 1% of nano-α-phase alumina as seed crystals to the boehmite, adding 0.5%-1.5% of mineralizer, and calcining at 1050-1150°C for 4h to obtain nano-alumina powder;
[0037] Step three, preparation of composite abrasive: grind and disperse the above-mentioned nano alumina powder in a ball mill, add 1%-1.5% sodium hexametaphosphate as a dispersant, grind until the nano alumina is completely dispersed, add 1%-1.5% citric acid, continue grinding to form an alumina-citric acid suspension, control the temperature of the suspension to 25-35°C, continue stirring, and slowly add silicate. The newly added silicate molecules will react with the hydrogen ions on the surface of the alumina to form metasilicic acid, and the metasilicic acid will dehydrate and condense to form silica molecules coated on the surface of the alumina particles. Calcine the coated composite particles at 500-550°C to obtain a composite abrasive with silica coated on the alumina surface.
[0038] The aluminum hydroxide raw material comprises one or more of the three crystal phases of gibbsite, nordstrandite and gibbsite.
[0039] The inducing agent is one or a mixture of aluminum nitrate, aluminum chloride, and aluminum isopropoxide.
[0040] The aluminum hydroxide powder is aluminum hydroxide powder with a regular surface morphology obtained through repeated grinding, and the average particle size thereof is 300nm-500nm.
[0041] The surfactant is one of ethylene glycol, anhydrous ethanol, polyvinyl alcohol, polyethylene glycol or a mixture of several thereof.
[0042] The silicate is one of sodium silicate, aluminum silicate, potassium silicate and calcium silicate or a mixture of several of them.
[0043] The mineralizer is one or a mixture of boric acid, ammonium chloride and aluminum fluoride.
[0044] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a composite abrasive for polishing a silicon carbide substrate, characterized in that: The composite abrasive comprises aluminum hydroxide powder and a Components by mass percentage: Inducer 1%-2%, Surfactant 1%-2%, Mineralizer 0.5%-1.5%, Dispersant 1%-1.5%, Citric acid 1%-1.5%, Silicate 2%-5%, pH regulator adjusts the pH to 3-6; The preparation method of the composite abrasive comprises the following steps: Step 1, preparation of nano-boehmite, using aluminum hydroxide with a purity of 99.99% as a raw material, adding aluminum hydroxide into a high-pressure reactor, adding 1%-1.5% of an inducer, adding a surfactant, and using one or more of hydrochloric acid, nitric acid, phosphoric acid, and citric acid to adjust the pH value to 3-6, adding high-purity water with a resistance of more than 10 megohms, making the slurry solid content 20-30%, heating the reaction, controlling the reaction temperature to 180°C-230°C, and reacting for 6-8h. The obtained product is separated and dried to obtain nano-boehmite; Step 2, preparation of nano-alumina, adding about 1% of nano-α-phase alumina as seed crystals to the boehmite, adding 0.5%-1.5% of mineralizer, and calcining at 1050-1150°C for 4h to obtain nano-alumina powder; Step three, preparation of composite abrasive: grind and disperse the above-mentioned nano alumina powder in a ball mill, add 1%-1.5% sodium hexametaphosphate as a dispersant, grind until the nano alumina is completely dispersed, add 1%-1.5% citric acid, continue grinding to form an alumina-citric acid suspension, control the temperature of the suspension to 25-35°C, continue stirring, and slowly add silicate. The newly added silicate molecules will react with the hydrogen ions on the surface of the alumina to form metasilicic acid, and the metasilicic acid will dehydrate and condense to form silica molecules coated on the surface of the alumina particles. Calcine the coated composite particles at 500-550°C to obtain a composite abrasive with silica coated on the alumina surface.
2. The method for preparing a composite abrasive for polishing a silicon carbide substrate according to claim 1, characterized in that: The aluminum hydroxide raw material comprises one or more of the three crystal phases of gibbsite, nordstrandite and gibbsite.
3. The method for preparing a composite abrasive for polishing a silicon carbide substrate according to claim 1, characterized in that: The inducing agent is one or a mixture of aluminum nitrate, aluminum chloride, and aluminum isopropoxide.
4. The method for preparing a composite abrasive for polishing a silicon carbide substrate according to claim 1, characterized in that: The aluminum hydroxide powder is aluminum hydroxide powder with a regular surface morphology obtained through repeated grinding, and the average particle size thereof is 300nm-500nm.
5. The method for preparing a composite abrasive for polishing a silicon carbide substrate according to claim 1, characterized in that: The surfactant is one of ethylene glycol, anhydrous ethanol, polyvinyl alcohol, polyethylene glycol or a mixture of several thereof.
6. The method for preparing a composite abrasive for polishing a silicon carbide substrate according to claim 1, characterized in that: The silicate is one of sodium silicate, aluminum silicate, potassium silicate and calcium silicate or a mixture of several of them.
7. The method for preparing a composite abrasive for polishing a silicon carbide substrate according to claim 1, characterized in that: The mineralizer is one or a mixture of boric acid, ammonium chloride and aluminum fluoride.