High-thermal-conductivity VNi alloy plate without neutron diffraction peak and manufacturing method of high-thermal-conductivity VNi alloy plate

By precisely proportioning high-purity vanadium and nickel raw materials and employing vacuum arc melting and hot processing techniques, VNi alloy plates with no neutron diffraction peaks and high thermal conductivity were prepared. This solved the problems of signal interference and poor plasticity in neutron scattering experiments, and improved experimental efficiency and material applicability.

CN118895451AActive Publication Date: 2024-11-05CHINA SPALLATION NEUTRON SOURCE SCI CENT +1

Patent Information

Application Number
CN202410899853.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-05
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

Existing vanadium and TiZr alloys suffer from problems such as interference signals from neutron diffraction peaks, poor processing plasticity, and poor thermal conductivity in neutron scattering experiments, which limit the efficiency and cost of neutron testing experiments under high and low temperature environments.

Method used

A neutron-free, high-thermal-conductivity VNi alloy plate was developed by precisely proportioning high-purity vanadium and nickel raw materials and employing vacuum arc melting, homogenization treatment, and hot working processes to ensure the uniformity and plasticity of the alloy composition, thus producing a neutron-free, high-thermal-conductivity alloy plate.

Benefits of technology

This invention achieves interference-free signal, excellent thermal conductivity and good plasticity in alloy plates for neutron scattering experiments, making them suitable for sample containers and neutron beam windows. It improves experimental efficiency and reliability under high and low temperature environments and has broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895451A_ABST
    Figure CN118895451A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of neutron scattering experiments, in particular to a neutron-diffraction-peak-free and high-thermal-conductivity VNi alloy plate for a neutron scattering experiment and a manufacturing method of the neutron-diffraction-peak-free and high-thermal-conductivity VNi alloy plate. The plate is composed of vanadium (V) and nickel (Ni), the mass percent of vanadium is 40%-60%, the mass percent of nickel is 40%-60%, the alloy plate has no neutron diffraction peak, and the theoretical thermal conductivity at the room temperature is not lower than 27 W / (m * K); the sample container has good processing plasticity, and meets the requirements of neutron scattering experiments on the sample container and the neutron beam window and the requirements of efficient high and low temperature in-situ experiments; the VNi plate prepared through the method is uniform in component and free of neutron diffraction peaks, meets the requirements of neutron scattering experiments and has excellent heat conductivity. The VNi plate prepared through the method is uniform in component and free of neutron diffraction peaks, has good stretching forming plasticity and meets the processing and preparing requirements of further finished products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of neutron scattering experiments, and in particular to a VNi alloy plate with no neutron diffraction peak and high thermal conductivity for neutron scattering experiments and a manufacturing method thereof. Background Art

[0002] In neutron scattering experiments, the selection of sample containers and neutron beam window materials has an important impact on the quality of experimental data. Currently, metal vanadium and TiZr alloys are commonly used as sample containers, and V or Al is used as neutron beam window materials, but these materials have certain problems. Metal vanadium and aluminum have neutron diffraction peaks, which will seriously interfere with the experimental sample signal and affect the acquisition of subsequent neutron diffraction data. Although TiZr alloy does not have a neutron diffraction peak, its processing plasticity is poor, the manufacturing cost is high, and the thermal conductivity is poor, which limits the efficiency of neutron testing experiments in high and low temperature sample environments.

[0003] The existing TiZr alloy manufacturing process has the problems of low production efficiency and high cost. In addition, due to the poor thermal conductivity of the alloy, the sample heating and cooling speed is slow in high and low temperature sample environments, which greatly limits the application of neutron testing experiments in high and low temperature environments. At present, although the composition of VNi alloy for neutron scattering experiments has been determined, the composition control accuracy of the smelting method is still a challenge, which makes large-scale processing and application difficult. In addition, VNi alloy has extremely strong oxygen affinity, which makes traditional hot rolling process unsuitable for the processing and preparation of alloy plates. At the same time, due to the low plasticity of VNi alloy, the existing cold rolling preparation process is also not suitable for this new alloy. Summary of the invention

[0004] In order to solve the above problems, it is urgent to develop a new type of alloy and a corresponding manufacturing process to meet the high requirements of neutron scattering experiments on sample containers and neutron beam windows, and to improve the efficiency of neutron testing experiments in high and low temperature environments; the present invention is proposed based on this demand.

[0005] The technical solution adopted by the present invention is: a VNi alloy plate with no neutron diffraction peak and high thermal conductivity, the plate is composed of vanadium (V) and nickel (Ni), wherein the mass percentage of vanadium is 40% to 60%, and the mass percentage of nickel is 40% to 60%. The alloy plate has no neutron diffraction peak, and the theoretical thermal conductivity at room temperature is not less than 27W / (m*K); and has good processing plasticity, meeting the requirements of neutron scattering experiments for sample holding containers and neutron beam windows, as well as the needs of efficient high and low temperature in-situ experiments.

[0006] The plate is obtained after homogenization treatment and heat treatment, ensuring that the internal composition of the alloy is uniform without obvious component segregation.

[0007] The shape of the plate includes but is not limited to a flat plate, a round plate, and a square plate, and the thickness of the plate can be adjusted as needed.

[0008] A method for manufacturing a VNi alloy plate having no neutron diffraction peak and high thermal conductivity, the manufacturing method mainly comprising the following steps:

[0009] (1) Preparation of alloy raw materials: First, high-purity vanadium (V) and nickel (Ni) raw materials need to be prepared;

[0010] (2) Smelting process: the prepared vanadium and nickel are mixed according to a predetermined mass percentage, and placed in a vacuum arc melting furnace or a vacuum induction furnace for smelting to form an alloy billet;

[0011] (3) Homogenization treatment: The alloy blank in (2) is subjected to homogenization treatment to ensure uniform distribution of components inside the alloy;

[0012] (4) Hot working: The alloy blank after homogenization treatment is subjected to hot working, including forging, rolling, etc., to obtain alloy plates of the desired shape and size; during the hot working process, multiple annealing-rolling cycles may be required to obtain the ideal plate thickness and mechanical properties.

[0013] (5) Quality inspection: Finally, the quality inspection of the prepared alloy plates is carried out, including composition analysis, thermal conductivity testing, processing plasticity evaluation, and neutron diffraction peak detection to ensure that the plates meet the requirements of the neutron scattering experiment.

[0014] In step (1), the ratio of the alloy raw materials is determined according to the required mass percentages of vanadium and nickel, so that the purity of the raw materials reaches a certain standard, wherein the purity of vanadium is better than 99.9% and the purity of nickel is better than 99.99%, to ensure the quality of the final alloy.

[0015] In step (2), the vacuum degree needs to be controlled during the smelting process. The vacuum degree is controlled to be better than 6.678*10-3Pa during the smelting process to ensure the purity of the alloy and prevent impurities from entering the alloy.

[0016] Step (3) is carried out in a high temperature furnace, wherein the temperature of the homogenization treatment is controlled between 800° C. and 1100° C., and the treatment time is not less than 24 hours.

[0017] A VNi alloy plate with no neutron diffraction peak and high thermal conductivity is used for manufacturing a sample holding container or a neutron beam window for neutron scattering experiments.

[0018] The beneficial effects achieved by the present invention are: the VNi plate prepared by the present invention has uniform composition, no neutron diffraction peak, meets the requirements of neutron scattering experiments, and has excellent thermal conductivity; the VNi plate prepared by this method has uniform composition, no neutron diffraction peak, and has good tensile forming plasticity, which meets the processing and preparation requirements of further finished products, which are specifically embodied as follows: (1) It has excellent physical properties: Through precise proportions and unique processing technology, the alloy plate exhibits excellent physical properties. High-purity raw materials ensure the purity of the alloy, thereby improving its overall mechanical properties and stability; (2) It has excellent high thermal conductivity: The alloy plate prepared by this technical solution has excellent thermal conductivity. This feature gives it a significant advantage in application scenarios that require efficient heat conduction, such as heat sinks and heat exchangers. (3) No neutron diffraction peak: This technical solution successfully eliminates the neutron diffraction peak, which means that when conducting neutron scattering experiments, the plate will not generate interference signals, thereby ensuring the accuracy and reliability of the experiment. (4) Has a wide range of application prospects: This alloy plate is not only suitable for neutron scattering experiments, but can also play an important role in high-end fields such as aerospace, nuclear industry, and chemical industry. Its excellent high temperature resistance and corrosion resistance make it an ideal material for working in extreme environments. (5) Has high quality standards: Through a strict quality inspection process, including composition analysis, thermal conductivity testing, etc., it is ensured that each alloy plate meets extremely high quality standards. This provides users with a reliable product guarantee and reduces the risk of use; (6) Can promote the development of related industries: The innovation and practicality of this technical solution is expected to promote the technological upgrading and product innovation of the related industrial chain, and make positive contributions to the country's scientific and technological development and industrial upgrading; In summary, this technical solution has successfully prepared alloy plates with excellent physical properties, high thermal conductivity and no neutron diffraction peaks through unique processing technology and high-quality raw materials, providing strong material support for applications in multiple fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram of the process flow of the preparation method of the present invention.

[0020] Figure 2 It is the neutron diffraction spectrum of the VNi alloy in the present invention.

[0021] Figure 3 It is the neutron diffraction spectrum of the VNi alloy plate in the present invention.

[0022] Figure 4 These are the mechanical properties of the VNi alloy 0.2 mm plate in the present invention. DETAILED DESCRIPTION

[0023] The specific implementation of the present invention is described in detail below with reference to the accompanying drawings:

[0024] like Figure 1 As shown, the present invention provides a neutron-free diffraction peak, high thermal conductivity VNi alloy plate for neutron scattering experiments and a manufacturing method thereof, including precise alloy composition control. By optimizing the steps of smelting, alloying, cooling solidification, rolling, etc., high-precision, high-efficiency, low-cost, and high-quality alloy plate processing and manufacturing are achieved, as follows:

[0025] Stage 1: Melting stage (vacuum suspension melting): The bulk V with a purity better than 99.9% and the single Ni with a purity better than 99.99% are alloyed according to the ratio, and the raw materials are washed with 10% HCl solution to remove the surface oxide layer. Vacuum arc melting is adopted, the melting process current is 300A, the refining time is 7 minutes, the power is slowly reduced to the minimum, and the furnace is cooled for 1 hour. The vacuum degree during the melting process is better than 6.678*10-3Pa, and 200g alloy ingots are obtained.

[0026] Stage 2: Multiple small ingots from stage 1 were melted together for 4 times. The first melting power was 275KW, the second melting power was 280KW, and then the power was reduced to 230KW. The third melting power was 260KW, and it dropped to 220KW with slight splashing. Each melting and refining time was 7 minutes, and the cooling time was 1 hour, to prepare kilogram-level alloy ingots with uniform composition.

[0027] Stage three: homogenization treatment: the alloy ingot is placed in a high temperature furnace at 800℃-1100℃ for more than 24 hours for homogenization treatment.

[0028] In stage 4, the homogenized bars are forged at temperatures above 700°C-1200°C to obtain bars or plates of ideal size.

[0029] In stage five, the prepared block is subjected to vacuum annealing treatment at 700°C-1000°C (vacuum better than 10-3Pa) for more than 1 hour, and then cold rolled using a two-roll rolling mill with a deformation amount not exceeding 20%. The annealing-rolling cycle is repeated until the plate has an ideal thickness.

[0030] The present invention adopts a distributed smelting method to ensure that the composition deviation of the entire alloy in different parts of the alloy ingot is less than 0.1wt%, thereby realizing high-precision preparation of alloy ingot composition control; secondly, since VNi has poor oxidation resistance and low tensile deformation capacity, this patent adopts a vacuum annealing process in the cold rolling gap, and realizes the processing and preparation of VNi alloy sheets by optimizing process parameters, the thinnest of which can be as thin as 50 microns.

[0031] Example 1: Distributed smelting method is used to ensure uniform alloy composition

[0032] Step 1: Fine smelting: Prepare alloys according to the ratio of bulk V with a purity better than 99.9% and single Ni with a purity better than 99.99%. The raw materials are washed with 10% HCl solution to remove the surface oxide layer. Vacuum arc melting is used, the current during the melting process is 300A, the refining time is 7 minutes, the power is slowly reduced to the minimum, and the furnace is cooled for 1 hour. The vacuum degree during the melting process is better than 6.678*10-3Pa, and 200g alloy ingots are obtained.

[0033] Step 2: Mixed smelting: Melt the multiple small ingots in stage 1 together for 4 times. The first smelting power is 275KW, the second smelting power is 280KW, and the power is reduced to 230KW. The third smelting power is 260KW, and it is reduced to 220KW with slight splashing. The smelting and refining time for each time is 7 minutes, and the cooling time is 1 hour to prepare kilogram-level alloy ingots with uniform composition.

[0034] Step three: homogenization treatment: the alloy ingot is placed in a high temperature furnace at 800°C-1100°C for more than 24 hours for homogenization treatment.

[0035] Step 4: The homogenized rods are forged at a temperature above 700°C-1200°C to obtain rods or plates of ideal size.

[0036] Step five, subjecting the prepared block to vacuum annealing treatment at 700°C-1000°C (vacuum better than 10-3Pa) for more than 1 hour. This step is the key to the sheet rolling process.

[0037] Step six, cold rolling is then carried out using a two-roll rolling mill with a deformation amount not exceeding 20%, and the annealing-rolling cycle is repeated until the plate has a desired thickness.

[0038] Example 2: Preparation of VNi alloy sheet

[0039] Step 1: Preparation of alloy raw materials: Select vanadium raw materials with a purity of 99.99% and nickel raw materials with a purity of 99.999%, and accurately weigh them according to the mass percentage of 60% vanadium and 40% nickel.

[0040] Step 2: Melting process: Put the weighed vanadium and nickel raw materials into the vacuum arc melting furnace, control the vacuum degree in the furnace to 6.67×10^-4Pa, and start arc melting. Keep the current stable during the melting process to ensure that the alloy components are evenly mixed.

[0041] Step 3: Homogenization treatment: Place the smelted alloy ingot into a high-temperature furnace for homogenization treatment at a temperature of 1000°C for 48 hours to ensure uniform internal structure of the alloy and eliminate internal stress.

[0042] Step 4: Hot working: The alloy ingot after homogenization treatment is forged and rolled. First, multiple forgings are performed to deform the alloy ingot and refine the grains, and then hot rolling is performed to obtain the required thickness of the plate. During the rolling process, the rolling temperature and rolling speed are controlled to obtain the ideal plate performance.

[0043] Step 5: Quality inspection: Conduct quality inspection on the prepared VNi alloy plates, including composition analysis, thermal conductivity test, processing plasticity evaluation, etc. Ensure that the plate composition is accurate, the thermal conductivity is high, the processing plasticity is good, and the requirements for materials in neutron scattering experiments are met.

[0044] Example 3: Optimizing the preparation process of VNi alloy sheet

[0045] Step 1: Alloy raw material preparation and optimization

[0046] Select higher purity vanadium raw materials (99.999%) and nickel raw materials (99.9999%), and accurately weigh them according to the optimized mass percentage of 55% vanadium and 45% nickel. By optimizing the purity of raw materials and alloy ratio, the performance of alloy plates can be further improved.

[0047] Step 2: Smelting and refining process

[0048] The weighed vanadium and nickel raw materials are placed in a vacuum induction furnace for smelting, and the vacuum degree in the furnace is controlled to a higher level of 6.67×10 -5 Pa. Refining agents are added during the smelting process to further remove impurities and gases in the alloy and improve the purity of the alloy.

[0049] Step 3: Homogenization and heat treatment

[0050] After the smelted alloy liquid is cast into ingots, it is homogenized and heat treated. The homogenization temperature is 1100℃ and the treatment time is 72 hours to ensure that the alloy composition is more uniform. The heat treatment includes solution treatment and aging treatment to improve the strength and hardness of the alloy.

[0051] Step 4: Precision heat treatment

[0052] The heat-treated alloy ingot is precision forged and rolled. By controlling the forging temperature and deformation, as well as the rolling speed and the number of rolling passes, the grains are further refined and the density of the sheet is improved. Finally, an alloy sheet with a more uniform thickness and a smoother surface is obtained.

[0053] Step 5: Comprehensive quality inspection and evaluation

[0054] The prepared optimized VNi alloy plates are comprehensively tested and evaluated for quality. In addition to conventional composition analysis, thermal conductivity testing and processing plasticity evaluation, neutron diffraction peak detection and corrosion resistance testing are also added to ensure that the plates not only meet the requirements of neutron scattering experiments, but also have better corrosion resistance and longer service life.

[0055] It should be noted that, according to the basic properties of vanadium (V) and nickel (Ni) alloys and their applications in materials science, especially the related properties of neutron diffraction, high thermal conductivity and processing plasticity, the content of vanadium and nickel in the alloy has a significant influence on the alloy properties (such as thermal conductivity, processing plasticity, etc.). Therefore, the mass percentages of vanadium (V) and nickel (Ni) in the embodiments of the present invention are the results of multiple experiments based on material properties.

Claims

1. A neutron-free diffraction peak, high thermal conductivity VNi alloy plate, characterized by: The plate is composed of vanadium (V) and nickel (Ni), wherein the mass percentage of vanadium is 40% to 60%, and the mass percentage of nickel is 40% to 60%. The alloy plate has no neutron diffraction peak, and the theoretical thermal conductivity at room temperature is not less than 27W / (m*K); and has good processing plasticity, meeting the requirements of neutron scattering experiments for sample holding containers and neutron beam windows, as well as the needs of efficient high and low temperature in-situ experiments.

2. The VNi alloy plate with no neutron diffraction peak and high thermal conductivity according to claim 1, characterized in that: The plate is obtained after homogenization treatment and heat treatment, ensuring that the internal composition of the alloy is uniform without obvious component segregation.

3. The VNi alloy plate with no neutron diffraction peak and high thermal conductivity according to claim 1, characterized in that: The shape of the plate includes but is not limited to a flat plate, a round plate, and a square plate, and the thickness of the plate can be adjusted as needed.

4. A method for manufacturing a VNi alloy plate having no neutron diffraction peak and high thermal conductivity, characterized in that: The manufacturing method mainly comprises the following steps: (1) Preparation of alloy raw materials: First, high-purity vanadium (V) and nickel (Ni) raw materials need to be prepared; (2) Smelting process: the prepared vanadium and nickel are mixed according to a predetermined mass percentage, and placed in a vacuum arc melting furnace or a vacuum induction furnace for smelting to form an alloy billet; (3) Homogenization treatment: The alloy blank in (2) is subjected to homogenization treatment to ensure uniform distribution of components inside the alloy; (4) Hot working: The alloy blank after homogenization is hot worked, including forging, rolling, etc., to obtain alloy plates of the desired shape and size. During the hot working process, multiple annealing-rolling cycles may be required to obtain the desired plate thickness and mechanical properties. (5) Quality inspection: Finally, the quality inspection of the prepared alloy plates is carried out, including composition analysis, thermal conductivity test, processing plasticity evaluation and neutron diffraction peak detection, to ensure that the plates meet the requirements of the neutron scattering experiment.

5. The method for manufacturing a neutron-free diffraction peak and high thermal conductivity VNi alloy sheet according to claim 4, characterized in that: In step (1), the ratio of the alloy raw materials is determined according to the required mass percentages of vanadium and nickel, so that the purity of the raw materials reaches a certain standard, wherein the purity of vanadium is better than 99.9% and the purity of nickel is better than 99.99%, to ensure the quality of the final alloy.

6. The method for manufacturing a neutron-free diffraction peak and high thermal conductivity VNi alloy sheet according to claim 4, characterized in that: In step (2), the vacuum degree needs to be controlled during the smelting process. The vacuum degree is controlled to be better than 6.678*10-3Pa during the smelting process to ensure the purity of the alloy and prevent impurities from entering the alloy.

7. The method for manufacturing a neutron-free diffraction peak and high thermal conductivity VNi alloy sheet according to claim 4, characterized in that: Step (3) is carried out in a high temperature furnace, wherein the temperature of the homogenization treatment is controlled between 800° C. and 1100° C., and the treatment time is not less than 24 hours.

8. The neutron-free diffraction peak and high thermal conductivity VNi alloy sheet according to any one of claims 1 to 7 is used, characterized in that: Used to manufacture sample containers or neutron beam windows for neutron scattering experiments.

Citation Information

Patent Citations

  • Novel helium ion sputtering-resistant vanadium alloy and preparation method thereof

    CN105506428A

  • Gadolinium iron alloy foil with high-neutron absorption performance and preparation method of gadolinium iron alloy foil

    CN109628816A

  • Vanadium-nickel alloy for neutron scattering experiment as well as preparation method and application of vanadium-nickel alloy

    CN115747536A

  • High-strength high-thermal-conductivity wrought nickel alloy

    WO2015100074A1

  • Iron-based alloy and method for producing iron-based alloy

    WO2020050229A1

Cited By

  • Anti-oxidation zero-coherence scattering alloy with BCC structure and preparation method of anti-oxidation zero-coherence scattering alloy

    CN120555853A

  • Neutron diffraction vectorization generation and identification method

    CN120877915A

  • Neutron diffraction vectorization generation and identification method

    CN120877915B