Environment-friendly lubricant for metal wire drawing

By using ingredients such as animal oils, sodium soaps, vegetable oils and other ingredients that are easy to decompose raw materials and antioxidants, an environmentally friendly metal brushing lubricant is prepared, which solves the problem of poor environmental protection of existing lubricants and achieves efficient metal brushing treatment.

CN118895174AInactive Publication Date: 2024-11-05TIANJIN HONGYA LUBRICATION POWDER MFG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410927842.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The raw materials of existing metal brushed lubricants contain a large amount of chemical formulas that are not easy to degrade, resulting in poor environmental protection and greater environmental pollution.

Method used

Using animal oils, sodium soaps, vegetable oils, stearic acid, brighteners, anti-wear pressure agents, antioxidants and dispersants as main components, environmentally friendly lubricants are prepared through grinding and melting and mixing steps to improve their environmental protection and performance.

Benefits of technology

It improves the environmental protection and performance of lubricants, is suitable for large-scale production, enhances its oxidation and wear resistance, and is suitable for metal wire drawing treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895174A_ABST
    Figure CN118895174A_ABST
Patent Text Reader

Abstract

Belonging to the technical field of lubricants, the invention discloses an environment-friendly lubricant for metal wire drawing, which comprises the following materials: animal fat, sodium soap, vegetable fat, stearic acid, a brightener, an antiwear extreme pressure agent, an antioxidant and a dispersant. According to the lubricant disclosed by the invention, the animal fat, the sodium soap and the vegetable fat are adopted as theme raw materials which are extremely easy to decompose in nature, so that the environmental protection property of the whole lubricant can be greatly improved, the lubricant can be put into large-scale lubricant production, and the anti-wear extreme pressure agent, the antioxidant and the dispersing agent are also arranged in the lubricant, so that the lubricant is environment-friendly. The materials can help to improve the oxidation resistance and wear resistance of the lubricant, so that the lubricant can be more suitable for metal wire drawing treatment, meanwhile, the materials are prepared in groups in the preparation method, and small components are equally input in the preparation process, so that the cost is reduced, and the production efficiency is improved. The fusion effect and efficiency of all components in the material can be improved, and the quality of a final finished product is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lubricants, and in particular relates to an environmentally friendly lubricant for metal wire drawing. Background Art

[0002] Lubricant is a lubricating medium used to reduce the friction resistance of the friction pair and slow down its wear. It can also cool, clean and prevent pollution of the friction pair. Lubricants are also needed when drawing metal.

[0003] A Chinese patent discloses (CN106675738A) a method for preparing a metal wire drawing lubricant, which belongs to the technical field of lubricant preparation. The lubricant uses methyl ricinoleate as a raw material to prepare a lubricating oil base oil, and then uses an ultrasonic assisted stripping method to strip molybdenum disulfide crystals to obtain graphene-like molybdenum disulfide, which is then compounded with a carbon nanotube dispersion, and the carbon nanotubes are doped between the graphene-like molybdenum disulfide to obtain a dispersion with high stability, high heat dissipation and good dispersibility. Finally, the lubricating oil base oil, polyvinyl alcohol, deionized water, etc. are stirred and mixed with the carbon-doped graphene-like molybdenum disulfide dispersion to obtain a metal wire drawing lubricant. The method uses the prepared graphene-like molybdenum disulfide to form a low shear stress film on the friction pair surface, thereby reducing the friction coefficient and filling and repairing the friction surface. At the same time, it is not easy for the metal wire to break and produce an unpleasant odor during use, and it is harmless to the environment and human body, and has broad application prospects. Although today's metal wire drawing lubricants have good lubrication functions, their raw materials mostly use a large number of chemical formulas. These formulas contain some environmental pollutants that are difficult to degrade, resulting in poor environmental performance of the lubricant. Mass production can easily cause great damage to the environment. In order to solve this problem, an environmentally friendly lubricant for metal wire drawing is urgently needed. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that although the current metal wire drawing lubricants also have good lubricating functions, their raw materials mostly use a large number of chemical formulas, which contain some environmental pollutants that are not easy to degrade, resulting in poor environmental protection of the lubricants. Mass production is likely to cause great damage to the environment. An environmentally friendly lubricant for metal wire drawing is proposed to solve the problem.

[0005] In order to achieve the above purpose, the present invention adopts the following technical scheme: an environmentally friendly lubricant for metal wire drawing, comprising the following materials: animal fat, sodium soap, vegetable fat, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant.

[0006] As a further description of the above technical solution:

[0007] The weight proportions of the animal fat, sodium soap, vegetable fat, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant are 8-12 parts, 3-5 parts, 6-7 parts, 5-8 parts, 1-3 parts, 2-3 parts, 2-4 parts and 2-5 parts respectively.

[0008] This article also discloses a method for preparing an environmentally friendly lubricant for metal wire drawing, comprising the following steps:

[0009] S1. Put the anti-wear extreme pressure agent and antioxidant into a grinding device, control the speed of the grinding device, and grind the mixed material;

[0010] S2. After grinding, sieve the ground material and divide the ground material into multiple portions;

[0011] S3, taking animal fat, sodium soap, and vegetable fat into a melt mixing device respectively, increasing the temperature of the device, and controlling the mixing rate to mix the mixed materials;

[0012] S4. During the mixing process, different components of the grinding materials are added into the device several times, and a certain time interval is maintained between each addition. After the mixing is completed, the mixed liquid is taken out and marked as component A;

[0013] S5, re-taking animal fat, sodium soap, and vegetable fat into a melt mixing device, respectively, raising the device temperature, and controlling the mixing rate to mix the mixed materials;

[0014] S6, respectively introducing stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant into the device, increasing the mixing rate, and maintaining the temperature for a period of time;

[0015] S7, marking the above reaction solution as component B, mixing component A with component B, increasing the reaction temperature, and maintaining it for a period of time;

[0016] S8, waiting for the mixed liquid to cool down, and filtering it;

[0017] S9. Collect and store the finished products.

[0018] As a further description of the above technical solution:

[0019] In S1, anti-wear extreme pressure agent and antioxidant are put into a grinding device, and the speed of the grinding device is controlled to 30-50 r / min to grind the mixed material.

[0020] As a further description of the above technical solution:

[0021] In S2, after grinding, the ground material is passed through a 80-100 mesh sieve, and the ground material is evenly divided into 3-4 parts.

[0022] As a further description of the above technical solution:

[0023] In S3, animal fat, sodium soap and vegetable fat are respectively placed in a melting and mixing device, the temperature of the device is increased to 180-200° C., and the mixing rate is controlled to 100-120 r / min to mix the mixed materials.

[0024] As a further description of the above technical solution:

[0025] In S4, during the mixing process, the grinding materials of different components are added into the device in 3-4 times, and each addition is kept for 5-8 minutes. After the mixing is completed, the mixed liquid is taken out and marked as component A.

[0026] As a further description of the above technical solution:

[0027] In S5, animal fat, sodium soap and vegetable fat are taken again and placed in a melting and mixing device respectively, the temperature of the device is increased to 210-230° C., and the mixing rate is controlled to 150-170 r / min to mix the mixed materials.

[0028] As a further description of the above technical solution:

[0029] In S6, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant are introduced into the device respectively, the mixing rate is increased to 180-200 r / min, and the temperature is maintained for 15-20 minutes.

[0030] As a further description of the above technical solution:

[0031] In S7, the reaction solution is marked as component B, component A is mixed with component B, and the reaction temperature is increased to 220-240° C. and maintained for 20-25 minutes.

[0032] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0033] The lubricant adopts animal fat, sodium soap and vegetable fat as main raw materials, and these materials are raw materials that are very easy to decompose in nature, so that the environmental friendliness of the overall lubricant can be greatly improved, and can be put into large-scale lubricant production. The lubricant is also provided with anti-wear extreme pressure agent, antioxidant and dispersant, and these materials can help to improve the anti-oxidation and anti-wear properties of the lubricant, so that the lubricant can be more suitable for metal wire drawing. At the same time, the materials are prepared in groups in the preparation method, and the small groups are also evenly distributed in the preparation process, which can greatly improve the fusion effect and efficiency between the components in the material, improve the quality of the final product, and the overall method has a good application effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The present invention is a flow chart of a method for preparing an environmentally friendly lubricant for metal wire drawing. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] See also Figure 1 The present invention provides a technical solution: an environmentally friendly lubricant for metal wire drawing, comprising the following materials: animal fat, sodium soap, vegetable fat, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant, with the weight proportions being 8-12 parts, 3-5 parts, 6-7 parts, 5-8 parts, 1-3 parts, 2-3 parts, 2-4 parts and 2-5 parts respectively.

[0038] This article also discloses a method for preparing an environmentally friendly lubricant for metal wire drawing, comprising the following steps:

[0039] S1. Put the anti-wear extreme pressure agent and antioxidant into the grinding equipment, control the speed of the grinding equipment to 30r / min, and grind the mixed material;

[0040] S2. After grinding, pass the ground material through an 80-mesh sieve and divide the ground material into three parts;

[0041] S3, taking animal fat, sodium soap, and vegetable fat into a melt mixing device respectively, raising the device temperature to 180°C, and controlling the mixing rate to 100r / min to mix the mixture;

[0042] S4. During the mixing process, different components of the grinding material are added into the device three times, each time interval is 5 minutes, and after the mixing is completed, the mixed liquid is taken out and marked as component A;

[0043] S5, re-take animal fat, sodium soap, and vegetable fat into the melting and mixing device respectively, increase the device temperature to 210° C., and control the mixing rate to 150 r / min to mix the mixture;

[0044] S6. Introduce stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant into the device respectively, increase the mixing rate to 180r / min, and maintain the temperature for 15min;

[0045] S7, marking the above reaction solution as component B, mixing component A with component B, raising the reaction temperature to 220°C, and maintaining for 20 minutes;

[0046] S8, waiting for the mixed liquid to cool down, and filtering it;

[0047] S9. Collect and store the finished products.

[0048] In this embodiment, the lubricant uses animal fats, sodium soaps, and vegetable fats as main raw materials. These materials are raw materials that are extremely easy to decompose in nature, which can greatly improve the environmental friendliness of the overall lubricant and can be put into large-scale lubricant production.

[0049] Example 2

[0050] See also Figure 1 The present invention provides a technical solution: an environmentally friendly lubricant for metal wire drawing, comprising the following materials: animal fat, sodium soap, vegetable fat, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant, with the weight proportions being 8-12 parts, 3-5 parts, 6-7 parts, 5-8 parts, 1-3 parts, 2-3 parts, 2-4 parts and 2-5 parts respectively.

[0051] This article also discloses a method for preparing an environmentally friendly lubricant for metal wire drawing, comprising the following steps:

[0052] S1. Put the anti-wear extreme pressure agent and antioxidant into a grinding device, control the speed of the grinding device to 40r / min, and grind the mixed material;

[0053] S2. After grinding, pass the ground material through a 90-mesh sieve and divide the ground material into 4 parts;

[0054] S3, taking animal fat, sodium soap, and vegetable fat into a melt mixing device respectively, raising the device temperature to 190°C, and controlling the mixing rate to 110r / min to mix the mixture;

[0055] S4. During the mixing process, different components of the grinding materials are added into the device 4 times, and the time interval between each addition is 7 minutes. After the mixing is completed, the mixed liquid is taken out and marked as component A.

[0056] S5, re-take animal fat, sodium soap, and vegetable fat into the melting and mixing device respectively, increase the device temperature to 220° C., and control the mixing rate to 150 r / min to mix the mixture;

[0057] S6, respectively introduce stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant into the device, increase the mixing rate to 190r / min, and maintain the temperature for 16min;

[0058] S7, marking the above reaction solution as component B, mixing component A with component B, raising the reaction temperature to 230°C, and maintaining for 22 minutes;

[0059] S8, waiting for the mixed liquid to cool down, and filtering it;

[0060] S9. Collect and store the finished products.

[0061] In this embodiment, the lubricant is also provided with an anti-wear extreme pressure agent, an antioxidant and a dispersant. These materials can help to improve the anti-oxidation and anti-wear properties of the lubricant, thereby making the lubricant more suitable for metal wire drawing processing.

[0062] Example 3

[0063] See also Figure 1 The present invention provides a technical solution: an environmentally friendly lubricant for metal wire drawing, comprising the following materials: animal fat, sodium soap, vegetable fat, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant, with the weight proportions being 8-12 parts, 3-5 parts, 6-7 parts, 5-8 parts, 1-3 parts, 2-3 parts, 2-4 parts and 2-5 parts respectively.

[0064] This article also discloses a method for preparing an environmentally friendly lubricant for metal wire drawing, comprising the following steps:

[0065] S1. Put the anti-wear extreme pressure agent and antioxidant into a grinding device, control the speed of the grinding device to 50r / min, and grind the mixed material;

[0066] S2. After grinding, pass the ground material through a 100-mesh sieve and divide the ground material into 4 parts;

[0067] S3, taking animal fat, sodium soap, and vegetable fat into a melt mixing device respectively, raising the device temperature to 200°C, and controlling the mixing rate to 120r / min to mix the mixture;

[0068] S4. During the mixing process, different components of the grinding materials are added into the device 4 times, and each addition is kept for 5-8 minutes. After the mixing is completed, the mixed liquid is taken out and marked as component A;

[0069] S5, re-take animal fat, sodium soap, and vegetable fat into the melting and mixing device respectively, increase the device temperature to 230° C., and control the mixing rate to 170 r / min to mix the mixture;

[0070] S6. Introduce stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant into the device respectively, increase the mixing rate to 200r / min, and maintain the temperature for 20min;

[0071] S7, marking the above reaction solution as component B, mixing component A with component B, raising the reaction temperature to 240°C, and maintaining for 25 minutes;

[0072] S8, waiting for the mixed liquid to cool down, and filtering it;

[0073] S9. Collect and store the finished products.

[0074] In this embodiment, the preparation method prepares the materials in groups, and during the preparation process, the small groups are also evenly distributed, which can greatly improve the fusion effect and efficiency between the components in the material, improve the quality of the final product, and the overall method has a good application effect.

[0075] Example 4

[0076] See also Figure 1 The present invention provides a technical solution: an environmentally friendly lubricant for metal wire drawing, comprising the following materials: animal fat, sodium soap, vegetable fat, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant, with the weight proportions being 8-12 parts, 3-5 parts, 6-7 parts, 5-8 parts, 1-3 parts, 2-3 parts, 2-4 parts and 2-5 parts respectively.

[0077] This article also discloses a method for preparing an environmentally friendly lubricant for metal wire drawing, comprising the following steps:

[0078] S1. Put the anti-wear extreme pressure agent and antioxidant into a grinding device, control the speed of the grinding device to 50r / min, and grind the mixed material;

[0079] S2. After grinding, pass the ground material through a 100-mesh sieve and divide the ground material into 4 parts;

[0080] S3, taking animal fat, sodium soap, and vegetable fat into a melt mixing device respectively, raising the device temperature to 200°C, and controlling the mixing rate to 120r / min to mix the mixture;

[0081] S4. During the mixing process, different components of the grinding materials are added into the device 4 times, and each addition is kept for 5-8 minutes. After the mixing is completed, the mixed liquid is taken out and marked as component A;

[0082] S5, re-take animal fat, sodium soap, and vegetable fat into the melting and mixing device respectively, increase the temperature of the device to 230° C., and control the mixing rate to 160 r / min to mix the mixture;

[0083] S6. Introduce stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant into the device respectively, increase the mixing rate to 200r / min, and maintain the temperature for 18min;

[0084] S7, marking the above reaction solution as component B, mixing component A with component B, raising the reaction temperature to 240°C, and maintaining for 25 minutes;

[0085] S8, waiting for the mixed liquid to cool down, and filtering it;

[0086] S9. Collect and store the finished products.

[0087] In this embodiment, the lubricant uses animal fats, sodium soaps, and vegetable fats as main raw materials. These materials are raw materials that are extremely easy to decompose in nature, which can greatly improve the environmental friendliness of the overall lubricant and can be put into large-scale lubricant production. The lubricant is also provided with anti-wear extreme pressure agents, antioxidants, and dispersants. These materials can help improve the lubricant's antioxidant and wear resistance, thereby making the lubricant more suitable for metal wire drawing processing. At the same time, the materials are grouped in the preparation method, and the small groups are evenly divided during the preparation process, which can greatly improve the fusion effect and efficiency between the components in the material, improve the quality of the final product, and the overall method has a good application effect.

[0088] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An environmentally friendly lubricant for metal wire drawing, characterized in that: Including the following materials: animal fats, sodium soap, vegetable fats, stearic acid, brighteners, anti-wear extreme pressure agents, antioxidants and dispersants.

2. The environmentally friendly lubricant for metal wire drawing according to claim 1, characterized in that: The weight proportions of the animal fat, sodium soap, vegetable fat, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant are 8-12 parts, 3-5 parts, 6-7 parts, 5-8 parts, 1-3 parts, 2-3 parts, 2-4 parts and 2-5 parts respectively.

3. A method for preparing an environmentally friendly lubricant for metal wire drawing, characterized in that: The steps include: S1. Put the anti-wear extreme pressure agent and antioxidant into a grinding device, control the speed of the grinding device, and grind the mixed material; S2. After grinding, sieve the ground material and divide the ground material into multiple portions; S3, taking animal fat, sodium soap, and vegetable fat into a melt mixing device respectively, increasing the temperature of the device, and controlling the mixing rate to mix the mixed materials; S4. During the mixing process, different components of the grinding materials are added into the device several times, and a certain time interval is maintained between each addition. After the mixing is completed, the mixed liquid is taken out and marked as component A; S5, re-taking animal fat, sodium soap, and vegetable fat into a melt mixing device, respectively, raising the device temperature, and controlling the mixing rate to mix the mixed materials; S6, respectively introducing stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant into the device, increasing the mixing rate, and maintaining the temperature for a period of time; S7, marking the above reaction solution as component B, mixing component A with component B, increasing the reaction temperature, and maintaining it for a period of time; S8, waiting for the mixed liquid to cool down, and filtering it; S9. Collect and store the finished products.

4. The method for preparing an environmentally friendly lubricant for metal wire drawing according to claim 3, characterized in that: In S1, anti-wear extreme pressure agent and antioxidant are put into a grinding device, and the speed of the grinding device is controlled to 30-50 r / min to grind the mixed material.

5. The method for preparing an environmentally friendly lubricant for metal wire drawing according to claim 3, characterized in that: In S2, after grinding, the ground material is passed through a 80-100 mesh sieve, and the ground material is evenly divided into 3-4 parts.

6. The method for preparing an environmentally friendly lubricant for metal wire drawing according to claim 3, characterized in that: In S3, animal fat, sodium soap and vegetable fat are respectively placed in a melting and mixing device, the temperature of the device is increased to 180-200° C., and the mixing rate is controlled to 100-120 r / min to mix the mixed materials.

7. The method for preparing an environmentally friendly lubricant for metal wire drawing according to claim 3, characterized in that: In S4, during the mixing process, the grinding materials of different components are added into the device in 3-4 times, and each addition is kept for 5-8 minutes. After the mixing is completed, the mixed liquid is taken out and marked as component A.

8. The method for preparing an environmentally friendly lubricant for metal wire drawing according to claim 3, characterized in that: In S5, animal fat, sodium soap and vegetable fat are taken again and placed in a melting and mixing device respectively, the temperature of the device is increased to 210-230° C., and the mixing rate is controlled to 150-170 r / min to mix the mixed materials.

9. The method for preparing an environmentally friendly lubricant for metal wire drawing according to claim 3, characterized in that: In S6, stearic acid, brightener, anti-wear extreme pressure agent, antioxidant and dispersant are introduced into the device respectively, the mixing rate is increased to 180-200 r / min, and the temperature is maintained for 15-20 minutes.

10. The method for preparing an environmentally friendly lubricant for metal wire drawing according to claim 3, characterized in that: In S7, the reaction solution is marked as component B, component A is mixed with component B, and the reaction temperature is increased to 220-240° C. and maintained for 20-25 minutes.