Splicing steel plate for 700MPa ultra-wide light and thin land transportation container and manufacturing method

By adjusting chemical composition and production process, a 700MPa ultra-wide light and thin container steel plate was designed, which solved the problems of insufficient strength and high cost of traditional container steel plates, and achieved high performance and low cost ultra-wide steel plates, meeting high strength and lightweight Quantification and corrosion resistance requirements.

CN118895465APending Publication Date: 2024-11-05BENGANG STEEL PLATES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048204.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The strength of traditional container steel plates is low, resulting in an increase in container weight, which cannot meet the needs of high strength and lightweight. At the same time, the existing 700MPa-grade hot-rolled container steel is costly and has limited width, making it difficult to meet the ultra-wide width demand.

Method used

By adjusting chemical composition and production process, a spliced ​​steel plate for 700MPa ultra-wide thin land container is designed, and the reasonable regulation of low C, Si, Cu, Cr, Ti and other elements is adopted, expensive Ni elements are abandoned, and strong cold steelmaking is used and Multi-stage heating and rolling process forms high-performance and low-cost steel, with a width of up to 2000-2150mm.

Benefits of technology

It realizes a high-performance and low-cost 700MPa class ultra-wide steel plate, which reduces the weight of the container, improves corrosion resistance and welding performance, meets the needs of complex land transportation environments, reduces the number of welding times, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895465A_ABST
    Figure CN118895465A_ABST
Patent Text Reader

Abstract

The invention relates to a spliced steel plate for a 700MPa ultra-wide light and thin land transportation container and a manufacturing method. The spliced steel plate comprises the following chemical components in percentage by weight: 0.04%-0.06% of C, 0.5%-0.68% of Si, 0.68%-0.98% of Mn, less than or equal to 0.015% of S, less than or equal to 0.015% of P, 0.050%-0.080% of Al, 0.085%-0.105% of Ti, 0.51%-0.68% of Cr, 0.20%-0.30% of Cu, less than or equal to 0.005% of N, less than or equal to 0.005% of O and the balance of Fe and other inevitable impurities. The light, thin and high-strength land transportation container steel which can serve in high-temperature and dry deserts and other land transportation zones and can resist accidental rainwater environment erosion is designed and manufactured mainly according to the actual land transportation environment condition. According to the land transportation container splicing steel plate and the manufacturing method thereof, the addition of a traditional expensive Ni element resistant to atmospheric corrosion is abandoned, the competition of Si, Cu and Cr is regulated and controlled according to the use environment of a land transportation container so as to meet different land transportation environment requirements, and finally the land transportation container splicing steel plate with the tensile strength larger than or equal to 700 MPa, the ductility larger than or equal to 18%, the width capable of reaching 2000-2150 mm and good corrosion resistance is manufactured through a reasonable production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of hot-rolled high-strength containers, and in particular to a 700MPa ultra-wide, light and thin spliced ​​steel plate for land transport containers and a manufacturing method thereof. Background Art

[0002] With the continuous opening of railway trains in China, the demand for land transport containers is increasing day by day. At the same time, facing the prominent international environmental and energy issues, containers should be developed in the direction of high strength and light weight. The strength of traditional container steel plates is generally low. When designing containers, the thickness of container plates needs to be increased to ensure the loading capacity of containers, which increases the weight of the entire container. Improving the strength of steel plates can reduce the wall thickness of containers, increase the effective volume, and increase the transport load. Experiments have shown that steel strength ≥ 700MPa can reduce its own weight by 15%.

[0003] The use of 1500mm-2150mm ultra-wide coils as container splicing steel plates can significantly reduce the number of splicing welds and reduce welding problems. Reasonable processes are used to maintain the stability of the ultra-wide coils to ensure that the steel coils have stable performance whether they are processed into corrugated plates for side panels, front wall panels or roof panels.

[0004] The patent document with application number CN202010362920.3 discloses a wide 700MPa grade hot-rolled weathering steel for containers and its manufacturing method. The steel contains C 0.058%~0.078%, Si 0.65%~0.75%, Mn 0.65%~0.85%, P 0.035%~0.045%, S≤0.006%, Al≤0.040%, Cr 0.22%~0.31%, Cu 0.11%~0.19%, Ti 0.060%~0.075%, RE 0.021%~0.035%, N≤0.005%, and the balance is iron and unavoidable impurities. The outlet temperature of the billet soaking section is 1283~1300℃, the holding time is 27~41min, and the total furnace time is ≤178min. The rough rolling outlet temperature is ≥1100℃, the finishing rolling start temperature is 1087~1108℃, the finishing rolling temperature is 925~947℃, and the coiling is cooled to 655~675℃ at a cooling rate of 37~47℃ / s, the flattening force is 5500~6500KN, and the bending roll force is 30~40KN. The flatness of the finished steel plate after flattening is ≤3mm / m. However, the width of the finished steel plate can only be 1350~1500mm, and the RE precious alloy element is added, which increases the cost. Summary of the invention

[0005] The purpose of the present invention is to provide a 700MPa ultra-wide, light and thin land container splicing steel plate and a manufacturing method. The present invention is mainly based on the actual land transportation environment, and designs and manufactures light, thin and high-strength land container steel that can be used in land transportation areas such as high-temperature and dry deserts, and can also resist occasional rainwater erosion. The present invention abandons the addition of the more expensive Ni element in traditional atmospheric corrosion resistance, and adjusts the competition of Si, Cu, and Cr to meet different land transportation environment requirements according to the use environment of land transportation containers. Finally, through a reasonable production process, a land container splicing steel plate with a tensile strength of ≥700MPa, an elongation of ≥18%, and a width of 2000-2150mm with good corrosion resistance is manufactured.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] 700MPa ultra-wide and thin splicing steel plate for land transport containers, the chemical composition of the steel is as follows by weight: C0.04%~0.06%, Si 0.5%~0.68%, Mn 0.68%~0.98%, S≤0.015%, P≤0.015%, Al0.050%~0.080%, Ti 0.085%~0.105%, Cr 0.51%~0.68%, Cu 0.20%~0.30%, N≤0.005%, O≤0.005%, and the rest is Fe and other unavoidable impurities.

[0008] Yield strength R of steel eL ≥700MPa, tensile strength R m ≥750MPa, elongation after fracture A≥18%, based on Q355B, relative corrosion rate ≤48%.

[0009] The steel plate has a thickness of 1.5 to 14 mm and a width of 2000 to 2150 mm and is mainly used for splicing steel plates such as container side plates and end plates.

[0010] The low C design adopted in the present invention can significantly reduce the carbon equivalent, improve the plasticity and weldability of the steel coil; and at the same time avoid Cr and C from easily forming carbides, which leads to a significant reduction in the corrosion resistance of the finished steel coil.

[0011] On the one hand, the Si element further inhibits the precipitation of Cr carbides, and on the other hand, forms a dense Si-rich layer on the surface of the steel coil, which improves the corrosion resistance of the steel coil while coating the Cu-rich liquid, increasing the viscosity and toughness of the surface layer and avoiding cracks caused by high-temperature Cu embrittlement.

[0012] The Mn element improves the strength of the steel coil through solid solution strengthening; at the same time, it can work together with Cu to weaken the harmful effects of S.

[0013] The Al element increases the precipitation temperature of AlN and the amount of AlN precipitation. The strong cooling mode is adopted in the steelmaking continuous casting section to allow the steel billet to precipitate dispersed and fine AlN, which serves as a parent phase to provide nucleation points for the precipitation of Ti compounds, greatly increasing the strengthening effect of Ti. No other expensive alloys are required to achieve 700Mpa-level container products.

[0014] Ti element can make the internal structure of steel dense, refine the grain force, reduce aging sensitivity and cold brittleness, improve welding performance. At the same time, it can regulate the precipitation size of Ti compounds, promote grain refinement, improve the toughness of steel while increasing strength, and the appropriate amount of Ti can help improve the corrosion resistance in rainy environments during land transportation.

[0015] In view of the land transportation service environment, the expensive Ni element, which has little contribution to corrosion resistance in the land transportation environment, is abandoned, and the competitive relationship between Si, Cu and Cr elements is adjusted to improve the corrosion resistance of steel in high temperature, sun exposure, rain and humidity environments encountered during land transportation.

[0016] Due to the presence of Mn and Cu, the S content does not need special control, which reduces the cost of desulfurization of the production design steel coil. At the same time, the appropriate S will increase the corrosion resistance contribution of the Cu element in the occasional rain environment, and the surface warping and edge cracking defects of Cu-containing steel can be almost eliminated by regulating the hot rolling process.

[0017] Finally, low control of O and N ensures fewer inclusions, which reduces the risk of cracking during subsequent processing and improves the quality of the weld.

[0018] A method for manufacturing a 700MPa ultra-wide, lightweight, land-transport container spliced ​​steel plate includes steelmaking and steel rolling, and the specific method is as follows:

[0019] 1. Steelmaking

[0020] 1) During the pretreatment of raw molten iron, 260-330g of lime is added per ton of steel, the magnesium powder injection rate is 8-14kg / min, and the mass ratio of molten iron to scrap steel is 1.1-1.5;

[0021] 2) Converter blowing time 12 to 17 minutes, refining Ar blowing time 42 to 52 minutes;

[0022] 3) The superheat of the continuous casting billet is controlled within 20°C, and a strong cooling mist cooling mode is adopted to increase the precipitation of AlN.

[0023] 2. Steel Rolling

[0024] 1) The hot charging furnace is adopted to prevent the cracks caused by the alternating stress concentration caused by the alternating changes in the temperature drop and rise process of the billet. The heating furnace atmosphere is a weak oxidizing atmosphere, and multi-stage heating is adopted. After the billet enters the furnace, it is slowly heated to 1065-1075℃ for 80-100min, then heated to 1150-1180℃ and kept warm for 70-90min, and then heated to 1200-1230℃ within 0.5-1min and kept warm for 25-40min before being taken out of the furnace. This process ensures the homogenization of austenite and alloy of the billet, the solidification of the Si layer, and prevents the large-scale enrichment of Cu from causing cracking.

[0025] 2) During the rolling process, the final rolling temperature of rough rolling is ≥1080℃, the final rolling temperature of fine rolling is 860~900℃, and the coiling temperature is 560~580℃. The high-pressure water descaling system and ultra-fast cooling system of the 2300mm unit are used to ensure the surface quality of the steel coil and the stable performance of the ultra-wide size.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1) In terms of composition design, the present invention adopts the fine grain strengthening and precipitation strengthening effects of Ti in steel to replace the Nb microalloying or Nb-Ti microalloying strengthening methods commonly used in traditional high-level container steel. At the same time, the competitive relationship between Si, Cu, and Cr is regulated, and the relatively expensive Ni is abandoned, so that the corrosion resistance of the steel can be more suitable for the complex environment of land transportation. The production of high-performance and low-cost land transportation container splicing steel plates is realized, which greatly reduces the cost.

[0028] 2) The present invention adopts a reasonable steelmaking process to precipitate a large amount of small dispersed AlN, which provides nucleation points for the precipitation of Ti compounds, greatly improving the strengthening effect of Ti, making the strengthening effect of Ti almost the same as the Nb-Ti composite strengthening effect.

[0029] 2) The present invention adopts a reasonable hot rolling process to obtain finer Ti compounds, which not only improves its own strength, but also obtains finer austenite, increases the grain boundary to provide a location for Cu precipitation, reduces the enrichment of Cu per unit area, and prevents rolling cracking. At the same time, the presence of Ti and Cu will improve the corrosion resistance of land transport containers during occasional rainfall.

[0030] 3) The present invention adopts a reasonable heating design, so that the liquid Fe2SiO4 in the steel billet hardly penetrates into the Fe matrix during the heating process, which can form an FeO+Fe2SiO4 layer with adhesion, and cooperate with the Cr layer to hinder the invasion of O and improve the corrosion resistance of the material; it can also coat the Cu-rich liquid at high temperature, slow down the trend of Cu-rich grain boundaries, and avoid high-temperature cracks.

[0031] 4) The present invention utilizes the equipment advantages of the 2300mm unit, and puts in a heat preservation cover during the rolling process to reduce the temperature difference between the temperature drop at the edge and the temperature drop at the core, thereby reducing the performance difference between the edge and the core of the ultra-wide steel coil; high-pressure water descaling will remove the loose rust layer and compact the dense rust layer; in conjunction with the ultra-fast cooling equipment of the unit, while producing 700MPa grade ultra-wide land transport container steel with a maximum width of up to 2150mm, the stability of the through-rolling performance of the ultra-wide container steel coil is ensured.

[0032] 5) The ultra-wide and light container splicing coil of the present invention has various mechanical properties that meet the requirements, excellent corrosion resistance, and good cost control. eL ≥700MPa, tensile strength R m ≥750MPa, elongation after fracture A≥18%, based on Q355B, relative corrosion rate ≤48%.

[0033] 6) The manufacturing method of the present invention can be used to mass-produce ultra-wide steel for land transport containers with a width of 2000-2150 mm. The advantages are that the number of welding times can be reduced, the production cost can be reduced, the utilization rate of steel can be increased, the weight of the container can be reduced, and the purpose of lightweight can be achieved, which is competitive in the market. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a typical metallographic structure of the steel plate of Example 1 of the present invention. DETAILED DESCRIPTION

[0035] The specific implementation of the present invention will be further described below in conjunction with the accompanying drawings.

[0036] The process flow of the present invention is: molten iron pretreatment → converter smelting → refining outside the furnace → continuous casting → (2300 hot rolling) heating → rough rolling, finish rolling → controlled cooling → coiling → finished product inspection → delivery.

[0037] Example

[0038] The embodiment of the present invention adopts a 2300mm unit to produce a product specification of (2.75-3.45mm)*2150mm, and takes the spliced ​​coil for ultra-wide and thin containers as an example to further illustrate the present invention. The container steel of the embodiment of the present invention is made according to the alloy element ratio in Table 1 (the balance is Fe and unavoidable impurities), and the steelmaking and rolling method is as follows:

[0039] During the pretreatment of raw molten iron, 260-330g of lime is added per ton of steel, the magnesium powder injection rate is 8-14kg / min, and the mass ratio of molten iron to scrap steel is 1.1-1.5; the converter blowing time is 12-17min, and the refining Ar blowing time is 42-52min;

[0040] 3) The superheat of the continuous casting billet is controlled within 20°C, and a strong cooling mist cooling mode is adopted to increase the precipitation of AlN.

[0041] Then it is hot loaded into the furnace, and after 80 to 100 minutes, it is slowly heated to 1065 to 1075°C, and then heated to 1150 to 1180°C and kept warm for 70 to 90 minutes. Then, it is heated to 1200 to 1230°C within 0.5 to 1 minute and kept warm for 25 to 40 minutes before being taken out of the furnace.

[0042] Subsequently, rough rolling is carried out, with the inlet temperature of R1 being 1000+15°C, the outlet temperature of R1 being 1080-1100°C, and the outlet temperature of R2 being 1090-1110°C. Three passes of rolling are performed for each process, and the rough rolling reduction rate is 81%-83%.

[0043] Then, the finishing rolling F1 inlet temperature is 1000-1054°C, and the final rolling temperature is 880-900°C. The finishing rolling is performed to a thickness of 2.75-3.45 mm. After the finishing rolling is completed, the steel is cooled to 560-580°C in an ultra-fast cooling mode for coiling. The main steelmaking process parameters of the embodiment are shown in Table 2, and the rolling process parameters are shown in Table 3.

[0044] The mechanical properties of the steel strip produced according to the steps of this embodiment are shown in Table 4, the corrosion properties are shown in Table 5, and the metallographic structure is shown in Table 6. Figure 1 , which is F+P+B.

[0045] Table 1 Example composition %

[0046] Example C Si Mn P S Ti Al Cu Cr O N 1 0.052 0.55 0.88 0.012 0.010 0.094 0.063 0.26 0.58 0.0021 0.0018 2 0.055 0.58 0.72 0.013 0.012 0.102 0.072 0.29 0.65 0.019 0.0015 3 0.048 0.64 0.92 0.010 0.011 0.098 0.068 0.26 0.59 0.0025 0.0013 4 0.059 0.62 0.85 0.012 0.009 0.099 0.059 0.28 0.63 0.0018 0.0015 5 0.042 0.51 0.69 0.013 0.012 0.088 0.070 0.21 0.51 0.0032 0.0012 6 0.045 0.53 0.75 0.009 0.008 0.100 0.062 0.25 0.52 0.0028 0.0018 7 0.057 0.66 0.95 0.014 0.010 0.104 0.069 0.23 0.60 0.0024 0.0023 8 0.046 0.67 0.96 0.010 0.013 0.092 0.071 0.24 0.55 0.0015 0.0040 Comparison 1 0.17 0.18 0.45 0.009 0.006 0.062 0.030 - - - 0.0042 Comparison 2 0.09 0.33 0.33 0.081 0.009 0.038 0.025 0.27 0.34 - -

[0047] Table 2 Example steelmaking process parameters

[0048]

[0049]

[0050] Table 3 Example rolling process parameters

[0051]

[0052] Table 4 Mechanical properties of the examples

[0053]

[0054] Table 5 Corrosion performance of examples

[0055]

[0056]

[0057] Comparative Example 1 is a traditional common plate, and Comparative Example 2 is a traditional corrosion-resistant plate.

Claims

1. 700MPa ultra-wide and thin land transport container splicing steel plate, characterized by: The chemical composition of the steel by weight percentage is: C 0.04%~0.06%, Si 0.5%~0.68%, Mn 0.68%~0.98%, S≤0.015%, P≤0.015%, Ti 0.085%~0.105%, Cr 0.51%~0.68%, Cu 0.20%~0.30%, Al 0.050%~0.080%, N≤0.005%, O≤0.005%, and the rest is Fe and other inevitable impurities.

2. The 700MPa ultra-wide, lightweight and spliced ​​steel plate for land transport containers according to claim 1 is characterized in that: Yield strength R of steel eL ≥700MPa, tensile strength R m ≥750MPa, elongation after fracture A≥18%, based on Q355B, relative corrosion rate ≤48%.

3. The 700MPa ultra-wide, lightweight and spliced ​​steel plate for land transport containers according to claim 1 is characterized in that: The steel plate has a thickness of 1.5 to 14 mm and a width of 2000 to 2150 mm.

4. The method for manufacturing the 700MPa ultra-wide, lightweight and thin spliced ​​steel plate for land transport containers according to any one of claims 1 to 3, comprising steelmaking and steel rolling, characterized in that: The steel rolling comprises: 1) The hot charging furnace method is adopted. After the billet is put into the furnace, it is slowly heated to 1065-1075℃ for 80-100min, then heated to 1150-1180℃ and kept warm for 70-90min, then heated to 1200-1230℃ within 0.5-1min and kept warm for 25-40min before being taken out of the furnace; 2) During the rolling process, the final rolling temperature of rough rolling is ≥1080℃, the final rolling temperature of fine rolling is 860~900℃, the coiling temperature is 560~580℃, and the high-pressure water descaling system and cooling system of the 2300mm unit are used.

5. The method for manufacturing a 700MPa ultra-wide, lightweight and thin spliced ​​steel plate for land transport containers according to claim 4, characterized in that: The steelmaking comprises: 1) During the pretreatment of raw molten iron, 260-330g of lime is added per ton of steel, the magnesium powder injection rate is 8-14kg / min, and the mass ratio of molten iron to scrap steel is 1.1-1.5; 2) Converter blowing for 12 to 17 minutes, refining Ar blowing time for 42 to 52 minutes; 3) The superheat of the continuous casting billet is controlled within 20°C, and the strong cooling mist cooling mode is adopted to increase the precipitation of AlN.