Q420qFNHY steel plate resistant to marine atmospheric environment corrosion and production method of Q420qFNHY steel plate

By rationally designing the chemical composition and production process of Q420qFNHY steel plate, the problem of failure of existing bridge steel in marine atmospheric environments is solved, and corrosion resistance and strength in high salt spray and high humidity and heat environments are achieved, meeting the manufacturing needs of large bridges , and reduce maintenance costs.

CN118895458AActive Publication Date: 2024-11-05NANYANG HANYE SPECIAL STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410909119.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-05
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The existing bridge steel that is resistant to marine atmospheric environment fails in high salt spray and high humidity and heat environments. The traditional coating method is costly and environmentally polluted, and the existing methods are difficult to meet the corrosion resistance needs of large-thickness bridges.

Method used

Using Q420qFNHY steel plate, the chemical composition is reasonably designed, containing 0.04-0.08% C, 0.10-0.20% Si, 0.70-1.50% Mn, etc., the grains are refined by Nb, V, and Ti, and Ni forms a dense rust layer. Increase hardenability, control Ni content between 3.5-4.0% to improve corrosion resistance, and use multi-stage rolling, cold-controlled and heat treatment processes to produce.

Benefits of technology

Steel plates show excellent corrosion resistance, strength and low-temperature impact toughness in the marine atmosphere, meeting the manufacturing needs of large cross-sea bridges, reducing maintenance costs, and reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004933029480000061
    Figure BDA0004933029480000061
  • Figure BDA0004933029480000121
    Figure BDA0004933029480000121
  • Figure FDA0004933029470000021
    Figure FDA0004933029470000021
Patent Text Reader

Abstract

The invention discloses a Q420qFNHY steel plate resistant to marine atmospheric environment corrosion and a production method of the Q420qFNHY steel plate, the thickness of the steel plate is 60-150 mm, and the steel plate comprises the following chemical components in percentage by mass: 0.04-0.08% of C, 0.10-0.20% of Si, 0.70-1.50% of Mn, less than or equal to 0.016% of P, less than or equal to 0.002% of S, 0.025-0.045% of Als, 0.025-0.040% of Nb, 0.010-0.65% of V, 3.50-4.00 wt% of Ni, 0.10-0.15% of Mo, 0.30-0.1.0% of Cu, less than or equal to 0.012% of Ti, less than or equal to 0.0005% of B and the balance of Fe and residual elements. The Q420qFNHY steel plate for resisting corrosion in the marine atmospheric environment can be used under the conditions that the annual average chloride ion deposition rate is less than or equal to 0.60 mdd and the annual average SO2 deposition rate is less than or equal to 2mdd in the marine atmosphere. The steel plate produced through the method is reasonable in matching of chemical components and matrix structures, can have high strength, low Pcm and excellent low-temperature impact toughness and marine atmosphere corrosion resistance at the same time, meets the requirements of industrial production and conforms to construction and manufacturing of large sea-crossing bridges.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wide and thick plate metallurgy, and specifically relates to a Q420qFNHY steel plate resistant to marine atmospheric corrosion and a production method thereof. Background Art

[0002] At present, the weather-resistant bridge steel developed in my country is mainly used in rural pastoral atmospheric environments without obvious corrosive pollution, or in densely populated urban environments with a small amount of corrosive pollution. These environments basically do not have accelerated corrosion particles such as Cl- and SO2, and the traditional weather-resistant bridge steel in GB / 714-2015 can meet the use requirements. However, with the development of my country's infrastructure, there are more and more coastal and cross-sea bridge projects. In this kind of strong radiation, long sunshine, high salt fog, high humidity and heat environment, ordinary weathering steel will quickly fail and break. Therefore, in order to ensure the corrosion resistance of bridge steel in the marine atmospheric environment, the method of brushing corrosion-resistant materials is generally used to solve the problem. However, after long-term service, it will fall off and cause environmental pollution, and it needs to be repainted and maintained, which has a high maintenance cost.

[0003] In the existing production method of marine atmospheric corrosion steel plates: Patent No. CN 115522137 "A marine atmospheric corrosion resistant steel and its manufacturing method", this method adds 0.8-9.0% Cr. However, Cr has the function of forming protective rust in an environment with relatively low salt content, which can hinder the inward development of corrosion; in an environment with high salt content, Cr reverses the corrosion resistance of steel and even accelerates corrosion. Mainly, the hydrolysis reaction process of Cr3+ will reduce the pH value of the metal surface, thereby accelerating corrosion. Secondly, this method is only suitable for coiling thin plates, not thick plates.

[0004] Patent publication number CN115323142 "A marine atmospheric corrosion resistant steel and its manufacturing method" requires mechanical grinding of the ingot surface before heating, and then spraying of high-temperature anti-oxidation coating. After rolling, the surface needs to be shot blasted and sprayed with an ion-mixed aqueous solution. The production process is cumbersome and the cost is high.

[0005] Publication No. CN202210570630.7 "A production method for Q420 grade high corrosion-resistant and high-strength offshore structural steel" has a thickness of only ≤60mm, which is difficult to meet the needs of large-span and heavy-loaded bridge manufacturing under marine environmental conditions.

[0006] In summary, the development of a thick Q420qFNHY bridge steel plate resistant to corrosion in marine atmospheric environment and its production method is of great significance for the construction and manufacturing of coastal cross-sea bridges in my country. Summary of the invention

[0007] In order to solve the above technical needs, the purpose of the present invention is to provide a Q420qFNHY steel plate resistant to corrosion in marine atmospheric environment. The steel plate has a reasonable combination of chemical components, excellent mechanical properties, resistance to marine atmospheric corrosion, and meets actual production, processing and use requirements.

[0008] Another object of the present invention is to provide a method for producing Q420qFNHY steel plate resistant to corrosion in marine atmospheric environment, which is convenient for organizing production in the field of wide and thick plate metallurgy technology and can make its comprehensive performance meet the use requirements.

[0009] To achieve the above object, the technical solution adopted by the present invention is: a Q420qFNHY steel plate for marine atmospheric corrosion resistance, the steel plate thickness is 60-150mm, including the following chemical components by mass percentage: 0.04-0.08% C, 0.10-0.20% Si, 0.70-1.50% Mn, ≤0.016% P, ≤0.002% S, 0.025-0.045% Als, 0.025-0.040% Nb, 0.010-0.65% V, 3.50-4.00wt% Ni, 0.10-0.15% Mo, 0.30-0.1.0% Cu, ≤0.012% Ti, ≤0.0005% B, the balance is Fe and residual elements;

[0010] The above-mentioned Q420qFNHY steel plate for marine atmospheric corrosion resistance meets the requirement that the annual average chloride ion deposition rate in marine atmosphere is ≤0.60mdd (refers to the deposition amount of chloride ions in the air in a certain time and a certain area, expressed in mg / dm 2 / day), and the annual average SO2 deposition rate ≤ 2mdd.

[0011] Q420qFNHY steel plate for marine atmospheric corrosion resistance

[0012] Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B≤0.22%;

[0013] Weathering resistant alloy index V value: V = 1 / {(1.0-0.16[C])*(1.05-0.05[Si])*(1.04-0.016[Mn])*(1.0-0.5[P])*(1.0+1.9[S])*(1.0-0.1[Cu])*(1.0-0.12[Ni])*(1.0-0.3[Mo])*(1.0-1.7[Ti])}≥1.6.

[0014] The above-mentioned thick Q420qFNHY steel plate resistant to corrosion in marine atmospheric environment has a total compression ratio of >5, a yield strength ≥420MPa, a tensile strength ≥540MPa, an elongation ≥25%, a longitudinal KV2 impact energy at -60℃ ≥200J, and a Z-direction section shrinkage rate ≥50%.

[0015] The composition design idea of ​​the present invention is: through low C design, the impact resistance and easy welding performance of the steel plate are guaranteed, and the excessive content of alloys such as Ni, Cu, and Mo is avoided, which makes welding difficult. Nb, V, and Ti are used to refine the grains, and the strength of the thick plate is improved by (Ti, Nb, V) C precipitates after tempering. Low Si is mainly to avoid the increase of Pcm and affect the welding performance. The content of harmful elements P and S in the steel is controlled as much as possible to avoid the formation of P and S inclusions.

[0016] Ni can effectively improve the impact toughness of thick plates, and can also effectively avoid the occurrence of Cu brittleness and reduce cracks in steel billets. Secondly, Ni helps to form a continuous and dense rust layer on the surface of steel, improve the physical and chemical properties of the matrix / rust layer section, inhibit the anodic dissolution of Fe, and significantly improve the corrosion resistance of steel. When the Ni content is less than 3.0%, the steel plate will quickly corrode and thin in an environment where the chloride ion deposition rate is ≤0.60mdd in coastal areas, and cannot meet the load-bearing requirements. When 3.0%≤Ni≤3.5%, the steel plate can be used in an environment where the chloride ion deposition rate is ≤0.60mdd, and a stable and dense rust layer is formed, thereby preventing corrosion from developing inward. When 3.5%≤Ni≤4.0%, the speed of forming a dense rust layer is faster and the stability of the rust layer is better. Secondly, when the Ni content is increased, it can effectively reduce the copper brittle effect of water-cooled die casting and prevent the occurrence of cracks on the surface of the steel ingot. However, when Ni is increased to >4.0%, the corrosion resistance is not significantly improved, and the cost is extremely high. Therefore, it is most appropriate to control it at 3.5% to 4.0%.

[0017] Mo can increase the hardenability of thick plates, improve the bainite ratio, and increase strength. In terms of corrosion resistance, first, Mo synergizes with Cr and other elements during the corrosion process to form a dense oxide film, which quickly repairs pitting defects; second, it helps to shift the self-corrosion potential of the steel matrix positively, reduce the corrosion current density, and make the rust layer denser; third, Mo alloying increases the affinity of steel for oxygen and inhibits the competitive adsorption of corrosive anions such as CL-.

[0018] The present invention needs to meet the requirement of weather resistance index V≥1.6 of weather resistance alloy content. V value is obtained from long-term exposure experiment of Japan on the Pacific coast, based on the composition of steel plate and corrosion thinning year by year. Generally, 0.9≤V≤2.5, the larger the V value, the less the corrosion loss in high-salinity environment. When V≥1.6, the increase of corrosion loss is basically not obvious, and it is in a stable state.

[0019] The production method of the Q420qFNHY steel plate for marine atmospheric corrosion resistance includes the following steps: molten iron pretreatment, converter smelting, argon station, LF refining, VD vacuum degassing, casting, ingot heating, billet rolling, secondary heating, two-stage rolling, controlled cooling, straightening, stack cooling, heat treatment, inspection, finishing, and warehousing, specifically:

[0020] Smelting process: Pre-treatment of molten iron by KR, after KR stirring and desulfurization, S content ≤0.008%. C content of converter steel ≤0.04%, P content ≤0.012%. Add 150Kg of deoxidizer aluminum block, and 300Kg of tapping lime. Use slag cone to block slag at the end of converter tapping to avoid P from returning to the slag. Strong argon gas is blown for 5 minutes at the argon station to make inclusions float fully. After the argon station is finished, enter VD to remove C, add 100-300Kg of iron oxide scale during the process, and ensure C content ≤0.02% during tapping. LF adjusts alloy composition, as well as deoxidation, slag making and S removal. LF is heated three times to fine-tune the composition, and the white slag is kept for 35-50min. After LF is finished, VD degassing is carried out. VD vacuum degree ≤67Pa, vacuum pressure holding time ≥18min, and fixed [H] content ≤1.5PPm.

[0021] During the casting process, the steel plate is produced by water-cooled mold casting with copper plate heat conduction to protect the casting throughout the whole process; the steel ingot is demoulded after water cooling for 12 to 14 hours, and is cleaned with warm water after high-temperature stack cooling for 24 hours, with the cleaning temperature at 150 to 300°C.

[0022] In the original ingot heating process, the heating time of the ingot is controlled at T = h (ingot thickness) × (16-18) min / cm, and positive pressure is used to burn the steel; the furnace temperature is controlled at ≤800°C before loading the steel, and the steel is preheated for 3-4 hours to reduce the temperature difference between the surface and the core of the ingot; the target insulation temperature in the high temperature section is 1250-1280°C, and the insulation time is 12 min / cm during heating.

[0023] In the billet rolling of the original steel ingot, the process of hot rolling to the bottom + controlled cooling is adopted; the rough rolling temperature is ≥1150℃, the reduction of the large reduction pass is carried out according to 50-55mm, and the surface is cooled by high-pressure water in each pass. No warming is carried out during rolling, and the intermediate billet with a thickness of 300 / 350mm is directly rolled; then the intermediate billet is controlled and cooled by super-intensity impact jet cooling SUPIC (Super Intensive Impinging Cooling), the roller speed is 1.0m / S, and the cooling is repeated 3-5 times, and the final cooling temperature is controlled at ≤850℃.

[0024] After the controlled cooling of the intermediate billet is completed, high-temperature pile cooling is carried out, and after slow cooling for 48 hours, it is loaded into the furnace for rolling.

[0025] In the secondary heating process of the intermediate billet, a heating furnace is used for heating, the first heating temperature is controlled at 800-850°C, the second heating temperature is 1230-1250°C, and the soaking section is 1220-1240°C; the heating time T = h (intermediate billet thickness) × 12min / cm;

[0026] In the two-stage rolling of the intermediate billet, the controlled rolling + controlled cooling process is adopted, and the rough rolling is 1030~

[0027] 1050℃, the maximum reduction pass is 45mm, and the steel is rolled in air-drying; from the initial 300-350mm rolling to the temperature waiting thickness, and then the temperature range required by the SUPIC controlled cooling process is used; then the finishing rolling is carried out until the finished steel plate thickness is 60-150mm; the final rolling, water entry, and controlled cooling process temperatures are as follows:

[0028]

[0029] After straightening, the steel plate is immediately cooled at a cooling temperature of ≥330°C and heat treated after 48 hours of cooling.

[0030] Heat treatment process: For steel plates with thickness ≥60-100mm, direct tempering process is adopted, tempering temperature is 580-630℃, tempering time = h (steel plate thickness) * 4.3min / mm; for thickness >100-150mm, quenching + tempering heat treatment process is adopted; the quenching heating temperature is controlled at 890±5℃, heating time T = h (steel plate thickness) * 2.5min / mm; after the steel plate is taken out of the furnace, it is water-cooled to room temperature in the quenching machine; tempering temperature is 580-630℃, tempering time = h (steel plate thickness) * 4.5min / mm, after taking out of the furnace, the stack is slowly cooled and removed when the temperature drops to ≤100℃.

[0031] If the steel plate is uneven, it will be flattened, then flame cut and finished, and then tested for performance, surface, and internal flaws before being put into storage.

[0032] The beneficial effects of the present invention include: the chemical composition and matrix structure of the large-thickness Q420qFNHY steel plate for resistance to marine atmospheric corrosion provided by the present application are reasonably matched, and it can simultaneously have high strength, low Pcm, and excellent low-temperature impact toughness and resistance to marine atmospheric corrosion, and it meets the requirements of industrial production and is suitable for the construction and manufacturing of large-scale cross-sea bridges. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0034] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0035] Example 1

[0036] This embodiment 1 provides a Q420qFNHY steel plate with a thickness of 80 mm, including the following chemical components in mass percentage: C0.05, Si0.13, Mn0.96, P0.012, S0.002, Als0.030, Nb0.036, V0.018, Ni3.56, Mo0.13, Cu0.32, Ti0.010, B0.0004, and the balance is Fe and residual elements.

[0037] Pcm of the steel plate = C + Si / 30 + Mn / 20 + Cu / 20 + Ni / 60 + Cr / 20 + Mo / 15 + V / 10 + 5B = 0.19% ≤ 0.22%.

[0038] Weathering resistance alloy index V value of steel plate: V = 1 / {(1.0-0.16[C])*(1.05-0.05[Si])*(1.04-0.016[Mn])*(1.0-0.5[P])*(1.0+1.9[S])*(1.0-0.1[Cu])*(1.0-0.12[Ni])*(1.0-0.3[Mo])*(1.0-1.7[Ti])} = 1.81> 1.6.

[0039] The production method includes:

[0040] After KR stirring and desulfurization, the S content of iron is 0.007%. The C content of the converter steel is 0.04% and the P content is 0.011%. 150Kg of aluminum blocks and 300Kg of tapping lime are added. At the end of the converter tapping, the slag is blocked by a slag cone, and the argon station blows argon for 5 minutes to make the inclusions float fully. After the argon station is completed, it enters the VD to remove C, and 200Kg of iron oxide is added during the process. The C content of the steel is guaranteed to be 0.02%. The LF white slag is kept for 36 minutes. The VD vacuum degree is 67Pa, the vacuum pressure holding time is 20 minutes, and the [H] content is set to ≤0.90PPm.

[0041] The original thickness of the steel ingot is 800mm, and the total compression ratio is 800 / 80 = 10. After water cooling for 13 hours, the ingot is demoulded and then cleaned after high temperature cooling for 24 hours. The cleaning temperature is 260℃.

[0042] The heating time of the steel ingot is controlled at T = 80cm × 16min / cm = 1280min, and the steel is burned under positive pressure. The furnace temperature is controlled at 685℃ before loading the steel, and the steel is preheated for 3h. The target insulation temperature of the high temperature section is 1330℃, and the insulation time is 960min during heating.

[0043] The rolling of the original steel ingot, the rough rolling starts at 1160℃, the large reduction pass is carried out at 55mm, and each pass uses high-pressure water to cool the surface. No warming is carried out during rolling, and the intermediate billet with a thickness of 300mm is directly rolled. SUPIC controlled cooling is used, the roller speed is 1.0m / S, and the cooling is repeated 4 times, and the final cooling temperature is controlled at 835℃.

[0044] After the intermediate billet is slowly cooled for 48 hours, it is loaded into the furnace for rolling. In the heating furnace, the first heating temperature is controlled at 808℃, the second heating temperature is 1246℃, and the soaking temperature is 1238℃. The heating time T=30cm×12=360min. For the rolling of the intermediate billet, the rough rolling temperature is 1045℃, the large reduction pass reduction is 45mm, the waiting thickness is 140mm, and the SUPIC is used to cool to 870℃ for finishing rolling, the final rolling temperature is 830℃, the water temperature is 785℃, and the red return temperature is 526℃.

[0045] After straightening, the steel plate is cooled at 356°C for 48 hours and then tempered at 615°C. The tempering time = 80mm*4.3min / mm = 344min.

[0046] Example 2

[0047] This embodiment 2 provides a Q420qFNHY steel plate with a thickness of 120 mm, including the following chemical components in mass percentage: C0.06, Si0.16, Mn1.06, P0.010, S0.002, Als0.035, Nb0.036, V0.028, Ni3.76, Mo0.15, Cu0.33, Ti0.008, B0.0003, and the remainder is Fe and residual elements.

[0048] Pcm of the steel plate = 0.21% ≤ 0.22%. Weathering resistance alloy index V value of the steel plate: V = 1.90 ≥ 1.60.

[0049] The thickness of the Q420qFNHY original ingot of Example 2 is 850 mm, and the total compression ratio = 850 / 120 = 7.08.

[0050] The production method of the Q420qFNHY steel plate differs from that in Example 1 in that:

[0051] The C content of the steel tapped from the converter is 0.03% and the P content is 0.008%. 130Kg of iron oxide scale is added during the VD C removal process, and the C content of the tapped steel is guaranteed to be 0.018%. The LF white slag retention time is 38 minutes. The VD vacuum degree is 67Pa, the vacuum holding time is 23 minutes, and the fixed [H] content is ≤0.78PPm.

[0052] The steel ingot is demoulded after 14 hours of water cooling, and the cleaning temperature is 280°C. The heating time of the steel ingot is controlled at T = 85cm × 16min / cm = 1360min, the furnace temperature is controlled at 706°C before loading the steel, the steel is preheated for 3.5 hours, the target insulation temperature of the high temperature section is 1350°C, and the insulation time is 1020min during heating.

[0053] The rolling of the original steel ingot, the rough rolling starts at 1166℃, and the intermediate billet is rolled to a thickness of 350mm. Using SUPIC to control cooling, cooling 5 times, the final cooling temperature is controlled at 826℃. Heating in the heating furnace, the first heating temperature is controlled at 836℃, the second heating is 1238℃, and the soaking section is 1236℃. Heating time T=35cm×12=420min. The rolling of the intermediate billet, the rough rolling starts at 1038℃, the waiting thickness is 140mm, and the SUPIC is used to cool to 830℃ for finishing rolling, the final rolling is 800℃, the water is 780℃, and the red return is 616℃.

[0054] After the steel plate is straightened, it is pile-cooled at a temperature of 388°C for 48 hours before heat treatment. The quenching heating temperature is 895°C, and the heating time is T = 120mm*2.5min / mm = 300min. After the steel plate is taken out of the furnace, it is water-cooled to room temperature in the quenching machine. The tempering temperature is 590°C, and the tempering time is 120mm*4.5min / mm = 5405min.

[0055] Example 3

[0056] This embodiment 3 provides a Q420qFNHY steel plate with a thickness of 150 mm, including the following chemical components in mass percentage: C0.045, Si0.13, Mn1.39, P0.010, S0.001, Als0.036, Nb0.039, V0.036, Ni3.88, Mo0.15, Cu0.36, Ti0.010, B0.0003, and the remainder is Fe and residual elements.

[0057] Pcm of the steel plate = 0.218% ≤ 0.22%. Weathering resistance alloy index V value of the steel plate: V = 1.97 ≥ 1.60.

[0058] The thickness of the Q420qFNHY original ingot of Example 3 is 900 mm, and the total compression ratio is 900 / 150=6.

[0059] The production method of the Q420qFNHY steel plate is different from that in Examples 1 and 2 in that:

[0060] The C content of the steel tapped from the converter is 0.03% and the P content is 0.008%. 150Kg of iron oxide scale is added during the VD C removal process, and the C content of the tapped steel is guaranteed to be 0.013%. The LF white slag retention time is 36 minutes. The VD vacuum degree is 67Pa, the vacuum holding time is 25 minutes, and the fixed [H] content is ≤0.77PPm.

[0061] The ingot was demoulded after 16 hours of water cooling, and the cleaning temperature was 256°C. The heating time of the ingot was controlled at T = 90cm × 17min / cm = 1530min, the furnace temperature was controlled at 586°C before loading, the steel was preheated for 3.5 hours, the target insulation temperature of the high temperature section was 1276°C, and the insulation time was 1080min during heating.

[0062] The rolling of the original steel ingot, the rough rolling starts at 1183℃, and the intermediate billet is rolled to a thickness of 350mm. Using SUPIC to control cooling, cooling 5 times, and controlling the final cooling temperature at 843℃. Heating in the heating furnace, the first heating temperature is controlled at 833℃, the second heating is 1236℃, and the soaking section is 1230℃. Heating time T=35cm×12=420min. The rolling of the intermediate billet, the rough rolling starts at 1050℃, the waiting thickness is 180mm, and the SUPIC is used to cool to 826℃ for finishing rolling, the final rolling is 813℃, the water is 776℃, and the red return is 625℃.

[0063] After the steel plate is straightened, the cooling temperature is 278℃, and the cooling time is 48h before heat treatment. The quenching heating temperature is 895℃, and the heating time is T=150mm*2.5min / mm=375min. After the steel plate is taken out of the furnace, it is water-cooled to room temperature in the quenching machine. The tempering temperature is 575℃, and the tempering time is =150mm*4.5min / mm=675min.

[0064] Example Performance

[0065] The Q420qFNHY steel plates obtained in Examples 1, 2, and 3 were used as the test products. The chemical composition, mechanical properties test specimen sampling location, and sample preparation of the steel plates were tested in accordance with the standard "GB / T2975". The low-temperature impact toughness test was tested in accordance with the standard "GB / T229", the tensile properties test was tested in accordance with the standard "GB / T228", and the bending properties test was tested in accordance with the standard "GB / T232". The test results are shown in the following table.

[0066] The following table shows the test results

[0067]

[0068] It can be seen from the above table that the Q420qFNHY steel plate provided in the embodiment of the present application has excellent strength and toughness matching.

[0069] Based on the above test results, it can be seen that the Q420qFNHY steel plate provided in the embodiment of the present application has strength performance, impact toughness, welding crack sensitivity index, weathering alloy index V and other indicators that meet the manufacturing and use requirements of bridge construction.

[0070] In addition, the pass rate of surface inspection and internal flaw detection of steel plates reached 100.00%.

[0071] In summary, the chemical composition, production process, and internal organization of the steel for Q420qFNHY steel plate provided in this application are reasonable, and can have good mechanical properties and welding properties at the same time. Its production method meets the organizational production of the metallurgical industry, can achieve the quality of Q420qFNHY steel plate, and improve its performance.

[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A Q420qFNHY steel plate for marine atmospheric corrosion resistance, characterized in that: The steel plate has a thickness of 60 to 150 mm and includes the following chemical compositions in mass percentage: 0.04-0.08% C, 0.10-0.20% Si, 0.70-1.50% Mn, ≤0.016% P, ≤0.002% S, 0.025-0.045% Als, 0.025-0.040% Nb, 0.010-0.65% V, 3.50-4.00wt% Ni, 0.10-0.15% Mo, 0.30-0.1.0% Cu, ≤0.012% Ti, ≤0.0005% B, and the balance is Fe and residual elements; The above-mentioned thick Q420qFNHY steel plate for marine atmospheric corrosion resistance meets the conditions of annual average chloride ion deposition rate ≤ 0.60mdd and annual average SO2 deposition rate ≤ 2mdd in marine atmosphere; The above-mentioned Q420qFNHY steel plate resistant to marine atmospheric corrosion has a Pcm≤0.22% and a weather resistance alloy index V≥1.6; a total compression ratio>5, a yield strength≥420MPa, a tensile strength≥540MPa, an elongation≥25%, a longitudinal KV2 impact energy at -60°C≥200J, and a Z-direction section shrinkage rate≥50%.

2. The method for producing the Q420qFNHY steel plate for marine atmospheric corrosion resistance according to claim 1 comprises the following steps: Hot metal pretreatment, converter smelting, argon station, LF refining, VD vacuum degassing, casting, ingot heating, billet rolling, secondary heating, two-stage rolling, controlled cooling, straightening, stack cooling, heat treatment, inspection, finishing, warehousing, characterized by: In the casting process, the steel plate is produced by water-cooled mold casting with copper plate heat conduction, and the casting is protected throughout the whole process; the steel ingot is demoulded after water cooling for 12 to 14 hours, and then it is cleaned with warm water after high-temperature stack cooling for 24 hours, and the cleaning temperature is between 150 and 300 °C; In the billet rolling of the original steel ingot, the process of hot rolling to the bottom + controlled cooling is adopted; the rough rolling temperature is ≥1150℃, the large reduction pass reduction is carried out according to 50-55mm, and the surface is cooled by high-pressure water in each pass. No warming is carried out during rolling, and the intermediate billet with a thickness of 300 / 350mm is directly rolled; then the intermediate billet is controlled to cool by ultra-strong impact jet cooling SUPIC, the roller speed is 1.0m / S, and the cooling is repeated 3-5 times, and the final cooling temperature is controlled at ≤850℃; In the secondary heating process of the intermediate billet, a heating furnace is used for heating, the first heating temperature is controlled at 800-850°C, the second heating temperature is 1230-1250°C, and the soaking section is 1220-1240°C; the heating time T = h (intermediate billet thickness) × 12min / cm; In the two-stage rolling of the intermediate billet, the controlled rolling + controlled cooling process is adopted, the rough rolling temperature is 1030-1050℃, the large reduction pass reduction is 45mm, and the steel is rolled in the air; from the initial 300-350mm rolling to the waiting thickness, and then the temperature range required by the SUPIC controlled cooling process is used; then the finishing rolling is carried out until the finished steel plate thickness is 60-150mm; the final rolling, water entry, and controlled cooling process temperatures are as follows: After the steel plate is straightened, it is immediately cooled at a temperature of ≥330°C. After 48 hours of cooling, heat treatment is performed. In the heat treatment process, for steel plates with a thickness of ≥60-100mm, direct tempering process is adopted, the tempering temperature is 580-630℃, and the tempering time is h (steel plate thickness)*4.3min / mm; for steel plates with a thickness of >100-150mm, quenching + tempering heat treatment process is adopted; the quenching heating temperature is controlled at 890±5℃, and the heating time T is h (steel plate thickness)*2.5min / mm; after the steel plate is taken out of the furnace, it is water-cooled to room temperature in the quenching machine. The tempering temperature is 580-630℃, and the tempering time is h (steel plate thickness)*4.5min / mm.

Citation Information

Patent Citations

  • Easy-welding and corrosion-resisting high strength Q690E steel plate for 80-120 mm thick deep sea submarine and production method of Q690E steel plate

    CN109234632A

  • Production method of Q420-grade high-corrosion-resistance high-strength offshore structural steel

    CN114854952A

  • Low-yield-ratio bridge steel Q460qFNH and production method thereof

    CN116790991A

  • Low-yield-ratio coating-free 500MPa-grade marine atmosphere corrosion-resistant steel and manufacturing method thereof

    CN117265410A

  • Easily-welded coating-free 420MPa-grade marine atmosphere corrosion-resistant steel plate and manufacturing method thereof

    CN117265411A