Copper-steel bimetallic self-lubricating material and manufacturing method thereof

By using powder metallurgy and copper-phosphorus alloy powder, the problem of insufficient bonding strength in copper-steel bimetallic self-lubricating materials has been solved, enabling the preparation of efficient and low-cost copper-steel bimetallic self-lubricating materials and improving the wear resistance and service life of the materials.

CN118895464APending Publication Date: 2024-11-05NBTM NEW MATERIALS GRP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410973512.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing copper-steel bimetallic self-lubricating materials have shortcomings in terms of bonding strength and preparation efficiency. In particular, they are prone to problems such as cracks, porosity, and segregation during welding, and traditional methods are difficult to achieve high-strength bonding.

Method used

A steel backing substrate is prepared using powder metallurgy, and copper-phosphorus alloy powder is added to the copper alloy layer. Through molding, sintering, and re-pressing processes, combined with a non-oxidizing atmosphere or vacuum environment, the density and bonding strength of the copper alloy layer are improved.

Benefits of technology

This study achieves a high-strength bond between copper and steel bimetallic self-lubricating materials, reducing production costs and energy consumption, improving preparation efficiency, and enhancing the wear resistance and service life of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895464A_ABST
    Figure CN118895464A_ABST
Patent Text Reader

Abstract

The invention discloses a copper-steel bimetallic self-lubricating material and a preparation method thereof. The copper-steel bimetallic self-lubricating material comprises a steel backing substrate and a copper alloy layer arranged on the steel backing substrate, the steel backing base body comprises, by weight, 0%-1.2% of phosphorus, 0%-5% of copper, 0.1%-1.0% of carbon, 0%-5% of nickel, 0%-2% of molybdenum, 0%-3.5% of chromium and the balance iron and inevitable impurities. The copper alloy layer comprises, by weight, 0.05%-1.2% of phosphorus, 0%-1.2% of sulfur, 0%-1.8% of molybdenum, 0%-6.0% of carbon, 0%-7% of silicon, 0%-15% of tin, 0%-5.0% of nickel, 0%-10.0% of zinc and the balance copper and inevitable impurities. The preparation method comprises the following steps: carrying out mold pressing to obtain the steel backing substrate and sintering to obtain the copper alloy layer. Compared with the prior art, the strength of the copper-steel bimetallic self-lubricating material is improved, the energy consumption is reduced, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of self-lubricating materials, and in particular to a copper-steel bimetal self-lubricating material and a manufacturing method thereof. Background Art

[0002] Copper-steel bimetallic self-lubricating materials not only meet the matching requirements of friction pair materials but also improve the fatigue strength of materials. They are widely used in sliding bearings, bushings, sliders, rails and other components to reduce friction and wear and extend service life, especially in situations where conventional lubrication is difficult or long-term maintenance-free is required. They provide reliable low friction and wear resistance and maintain stable operation in extreme environments. Copper-steel bimetallic self-lubricating materials have unique advantages: they can improve the working efficiency and service life of equipment in a variety of harsh environments, reduce maintenance requirements, and reduce energy consumption and operating costs.

[0003] Since copper alloys are expensive and have low strength, in order to reduce costs, the industry does not directly use copper alloys as self-lubricating materials, but instead combines a copper alloy layer on the steel back. Steel and copper are directly combined together through methods such as melting welding, brazing, solid diffusion welding, and powder metallurgy.

[0004] When using fusion welding, copper often penetrates between steel grains, generating thermal stress and causing weld fractures. At the same time, alloy elements are easily burned and evaporated, and segregation of elements such as tin and lead is easily generated in the weld. Brazing is mostly used for more precise welding of steel, copper and copper alloys. Although brazing does not have the problems of cracks, pores, segregation, etc. that are easily generated during fusion welding, it is easy to reduce the corrosion resistance of the joint during brazing, the joint strength is low, and the scope of use is subject to certain restrictions. In addition, for copper-steel bimetallic self-lubricating materials, the welding area is too large, the deformation is uneven during the heating process, and it is difficult to ensure the integrity of the copper-steel bond.

[0005] Vacuum diffusion welding is the most widely used solid diffusion welding. Since there is no melting between the solid welding joints and there is no fusion zone, problems such as organizational changes, component segregation and grain growth caused by melting of the joints are avoided. However, vacuum diffusion welding first requires the copper alloy to be sintered. At present, common alloying elements are generally not directly used in copper-based alloy layers. It is necessary to add additional wear-reducing and wear-resistant units, such as molybdenum disulfide and graphite. These substances are difficult to add directly to the alloy during casting and melting, and often need to be added in powder form. After forming, it is pressurized and sintered and diffusion welded. If no pressure is applied or the pressure is low during the welding process, problems such as low joint strength and deformation of the welded specimen are prone to occur. This technology is not suitable for direct preparation of parts.

[0006] For example, the Chinese invention application with publication number CN1775426A proposed a copper-steel bimetallic bearing material manufacturing process. This application requires adding a transition layer on the steel substrate to ensure the complete bonding of the copper and the steel back substrate. This method requires repeated rolling and is not easy to directly manufacture parts, resulting in low manufacturing efficiency.

[0007] Therefore, it is necessary to optimize the preparation process of copper-steel bimetallic self-lubricating materials and their parts. Summary of the invention

[0008] The first technical problem to be solved by the present invention is to provide a copper-steel bimetallic self-lubricating material with a steel back substrate and a copper alloy layer having better strength in view of the above technical status.

[0009] The second technical problem to be solved by the present invention is to provide a method for manufacturing a copper-steel bimetallic self-lubricating material with higher copper-steel bonding strength in view of the above-mentioned technical status quo.

[0010] The technical solution adopted by the present invention to solve the above-mentioned first technical problem is: a copper-steel bimetallic self-lubricating material, characterized in that it includes a steel back substrate and a copper alloy layer arranged on the steel back substrate; the steel back substrate includes the following components by weight: 0-1.2% phosphorus, 0-5% copper, 0.1-1.0% carbon, 0-5% nickel, 0-2% molybdenum, 0-3.5% chromium, and the balance is iron and unavoidable impurities;

[0011] The copper alloy layer comprises the following components by weight: 0.05-1.2% phosphorus, 0-1.2% sulfur, 0-1.8% molybdenum, 0-6.0% carbon, 0-7w% silicon, 0-15% tin, 0-5.0% nickel, 0-10.0% zinc, and the balance is copper and unavoidable impurities.

[0012] The technical solution adopted by the present invention to solve the above second technical problem is: a method for preparing a copper-steel bimetallic self-lubricating material, characterized in that it comprises the following steps:

[0013] ① Making a steel back matrix: weighing raw materials of the steel back matrix according to the weight composition, placing the raw materials in a mold and molding to obtain a steel back matrix green body; sintering the steel back matrix green body to obtain a steel back matrix, wherein the sintering temperature is 1050-1200° C.;

[0014] ② Making a copper alloy layer: weighing the raw materials of the copper alloy layer according to the weight composition, laying the raw materials of the copper alloy layer on the steel back substrate and sintering them in a sintering furnace at a sintering temperature of 700 to 1000° C. to obtain a copper-steel bimetallic self-lubricating material.

[0015] The steel back is manufactured using powder metallurgy technology. Compared with traditional methods, powder metallurgy technology can achieve efficient production of steel back, improve production efficiency and reduce production costs.

[0016] The copper-phosphorus alloy powder in the copper alloy layer that contacts the steel back substrate is melted, which is conducive to the diffusion between copper and iron, and is conducive to improving the bonding strength between the steel back and the copper alloy layer. This is something that the existing technology cannot do. The existing preparation method of copper-steel bimetallic composite materials often cannot achieve high-strength bonding between the copper alloy layer and the steel back substrate.

[0017] In order to further densify the copper alloy layer, preferably, a post-processing is also included, and the post-processing is: re-pressing the copper-steel bimetallic self-lubricating material obtained in step ②. In addition, a step ③ can be added between step ② and the post-processing: flipping the product obtained in step ② and repeating step ②; this method can be used not only to prepare a copper-steel bimetallic composite material with a copper alloy layer on one side, but also to prepare a sandwich-type copper-steel bimetallic self-lubricating bearing, that is, the steel back is in the middle layer and the two ends are copper alloy layers, which has strong adaptability.

[0018] In order to reduce environmental pollution and meet environmental protection requirements, preferably, the sintering atmosphere in steps ① and ② is non-oxidizing gas or vacuum.

[0019] Preferably, the sintering atmosphere in steps ① and ② is one of nitrogen, nitrogen-hydrogen mixed gas, decomposed ammonia, hydrogen or vacuum.

[0020] Preferably, the molding pressure in step ① is 300-900 MPa.

[0021] Preferably, the raw materials of the steel back substrate in step ① are as follows by weight: 0.1-1.2% graphite, 0-5.0% electrolytic copper powder, 0.1-5% iron-phosphorus alloy powder, 0-5% nickel, 0.1-0.8% lubricant powder, and the balance is pure iron powder or iron alloy powder. The phosphorus content in the iron-phosphorus alloy powder is 13-25wt%, and the D 99 Less than 80μm.

[0022] Preferably, the lubricant is polyamide wax.

[0023] Preferably, the graphite has a D 90 <100 microns.

[0024] Preferably, the raw materials of the copper alloy layer in step ② include, by weight: 0.1-10% copper-phosphorus alloy powder, 0-3% molybdenum disulfide, 0-3.0% graphite, 0-10% silicon carbide, 0-15% tin, 0-5.0% nickel, 0-10.0% zinc, and the balance is copper and unavoidable impurities. The copper-phosphorus alloy powder is prepared by water atomization, gas atomization or water-vapor combined atomization. The P content of the copper-phosphorus alloy powder is 5-15wt%, and the balance is copper; the particle size D of the copper-phosphorus alloy powder is 1000 g / cm2. 99Less than 90μm. In order to improve the wear resistance of the copper alloy layer, silicon carbide in the raw material can be replaced by Al2O3, SiO2, WC, TiC, ZrO2, TiO2, CBN, Si3N4, TiB2, etc.

[0025] Compared with the prior art, the advantages of the present invention are: phosphorus is added as an alloy element in the steel back matrix, which improves the strength of the steel back and reduces the sintering temperature; copper-phosphorus alloy powder is added to the copper alloy layer, which reduces the sintering temperature of the copper alloy layer, improves the density and strength of the copper alloy layer, reduces energy consumption, and reduces costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a cross-sectional view of the bimetallic self-lubricating material of Example 1;

[0027] Figure 2 This is the metallographic diagram of the bimetallic self-lubricating material after sintering in Example 1;

[0028] Figure 3 This is the metallographic diagram of the bimetallic self-lubricating material after re-pressing in Example 1;

[0029] Figure 4 This is the metallographic image of the bimetallic self-lubricating material after sintering in Comparative Example 1;

[0030] Figure 5 This is the metallographic image of the bimetallic self-lubricating material after re-pressing in Comparative Example 1;

[0031] Figure 6 This is the metallographic image of the bimetallic self-lubricating material after sintering in Comparative Example 2;

[0032] Figure 7 This is the metallographic image of the bimetallic self-lubricating material of comparative example 2 after re-pressing. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below with reference to the accompanying drawings.

[0034] Example 1

[0035] ① Mixed steel back matrix raw materials: 0.9wt% graphite powder, 2.0wt% electrolytic copper powder, 3.0% Fe3P powder, 0.6wt% polyamide wax powder as lubricant, and the rest is pure iron powder. 90 Less than 10 microns, Fe3P powder D 90 Less than 42μm.

[0036] ② Mixed copper alloy layer raw materials; 2% copper-phosphorus alloy powder and 98wt% copper alloy powder, wherein the phosphorus content of the copper-phosphorus alloy powder is 10wt%, and the copper alloy powder includes: 10wt% Sn, 2wt% Ni, and the balance is Cu.

[0037] ③Preparation of steel back matrix: The steel back matrix raw material powder of step ① is placed in a mold designed according to the requirements of the parts and pressed at a pressure of 600 MPa to obtain a density of 7.02 g / cm 3 The green steel back matrix is ​​sintered in a mesh belt furnace at 1120° C. for 20 minutes in a nitrogen-hydrogen mixed gas atmosphere. The obtained steel back matrix comprises the following components: 0.45wt% phosphorus, 2wt% copper, 0.85wt% carbon, 1.06wt% other uncontrollable elements, and the balance is iron.

[0038] ④ Preparation of copper alloy layer: Using the steel back substrate as a sintering fixture, evenly spread the copper alloy layer raw material powder prepared in step ② on the steel back, and the thickness of the copper alloy layer raw material powder is 1.5 mm; sinter the steel back substrate with the copper alloy layer raw material powder at 900°C for 60 minutes in a sintering atmosphere of a nitrogen-hydrogen mixture containing 70 Vol% hydrogen to obtain a copper-steel bimetallic self-lubricating material.

[0039] ⑤ Sintering the copper alloy layer on the other side: Flip the material obtained in step ④ to the other side, and repeat steps ③ and ④ to obtain a copper-steel bimetallic self-lubricating material having two copper alloy layers.

[0040] ⑥ Re-pressing: placing the copper-steel bimetallic self-lubricating material obtained in step ⑤ in a finishing mold and applying pressure, the height of the copper-steel layer reaches the predetermined requirement, and the copper alloy layer is further densified.

[0041] ⑦ Mechanical processing: The copper-steel bimetal self-lubricating material after re-pressing is processed into the required size to obtain the copper-steel bimetal self-lubricating parts.

[0042] Cut and polish the parts in step ⑦, and the cross section is as follows Figure 1 As shown, it can be seen that the steel back substrate is in the middle, and the two copper alloy layers are located outside the steel back substrate, and the copper and iron are tightly combined. The hardness of the steel back substrate reaches HRB85, and the hardness of the copper alloy layer reaches 240HV0.3.

[0043] The product after sintering in step ④ is cut, and its metallographic structure is as follows Figure 2 It can be seen that the density of the copper alloy layer in Example 1 after sintering is significantly higher than that in Comparative Examples 1 and 2. Figure 3 This is a metallographic photograph of the copper-steel bimetallic self-lubricating material after the re-pressing in step ⑥. It can be seen that the copper and steel are more closely combined after the re-pressing.

[0044] Example 2

[0045] ① Mixed steel back matrix raw materials: 0.7wt% graphite powder, 1.5wt% electrolytic copper powder, 3.3wt% Fe3P powder, 0.6wt% polyamide wax powder as lubricant, and the rest is pure iron powder. 90Less than 10 microns. Fe3P powder D 90 Less than 42μm.

[0046] ② Mixed copper alloy layer raw materials: 6wt% copper-phosphorus alloy powder, 2.0wt% MoS2 and 92wt% copper alloy powder; wherein the phosphorus content of the copper-phosphorus alloy powder is 10wt%; the copper alloy powder includes: 10wt% Sn, 2wt% Ni, and the remainder is Cu.

[0047] ③Preparation of steel back matrix: The steel back matrix raw material powder of step ① is placed in a mold and pressed at a pressing pressure of 600 MPa to obtain a density of 7.025 g / cm 3 The green steel back matrix is ​​sintered in a mesh belt furnace at 1120° C. for 30 minutes in a nitrogen-hydrogen mixed gas atmosphere. The obtained steel back matrix comprises the following components: 0.5wt% phosphorus, 1.5wt% copper, 1.75wt% nickel, 0.50wt% molybdenum, 0.65wt% carbon, 0.9wt% other uncontrollable elements, and the balance is iron.

[0048] ④ Spreading copper alloy layer powder: Using the steel back substrate as a sintering fixture, evenly spread the copper alloy layer raw material prepared in step ② on the steel back, and the thickness of the copper alloy layer raw material is 1.5 mm; sinter the steel back substrate with the copper alloy layer raw material powder at 880°C for 50 minutes in a sintering atmosphere of a nitrogen-hydrogen mixture containing 70 Vol% hydrogen to obtain a copper-steel bimetallic self-lubricating material.

[0049] ⑤ Sintering the copper alloy layer on the other side: Flip the material obtained in step ④ to the other side, and repeat steps ③ and ④ to obtain a copper-steel bimetallic self-lubricating material having two copper alloy layers.

[0050] ⑥ Re-pressing: placing the copper-steel bimetallic self-lubricating material obtained in step ⑤ in a finishing mold and applying pressure, the height of the copper-steel layer reaches the predetermined requirement, and the copper alloy layer is further densified.

[0051] After testing, the hardness of the steel back substrate reached HRB88 after re-pressing, and the hardness of the copper alloy layer reached 235HV0.3.

[0052] Example 3

[0053] ① Mixed steel back matrix raw materials: 0.75wt% graphite powder, 2.2wt% copper-phosphorus alloy powder (with a phosphorus content of 10wt%), 0.6wt% polyamide wax powder as a lubricant, and the remainder is pure iron powder. 90 Less than 10 microns, copper-phosphorus alloy powder D 90 Less than 45μm.

[0054] ② Mixed copper alloy layer raw materials: 7wt% copper-phosphorus alloy powder, 2.0wt% graphite powder, 91wt% copper alloy powder; the phosphorus content of the copper-phosphorus alloy powder is 10wt%, and the copper alloy powder includes: 10wt% Sn, 2wt% Ni, and the balance is Cu.

[0055] ③Preparation of steel back matrix: The steel back matrix raw material powder of step ① is placed in a mold designed according to the requirements of the parts and pressed at a pressure of 600 MPa to obtain a density of 7.025 g / cm 3 The green steel back substrate is sintered in a mesh belt furnace at 1120° C. for 30 minutes in a nitrogen-hydrogen mixed gas atmosphere. The obtained steel back substrate comprises the following components: 0.2wt% phosphorus, 2.0wt% copper, 1.50wt% molybdenum, 0.70wt% carbon, 0.9wt% other uncontrollable elements, and the balance is iron.

[0056] ④ Preparation of copper alloy layer: Using the steel back substrate as a sintering fixture, evenly spread the copper alloy layer raw material powder prepared in step ② on the steel back, and the thickness of the copper alloy layer raw material is 1.5 mm. Sinter the steel back substrate with the copper alloy layer raw material powder at 860°C for 50 minutes in a nitrogen-hydrogen mixed gas containing 70 Vol% hydrogen to obtain a copper-steel bimetallic self-lubricating material.

[0057] ⑤ Sintering the copper alloy layer on the other side: Flip the material obtained in step ④ to the other side, and repeat steps ③ and ④ to obtain a copper-steel bimetallic self-lubricating material having two copper alloy layers.

[0058] ⑥ Re-pressing: placing the copper-steel bimetallic self-lubricating material obtained in step ⑤ in a finishing mold and applying pressure, the height of the copper-steel layer reaches the predetermined requirement, and the copper alloy layer is further densified.

[0059] After testing, the hardness of the steel back substrate reached HRB90 after re-pressing, and the hardness of the copper alloy layer reached HB132.

[0060] Example 4

[0061] ① Mixed steel back matrix raw materials: 0.75wt% graphite powder, 5.0wt% Fe3P powder (with a phosphorus content of 10wt%), 0.6wt% polyamide wax powder as lubricant, and the remainder is pure iron powder. 90 Less than 10 microns, Fe3P powder D 90 Less than 45μm.

[0062] ② Mixed copper alloy layer raw materials: 7wt% copper-phosphorus alloy powder, 2.0wt% graphite powder, 91wt% copper alloy powder, 1.0wt% SiC powder. Among them, the phosphorus content of the copper-phosphorus alloy powder is 10wt%; the copper alloy powder includes: 10wt% Sn, 2wt% Ni, 5wt% zinc, and the balance is Cu.

[0063] ③Preparation of steel back matrix: The powder of step ① is placed in a mold designed according to the requirements of the parts and pressed at a pressure of 600 MPa to obtain a density of 7.025 g / cm 3 The green steel back matrix was sintered in a mesh belt furnace at 1120° C. for 30 minutes in a nitrogen-hydrogen mixed gas atmosphere. The obtained steel back matrix includes the following components: 0.8wt% phosphorus, 2.0wt% copper, 0.50wt% molybdenum, 3.0wt% chromium, 0.70wt% carbon, 0.9wt% other uncontrollable elements, and the balance is iron.

[0064] ④ Preparation of copper alloy layer: Using the steel back substrate as a sintering fixture, evenly spread the copper alloy layer raw material powder prepared in step ② on the steel back, and the thickness of the copper alloy layer raw material is 1.5 mm. The steel back substrate with the copper alloy layer raw material powder is sintered at 890°C for 50 minutes in a sintering atmosphere of a nitrogen-hydrogen mixed gas containing 70 Vol% hydrogen to obtain a copper-steel bimetallic self-lubricating material.

[0065] ⑤ Sintering the copper alloy layer on the other side: Flip the material obtained in step ④ to the other side, and repeat steps ③ and ④ to obtain a copper-steel bimetallic self-lubricating material having two copper alloy layers.

[0066] ⑥ Re-pressing: The copper-steel bimetallic self-lubricating material obtained in step ⑤ is placed in a finishing mold and pressure is applied to further densify the copper alloy layer.

[0067] After testing, the hardness of the steel back substrate reached HRB95 after re-pressing, and the hardness of the copper alloy layer reached 247HV0.3.

[0068] Comparative Example 1

[0069] ① Mixed steel back matrix raw materials: 0.9wt% graphite powder, 2.0wt% electrolytic copper powder, 0.6wt% polyamide wax powder as lubricant, and the rest is pure iron powder. 90 Less than 10 microns.

[0070] ② Mixed copper alloy layer raw materials: 100wt% copper alloy powder (10wt% Sn, 2wt% Ni, and the balance is Cu).

[0071] ③Preparation of steel back matrix: The steel back matrix raw material powder of step ① is placed in a mold designed according to the requirements of the parts and pressed at a pressure of 600 MPa to obtain a density of 7.04 g / cm 3 The green steel back substrate is sintered in a mesh belt furnace at 1120° C. for 20 minutes in a nitrogen-hydrogen mixed gas atmosphere. The obtained steel back substrate includes the following components: 2wt% copper, 0.85wt% carbon, 1.06wt% other uncontrollable elements, and the balance is iron.

[0072] ④ Preparation of copper alloy layer: Using the steel back substrate as a sintering fixture, evenly spread the copper alloy layer raw material powder prepared in step ② on the steel back, with a thickness of 1.5 mm. Sinter the steel back substrate with the copper alloy layer raw material powder at 920°C for 60 minutes in a sintering atmosphere of a nitrogen-hydrogen mixed gas containing 70 Vol% hydrogen.

[0073] ⑤ Sintering the copper alloy layer on the other side: Turn the material obtained in step ④ over to the other side, and repeat steps ③ and ④ to obtain a copper-steel bimetallic self-lubricating material.

[0074] ⑥ Re-pressing: placing the copper-steel bimetallic self-lubricating material obtained in step ⑤ in a finishing mold and applying pressure, the height of the copper-steel layer reaches the predetermined requirement, and the copper alloy layer is further densified.

[0075] ⑦ Mechanical processing: The copper-steel bimetal self-lubricating material after re-pressing is processed into a specified size to obtain a copper-steel bimetal self-lubricating part.

[0076] The product after sintering in step ④ is cut, and its metallographic structure is as follows Figure 4 As shown. It can be seen that the pores after sintering are significantly larger than those in Example 1. Figure 2 More and larger. See the photo after re-pressing Figure 5 The copper and steel are tightly combined, the steel back matrix hardness reaches HRB75, and the copper alloy layer hardness reaches 205HV0.3.

[0077] Comparative Example 2

[0078] ① Mixed copper alloy layer raw material: 100wt% copper alloy powder (10wt% Sn, 2wt% Ni, and the balance is Cu).

[0079] ② Processing of steel back substrate: Use 45 steel machine to process into steel back substrate.

[0080] ③ Spreading copper alloy layer powder: Using the steel back substrate as a sintering fixture, spread the copper alloy layer raw material powder prepared in step ① evenly on the steel back. The thickness of the copper alloy layer raw material powder is 1.5 mm.

[0081] ④ Sintering copper alloy layer: The steel back with copper powder in step ⑤ is sintered at 900° C. for 60 minutes in a sintering atmosphere of a nitrogen-hydrogen mixed gas containing 70 Vol% hydrogen.

[0082] ⑤ Sintering the copper alloy layer on the other side: Turn the material obtained in step ④ over to the other side and repeat steps ③ and ④.

[0083] ⑥ Re-pressing: placing the steel back with the sintered copper alloy layer in step ⑤ in a finishing mold and applying pressure, so that the copper alloy layer is further densified to obtain a copper-steel bimetallic self-lubricating material.

[0084] ⑦ Mechanical processing: Process the copper-steel bimetallic self-lubricating material after re-pressing into the required size.

[0085] The product after sintering in step ④ is cut, and its metallographic structure is as follows Figure 6 As shown in Figure 2, it can be seen that the pores are significantly smaller after sintering. Figure 2 There are many and large pores between copper and steel.

[0086] Cut and polish the parts in step ⑦, and the cross section is as follows Figure 7 As shown, it can be seen that compared with Example 1, the copper and iron in Comparative Example 2 have a little gap and are not tightly combined. The hardness of the steel back substrate reaches HRB70, and the hardness of the copper alloy layer reaches 210HV0.3.

Claims

1. A copper-steel bimetallic self-lubricating material, Features: It comprises a steel back substrate and a copper alloy layer arranged on the steel back substrate; the steel back substrate comprises the following components by weight: 0-1.2% phosphorus, 0-5% copper, 0.1-1.0% carbon, 0-5% nickel, 0-2% molybdenum, 0-3.5% chromium, and the balance is iron and unavoidable impurities; The copper alloy layer comprises the following components by weight: 0.05-1.2% phosphorus, 0-1.2% sulfur, 0-1.8% molybdenum, 0-6.0% carbon, 0-7w% silicon, 0-15% tin, 0-5.0% nickel, 0-10.0% zinc, and the balance is copper and unavoidable impurities.

2. A method for preparing the copper-steel bimetallic self-lubricating material according to claim 1, Features: The following steps are involved: ① Making a steel back matrix: weighing raw materials of the steel back matrix according to the weight composition, placing the raw materials in a mold and molding to obtain a steel back matrix green body; sintering the steel back matrix green body to obtain a steel back matrix, wherein the sintering temperature is 1050-1200° C.; ② Making a copper alloy layer: weighing the raw materials of the copper alloy layer according to the weight composition, laying the raw materials of the copper alloy layer on the steel back substrate and sintering them in a sintering furnace at a sintering temperature of 700 to 1000° C. to obtain a copper-steel bimetallic self-lubricating material.

3. The preparation method according to claim 2, Features: The method further comprises post-processing, wherein the post-processing comprises re-pressing the copper-steel bimetallic self-lubricating material obtained in step ②.

4. The preparation method according to claim 2, Features: The sintering atmosphere in steps ① and ② is non-oxidizing gas or vacuum.

5. The preparation method according to claim 4, Features: The sintering atmosphere in steps ① and ② is nitrogen, nitrogen-hydrogen mixed gas, decomposed ammonia, hydrogen or vacuum.

6. The preparation method according to claim 2, Features: The molding pressure in step ① is 300-900 MPa.

7. The preparation method according to claim 2, Features: The raw materials of the steel back substrate in step ① are as follows by weight: 0.1-1.2% graphite, 0-5.0% electrolytic copper powder, 0.1-5% iron-phosphorus alloy powder, 0-5% nickel, 0.1-0.8% lubricant powder, and the remainder is pure iron powder or iron alloy powder.

8. The preparation method according to claim 7, Features: The lubricant is polyamide wax.

9. The preparation method according to claim 7, Features: The graphite D 90 <100 microns.

10. The preparation method according to claim 2, Features: The raw materials of the copper alloy layer in step ② include, by weight: 0.1-10% copper-phosphorus alloy powder, 0-3% molybdenum disulfide, 0-3.0% graphite, 0-10% silicon carbide, 0-15% tin, 0-5.0% nickel, 0-10.0% zinc, and the balance is copper and unavoidable impurities.

Citation Information

Patent Citations

  • Process for manufacturing phosphor bronze-steel bimetal bearing material with phosphor content more than 0.1%

    CN1775426A