Preparation method of cast magnesium-aluminum alloy material

By coating modified diatomaceous earth modified coatings on the surface of magnesium-aluminum alloy materials, the problem of unstable corrosion resistance of magnesium-aluminum alloy materials is solved, significantly improving its corrosion resistance and service life, and enhancing market competitiveness.

CN118895446APending Publication Date: 2024-11-05FENGYANG AER SI LIGHT ALLOY PRECISION MOLDING CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410921303.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The corrosion resistance of magnesium-aluminum alloy materials is unstable, resulting in limited application prospects and shortened service life. The existing corrosion-resistant coatings have poor adhesion and short working time, so they cannot effectively improve their corrosion resistance.

Method used

The coating method is used to uniformly coat the corrosion-resistant coating on the surface of the magnesium-aluminum alloy matrix. The coating amount is controlled at 15-25g/cm2, and cured in an oven at 100-120℃ for 4-8 hours. The coating is made of epoxy resin and curing agent. , diatomaceous earth, etc., form fluorine hydrophobic chain segments through ultrasonic dispersion and catalyst modification, enhancing the density and barrier ability of the coating.

Benefits of technology

The corrosion resistance of magnesium-aluminum alloy materials is significantly improved, the corrosion rate is reduced to 0.07mg/cm2·d, which is significantly lower than 1.52mg/cm2·d of corrosion-resistant coatings, extending the service life and improving market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895446A_ABST
    Figure CN118895446A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of alloy materials, and discloses a preparation method of a cast magnesium alloy material, the surface of a magnesium-aluminum alloy matrix is uniformly coated with a corrosion-resistant coating by adopting a coating method to prepare a corrosion-resistant magnesium-aluminum alloy material, and the magnesium-aluminum alloy matrix comprises the following raw materials: silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc; according to the corrosion-resistant coating, epoxy resin serves as a film forming matter, organic kieselguhr serves as an additive, the organic kieselguhr can participate in the curing reaction of the epoxy resin, then chemical bonding of the epoxy resin and the organic kieselguhr is achieved, and meanwhile a large number of fluorine-containing hydrophobic chain segments on the surface of the kieselguhr can be utilized; and water is prevented from entering the coating to corrode the magnesium-aluminum alloy material, and the diffusion path of a corrosive medium can be prolonged by utilizing the pore structure of diatomite, so that the corrosion resistance of the epoxy resin coating is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy materials, and in particular to a method for preparing a cast magnesium-aluminum alloy material. Background Art

[0002] Magnesium or magnesium alloy is the lightest metal structural material with low density, high strength and easy recycling of waste, and is known as the green metal structural material of the 21st century. Among them, magnesium-aluminum alloy has light weight, good dimensional safety and stability, low density, high rigidity and strength. It has obvious advantages over other lightweight materials, and has low melting temperature and easy casting and processing. It is a new type of high-tech environmentally friendly material that meets the requirements of low energy consumption, environmental protection and energy saving. It is widely used in the automotive, aerospace, machinery manufacturing, chemical and electronic industries, and has broad development prospects.

[0003] In practical applications, the corrosion resistance of magnesium-aluminum alloy materials is a very important performance indicator. The unstable corrosion resistance of magnesium-aluminum alloy materials will lead to the performance of magnesium-aluminum alloy related products not reaching the ideal effect, shortening the service life, causing economic losses and industrial damage. The corrosion of magnesium-aluminum alloy materials is affected by many factors, such as alloy composition, strain rate, pH value, environmental factors, etc., which to a certain extent limit the application and promotion of magnesium-aluminum alloy materials.

[0004] There are many methods to improve the corrosion resistance of alloy materials, such as the common ones: chemical plating, surface laser cladding, plasma electrolytic oxidation, anodizing, cold spraying and organic coating, etc., and coating with corrosion-resistant coating is one of the most effective protection methods at present, with many advantages such as low cost, good effect and simple process. By coating the corrosion-resistant coating on the surface of the alloy material, the corrosion resistance of the alloy material is improved and the service life of the alloy material is increased. At present, most corrosion-resistant coatings have problems such as poor adhesion and short action time, resulting in poor corrosion resistance. The corrosion-resistant coating prepared by the present invention plays a good barrier role, enhances hardness and reduces brittleness, has high density and stability, and strong adhesion. With the development of science and technology, corrosion-resistant coatings have received attention from enterprises, and their quality requirements are also higher and their applications are more extensive. The corrosion-resistant coating is coated on the surface of the magnesium-aluminum alloy material to obtain the corrosion-resistant magnesium-aluminum alloy material, which can make the application prospects of both broader and the development technology more perfect. For this reason, the present invention proposes a preparation method of cast magnesium-aluminum alloy material. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a cast magnesium-aluminum alloy material, which solves the problem that the magnesium-aluminum alloy is not resistant to corrosion.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a cast magnesium alloy material comprises the following steps:

[0008] The corrosion-resistant coating is evenly coated on the surface of the magnesium-aluminum alloy substrate by coating method, and the coating amount is controlled to be 15-25g / cm 2 After coating, the material is cured in an oven at 100-120°C for 4-8 hours to obtain a corrosion-resistant magnesium-aluminum alloy material.

[0009] The magnesium-aluminum alloy matrix comprises the following raw materials in parts by weight: 0.3-0.4 parts of silicon, 35-46 parts of aluminum, 40-55 parts of magnesium, 0.2-0.4 parts of manganese, 0.6-1 parts of copper, 0.09-0.14 parts of iron, 0.09-0.16 parts of zirconium, and 0.38-0.42 parts of zinc;

[0010] The corrosion-resistant coating comprises the following raw materials in parts by weight: 100-120 parts of epoxy resin, 30-50 parts of curing agent, 15-25 parts of xylene, 5-15 parts of n-butanol, and 2.5-5 parts of organic diatomaceous earth.

[0011] Furthermore, the magnesium-aluminum alloy matrix is ​​prepared by the following method:

[0012] Step 1, prepare silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc raw materials for use;

[0013] Step 2: Pour silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc into a mixer, mix them evenly and pour them into a mold, and press them into a magnesium-aluminum alloy green body;

[0014] Step 3, placing the magnesium-aluminum alloy green body in a sintering furnace, introducing helium into the sintering furnace, exhausting the air in the sintering furnace, and then heating the sintering furnace to 700-900° C. until the magnesium-aluminum alloy green body is completely melted to obtain a magnesium-aluminum alloy liquid;

[0015] Step 4: Pour the magnesium-aluminum alloy liquid into the mold, take it out after it is formed, keep the formed ingot at 450-500°C for 1-3h, water quench at room temperature, and age it after quenching. The aging process is to keep it at 100-120°C for 4-6h, then adjust the temperature to 160-180°C, keep it for 6-9h, then adjust the temperature to 100-120°C, and keep it for 14-17h.

[0016] Furthermore, the epoxy resin is E44 epoxy resin, and the curing agent is methyltetrahydrophthalic anhydride.

[0017] Furthermore, the preparation method of the organic diatomaceous earth is:

[0018] Step A, adding diatomaceous earth to a mixed solution of methanol and N,N-dimethylformamide, uniformly dispersing by ultrasonication, then adding an aqueous solution of carboxyethylsilanetriol sodium salt, reacting at 50-60° C. for 6-12 hours under nitrogen protection, cooling to room temperature, centrifuging, washing, and drying to obtain modified diatomaceous earth;

[0019] Step B, adding the modified diatomaceous earth to toluene, ultrasonically dispersing, adding 3-(perfluoro-n-hexyl)propylene oxide, heating to 65-75° C. after the addition, adding a catalyst, mixing evenly, reacting for 2-4 hours, naturally cooling to room temperature, separating, and obtaining organic diatomaceous earth.

[0020] By adopting the above technical scheme, the diatomite surface contains silanol groups, which are modified by sodium carboxyethylsilanetriol and then introduced with active substituted carboxyl groups to obtain modified diatomite. Under the action of a catalyst, these active substituted carboxyl groups can undergo ring-opening esterification with the epoxy groups in 3-(perfluoro-n-hexyl)propylene oxide to form an organic diatomite with a large number of fluorine hydrophobic segments modified on the surface.

[0021] Furthermore, in step A, the average particle size of the diatomaceous earth is 5 μm.

[0022] Furthermore, in step A, the volume ratio of methanol to N,N-dimethylformamide is 4-6:1-1.5.

[0023] Furthermore, in step A, the mass fraction of the carboxyethylsilanetriol sodium salt aqueous solution is 20-30%.

[0024] Furthermore, in step B, the catalyst is any one of tetrabutylammonium hydrogen sulfate, tetrabutylammonium bromide, tetramethylammonium chloride or trioctylmethylammonium chloride.

[0025] Furthermore, the preparation method of the corrosion-resistant coating is:

[0026] Take epoxy resin and curing agent as solutes, xylene and n-butanol as solvents, mix the two to obtain a solution, add the organic diatomaceous earth obtained in step B to the solution for ultrasonic dispersion, evacuate until there are no bubbles, and let it stand at room temperature for 85-95 minutes to obtain a corrosion-resistant coating.

[0027] By adopting the above technical scheme, the surface of the organic diatomaceous earth contains hydroxyl functional groups produced by the ring-opening esterification reaction, which can participate in the curing reaction of the epoxy resin, thereby realizing the chemical bonding of the epoxy resin and the organic diatomaceous earth, avoiding the agglomeration problem of the diatomaceous earth, greatly improving the interfacial bonding force between the diatomaceous earth and the epoxy resin and the cohesive force between the molecules, filling the pore problem, enhancing the density of the coating, and improving the barrier ability, thereby enhancing the corrosion resistance of the coating.

[0028] Beneficial effects of the present invention:

[0029] 1. The present invention adopts the method of coating the magnesium-aluminum alloy material with a corrosion-resistant coating, so that the corrosion resistance of the magnesium-aluminum alloy is greatly improved, the market competitiveness of the magnesium-aluminum alloy material is improved, and it is beneficial to the subsequent use and promotion of the magnesium-aluminum alloy material.

[0030] 2. The surface of the organic diatomite prepared by the present invention contains a large number of fluorine-containing hydrophobic segments, which can make the epoxy resin coating have a strong hydrophobic effect, thereby preventing moisture from entering the coating to corrode the magnesium-aluminum alloy material. In addition, the uniform dispersion of diatomite can extend the diffusion path of the corrosive medium, thereby further improving the corrosion resistance of the epoxy resin coating. According to the test, the corrosion rate of the magnesium-aluminum alloy coated with the corrosion-resistant coating is as low as 0.07mg / cm 2 d, significantly lower than the corrosion rate of magnesium-aluminum alloy without corrosion-resistant coating on the surface (1.52 mg / cm 2 ·d.

[0031] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0033] Figure 1 It is the thermogravimetric analysis diagram of diatomite, modified diatomite and organic diatomite in the examples of the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] A method for preparing a cast magnesium-aluminum alloy material comprises the following steps:

[0037] The corrosion-resistant coating is evenly coated on the surface of the magnesium-aluminum alloy substrate by coating method, and the coating amount is controlled to be 15g / cm 2 , and then placed in an oven at 100°C for curing for 8 hours to obtain a corrosion-resistant magnesium-aluminum alloy material;

[0038] The magnesium-aluminum alloy matrix is ​​prepared by the following method:

[0039] Step 1: Take 0.3 parts of silicon, 44.5 parts of aluminum, 51.5 parts of magnesium, 0.4 parts of manganese, 0.6 parts of copper, 0.13 parts of iron, 0.15 parts of zirconium and 0.42 parts of zinc for later use;

[0040] Step 2: Pour silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc into a mixer, mix them evenly and pour them into a mold, and press them into a magnesium-aluminum alloy green body;

[0041] Step 3, placing the magnesium-aluminum alloy green body in a sintering furnace, introducing helium into the sintering furnace, exhausting the air in the sintering furnace, and then heating the sintering furnace to 700° C. until the magnesium-aluminum alloy green body is completely melted to obtain a magnesium-aluminum alloy liquid;

[0042] Step 4: Pour the magnesium-aluminum alloy liquid into the mold, take it out after it is formed, keep the formed ingot at 450°C for 3 hours, water quench at room temperature, and age it after quenching. The aging process is to keep it at 100°C for 6 hours, then adjust the temperature to 160°C, keep it for 9 hours, then adjust the temperature to 100°C, and keep it for 17 hours.

[0043] The corrosion-resistant coating is prepared by the following method:

[0044] Step A, adding 3 g of diatomaceous earth to a mixed solution of 100 mL of methanol solution and 25 mL of N,N-dimethylformamide, ultrasonically dispersing the mixture uniformly, then adding 5 mL of a 25% by mass aqueous solution of carboxyethylsilanetriol sodium salt, reacting at 60° C. for 10 h under nitrogen protection, cooling to room temperature, centrifuging, washing, and drying to obtain modified diatomaceous earth;

[0045] Step B: add 2.5 g of modified diatomaceous earth to toluene, disperse by ultrasonication, add 2.5 g of 3-(perfluoro-n-hexyl)propylene oxide, raise the temperature to 75° C., add 0.5 g of tetrabutylammonium hydrogen sulfate as a catalyst, mix well, react for 3 h, cool naturally to room temperature, separate, and obtain organic diatomaceous earth.

[0046] Thermogravimetric analysis was used to characterize diatomite, modified diatomite and organic diatomite. Figure 1 It can be seen that under high temperature conditions, the final mass retention rate of diatomite is 96.3%, and the lost part is caused by the evaporation of crystalline water in the diatomite structure; the final mass retention rate of modified diatomite is 37.5%, and the lost part is caused by the thermal decomposition of carboxyethylsilanetriol sodium salt; the final mass retention rate of organic diatomite is 17.7%, which is caused by the thermal decomposition of organic matter on the organic diatomite.

[0047] Step C, weigh 100g of E44 epoxy resin and 35g of curing agent methyltetrahydrophthalic anhydride as solute, 21g of xylene and 9g of n-butanol as solvent, mix the two to obtain a solution, add 2.5g of organic diatomaceous earth obtained in step B to the solution, ultrasonicate, disperse evenly, evacuate until there are no bubbles, and let stand at room temperature for 90min to obtain a corrosion-resistant coating.

[0048] Example 2

[0049] A method for preparing a cast magnesium-aluminum alloy material comprises the following steps:

[0050] The corrosion-resistant coating is evenly coated on the surface of the magnesium-aluminum alloy substrate by coating method, and the coating amount is controlled to be 20g / cm 2 , and then placed in an oven at 110°C for curing for 7 hours to obtain a corrosion-resistant magnesium-aluminum alloy material.

[0051] The magnesium-aluminum alloy matrix is ​​prepared by the following method:

[0052] Step 1: Take 0.3 parts of silicon, 40.5 parts of aluminum, 55.5 parts of magnesium, 0.4 parts of manganese, 0.6 parts of copper, 0.13 parts of iron, 0.15 parts of zirconium and 0.42 parts of zinc for later use;

[0053] Step 2: Pour silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc into a mixer, mix them evenly and pour them into a mold, and press them into a magnesium-aluminum alloy green body;

[0054] Step 3: placing the magnesium-aluminum alloy green body in a sintering furnace, introducing helium into the sintering furnace, exhausting the air in the sintering furnace, and then heating the sintering furnace to 800° C. to melt the magnesium-aluminum alloy green body completely to obtain magnesium-aluminum alloy liquid;

[0055] Step 4: Pour the magnesium-aluminum alloy liquid into the mold, take it out after it is formed, keep the formed ingot at 480°C for 2 hours, water quench it at room temperature, and age it after quenching. The aging process is to keep it at 110°C for 5 hours, then adjust the temperature to 170°C, keep it for 8 hours, and then adjust the temperature to 110°C and keep it for 16 hours.

[0056] The preparation method of the corrosion-resistant coating is the same as that in Example 1.

[0057] Example 3

[0058] A method for preparing a cast magnesium-aluminum alloy material comprises the following steps:

[0059] The corrosion-resistant coating is evenly coated on the surface of the magnesium-aluminum alloy substrate by coating method, and the coating amount is controlled to be 25g / cm 2 , and then placed in an oven at 120°C for curing for 6 hours to obtain a corrosion-resistant magnesium-aluminum alloy material.

[0060] The magnesium-aluminum alloy matrix is ​​prepared by the following method:

[0061] Step 1: Take 0.3 parts of silicon, 36.5 parts of aluminum, 59.5 parts of magnesium, 0.4 parts of manganese, 0.6 parts of copper, 0.13 parts of iron, 0.15 parts of zirconium and 0.42 parts of zinc for later use;

[0062] Step 2: Pour silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc into a mixer, mix them evenly and pour them into a mold, and press them into a magnesium-aluminum alloy green body;

[0063] Step 3: placing the magnesium-aluminum alloy green body in a sintering furnace, introducing helium into the sintering furnace, exhausting the air in the sintering furnace, and then heating the sintering furnace to 900° C. to melt the magnesium-aluminum alloy green body completely to obtain magnesium-aluminum alloy liquid;

[0064] Step 4: Pour the magnesium-aluminum alloy liquid into the mold, take it out after it is formed, keep the formed ingot at 500°C for 1 hour, water quench at room temperature, and age it after quenching. The aging process is to keep it at 120°C for 4 hours, then adjust the temperature to 180°C, keep it for 6 hours, then adjust the temperature to 120°C, and keep it for 15 hours.

[0065] The preparation method of the corrosion-resistant coating is the same as that in Example 1.

[0066] Comparative Example 1

[0067] A method for preparing a cast magnesium-aluminum alloy material comprises the following steps:

[0068] The magnesium-aluminum alloy matrix is ​​prepared by the following method:

[0069] Step 1: Take 0.3 parts of silicon, 40.5 parts of aluminum, 55.5 parts of magnesium, 0.4 parts of manganese, 0.6 parts of copper, 0.13 parts of iron, 0.15 parts of zirconium and 0.42 parts of zinc for later use;

[0070] Step 2: Pour silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc into a mixer, mix them evenly and pour them into a mold, and press them into a magnesium-aluminum alloy green body;

[0071] Step 3: placing the magnesium-aluminum alloy green body in a sintering furnace, introducing helium into the sintering furnace, exhausting the air in the sintering furnace, and then heating the sintering furnace to 800° C. to melt the magnesium-aluminum alloy green body completely to obtain magnesium-aluminum alloy liquid;

[0072] Step 4: Pour the magnesium-aluminum alloy liquid into the mold, take it out after it is formed, keep the formed ingot at 480°C for 2 hours, water quench it at room temperature, and age it after quenching. The aging process is to keep it at 110°C for 5 hours, then adjust the temperature to 170°C, keep it for 8 hours, and then adjust the temperature to 110°C and keep it for 16 hours.

[0073] Performance Testing

[0074] Corrosion resistance test of a cast magnesium-aluminum alloy material prepared in Examples 1 to 3 of the present invention and Comparative Example 1:

[0075] The present invention conducts a salt spray test to simulate atmospheric corrosion, and the test is conducted in a salt spray test box. A 5% mass fraction NaCl solution is prepared as a test solution, the experimental temperature is 35°C, the air pressure of the atomized salt solution is maintained within the range of 125kPa, the pH value is 6.5, and the spray is continuously sprayed. The magnesium-aluminum alloy material atomized for 168h is analyzed, and the corrosion rate is calculated using the weight loss rate before and after corrosion. The measurement results are shown in Table 1:

[0076] Table 1 - Salt spray test results of magnesium aluminum alloy matrix

[0077] <![CDATA[Corrosion rate mg / cm 2 ·d]]> Example 1 0.15 Example 2 0.07 Example 3 0.13 Comparative Example 1 1.52

[0078] It can be concluded from the data in Table 1 that the magnesium-aluminum alloy materials coated with corrosion-resistant coatings prepared in Examples 1 to 3 of the present invention have good corrosion resistance, and the corrosion rate is as low as 0.07 mg / cm 2 d; Comparative Example 1 added a magnesium-aluminum alloy material without corrosion-resistant coating, which could not utilize the large amount of fluorine-containing hydrophobic segments on the surface of the organic diatomite to prevent moisture from entering the coating to corrode the magnesium-aluminum alloy. The corrosion rate was 1.52 mg / cm 2 d. Poor corrosion resistance.

[0079] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a cast magnesium alloy material, characterized in that: The following steps are involved: The corrosion-resistant coating is evenly coated on the surface of the magnesium-aluminum alloy substrate by coating method, and the coating amount is controlled to be 15-25g / cm 2 After coating, the material is cured in an oven at 100-120°C for 4-8 hours to obtain a corrosion-resistant magnesium-aluminum alloy material. The magnesium-aluminum alloy matrix comprises the following raw materials in parts by weight: 0.3-0.4 parts of silicon, 35-46 parts of aluminum, 40-55 parts of magnesium, 0.2-0.4 parts of manganese, 0.6-1 parts of copper, 0.09-0.14 parts of iron, 0.09-0.16 parts of zirconium, and 0.38-0.42 parts of zinc; The corrosion-resistant coating comprises the following raw materials in parts by weight: 100-120 parts of epoxy resin, 30-50 parts of curing agent, 15-25 parts of xylene, 5-15 parts of n-butanol, and 2.5-5 parts of organic diatomaceous earth.

2. The method for preparing a cast magnesium alloy material according to claim 1, characterized in that: The magnesium-aluminum alloy matrix is ​​prepared by the following method: Step 1, prepare silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc raw materials for later use; Step 2: Pour silicon, aluminum, magnesium, manganese, copper, iron, zirconium and zinc into a mixer, mix them evenly and pour them into a mold, and press them into a magnesium-aluminum alloy green body; Step 3, placing the magnesium-aluminum alloy green body in a sintering furnace, introducing helium into the sintering furnace, exhausting the air in the sintering furnace, and then heating the sintering furnace to 700-900° C. until the magnesium-aluminum alloy green body is completely melted to obtain a magnesium-aluminum alloy liquid; Step 4: Pour the magnesium-aluminum alloy liquid into the mold, take it out after it is formed, keep the formed ingot at 450-500°C for 1-3h, water quench at room temperature, and age it after quenching. The aging process is to keep it at 100-120°C for 4-6h, then adjust the temperature to 160-180°C, keep it for 6-9h, then adjust the temperature to 100-120°C, and keep it for 14-17h.

3. The method for preparing a cast magnesium alloy material according to claim 1, characterized in that: The epoxy resin is E44 epoxy resin, and the curing agent is methyltetrahydrophthalic anhydride.

4. The method for preparing a cast magnesium alloy material according to claim 1, characterized in that: The preparation method of the organic diatomaceous earth is: Step A, adding diatomaceous earth to a mixed solution of methanol and N,N-dimethylformamide, uniformly dispersing by ultrasonication, then adding an aqueous solution of carboxyethylsilanetriol sodium salt, reacting at 50-60° C. for 6-12 hours under nitrogen protection, cooling to room temperature, centrifuging, washing, and drying to obtain modified diatomaceous earth; Step B, adding the modified diatomaceous earth to toluene, ultrasonically dispersing, adding 3-(perfluoro-n-hexyl)propylene oxide, heating to 65-75° C. after the addition, adding a catalyst, mixing evenly, reacting for 2-4 hours, naturally cooling to room temperature, separating, and obtaining organic diatomaceous earth.

5. The method for preparing a cast magnesium alloy material according to claim 4, characterized in that: In step A, the average particle size of the diatomaceous earth is 5 μm.

6. The method for preparing a cast magnesium alloy material according to claim 4, characterized in that: In step A, the volume ratio of methanol to N,N-dimethylformamide is 4-6:1-1.

5.

7. The method for preparing a cast magnesium alloy material according to claim 4, characterized in that: In step A, the mass fraction of the carboxyethylsilanetriol sodium salt aqueous solution is 20-30%.

8. The method for preparing a cast magnesium alloy material according to claim 4, characterized in that: In step B, the catalyst is any one of tetrabutylammonium hydrogen sulfate, tetrabutylammonium bromide, tetramethylammonium chloride or trioctylmethylammonium chloride.

9. The method for preparing a cast magnesium alloy material according to claim 1, characterized in that: The preparation method of the corrosion-resistant coating is: Take epoxy resin and curing agent as solutes, xylene and n-butanol as solvents, mix the two to obtain a solution, add the organic diatomaceous earth obtained in step B to the solution for ultrasonic dispersion, evacuate until there are no bubbles, and let it stand at room temperature for 85-95 minutes to obtain a corrosion-resistant coating.

Citation Information

Cited By

  • Corrosion-resistant aluminum profile machining process

    CN120326293A