High-strength easily-formed 7xxx aluminum alloy material for thin plate component and preparation method and application of high-strength easily-formed 7xxx aluminum alloy material

By treating the natural aging state of 7xxx aluminum alloy materials for short-term peak aging, the problem of low forming performance of 7xxx aluminum alloy sheets is solved, high strength and good forming properties are achieved, and high-strength complex thin walls are suitable for automobiles and 3C electronics fields. Preparation of aluminum alloy components.

CN118895474APending Publication Date: 2024-11-05CHONGQING NATIONAL INNOVATION INSTITUTE OF LIGHT ALLOYS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411366369.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing 7xxx series aluminum alloy plates in automobiles and 3C electronics are limited by their low room temperature forming performance, and the existing hot stamping forming process consumes high energy, long process flow and expensive, so they cannot effectively utilize the pre-strengthening effect of the plate. .

Method used

The natural aging 7xxx aluminum alloy material is used for short-term peak aging treatment, and differential temperature heating is achieved through box furnace or electromagnetic induction heating, reducing the strength before material forming to ensure the forming quality, and precipitating a reinforced phase during the paint baking process to improve the strength of the material .

Benefits of technology

It realizes high strength and good formability of the material, reduces production difficulty and energy consumption, and significantly improves the yield strength, tensile strength and elongation of the board. It is suitable for high-strength complex thin-wall aluminum in the automotive, aerospace and 3C electronics fields. Alloy component preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

According to the high-strength easily-formed 7xxx aluminum alloy material for the thin plate component and the preparation method and application of the high-strength easily-formed 7xxx aluminum alloy material, on the basis of the characteristics of a short-time peak age forming integrated technology, a natural aging state alloy plate has the cluster dissolving capacity under the short-time heating condition, solution treatment is completed in the preparation process of the plate, natural aging is conducted, and the high-strength easily-formed 7xxx aluminum alloy material is obtained. Clusters separated out in the natural aging process are fully dissolved through short-time peak aging, nucleation is carried out to a certain extent at the same time, then materials are formed, paint baking treatment is further carried out, the yield strength of the final plate is larger than 450 MPa, the tensile strength is larger than 500 MPa, the ductility is larger than 8%, and the performance of the final plate is higher than that of a paint baking plate obtained after conventional cold and hot stamping. The plate provided by the invention has formability and high strength, and is suitable for preparation of high-strength complex thin-wall aluminum alloy components required in the fields of automobiles, aerospace, 3C and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aluminum alloys, and in particular relates to a high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components, and a preparation method and application thereof. Background Art

[0002] Aluminum alloy materials have the characteristics of low density, high specific strength, good corrosion resistance, and good processability. They are widely used in aviation, aerospace, automobile, machinery manufacturing, shipbuilding, construction, 3C electronics and other fields. The application of aluminum alloy sheets in the fields of automobiles and 3C electronics has greatly promoted the development of the domestic aluminum processing industry. At present, the sheets that are widely used in the fields of automobiles and 3C are 5xxx and 6xxx series aluminum alloys. 5xxx aluminum alloy sheets cannot be heat-treated and strengthened, and are usually directly stamped. 6xxx aluminum alloys are aging-strengthened aluminum alloys, which require solution treatment + pre-aging treatment, and then baking paint strengthening treatment after stamping. However, the strength grades of 5xxx and 6xxx series aluminum alloys are generally low. In order to further pursue lightweight, it is necessary to consider the application of higher-strength 2xxx and 7xxx series aluminum alloy sheets.

[0003] However, the room temperature formability of 2xxx and 7xxx series aluminum alloy sheets is relatively low, which limits their application in automobile bodies or mobile phones. Seeking materials and preparation methods that have both strength and formability is the main idea to promote the application of high-strength sheets in the automotive, aerospace and 3C electronics fields.

[0004] In the prior art, the invention patent "Aluminum Alloy Sheet Stamping Forming Method" with the authorization announcement number CN104117562B proposes an aluminum alloy forming method, which first heats the sheet to 495-500°C, keeps it warm for 30-60 minutes, then quickly quenches it with water, and completes the stamping forming within the range of 250-290°C within 8 hours. This method can reduce the problems of scratches, deformation and cracking caused by high temperature during the stamping process, but the process requires the workpiece to be heated to a higher temperature and then water quenched before forming, which has high energy consumption, a long process flow, and cannot utilize the pre-strengthening effect of the sheet.

[0005] The invention patent "A medium-strength 7xxx series aluminum alloy sheet suitable for hot stamping forming-quenching integrated process" with the authorization announcement number CN110885942B proposes a hot stamping forming-quenching integrated process aluminum alloy processing process, which combines the forming process and the heat treatment process, and relies on the same set of molds to achieve "forming" and "controllability". This process improves the plasticity of the material during the forming process while ensuring the strength of the material. The aluminum alloy sheet after complete solid solution is quickly transferred to the water-cooled mold, and then the mold is quickly closed to form. After the forming is completed, the mold is kept closed to complete the in-mold quenching of the part, and finally aging treatment is performed to improve its strength. However, this process requires the aluminum alloy to be heated to 450-510℃ and kept warm for 5-20 minutes to complete the solid solution. The high heating temperature is prone to local excessive thinning and tearing, and has extremely high requirements for mold cooling, which is expensive. Summary of the invention

[0006] The purpose of the present invention is to provide a high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components, its preparation method and application. The 7xxx aluminum alloy material in the present invention has both formability and high strength, and the process operability is high, and it is easy to achieve large-scale production. It is suitable for the preparation of high-strength and complex thin-walled aluminum alloy components required in the fields of automobiles, aerospace, 3C, etc.

[0007] The present invention provides a high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components, which is obtained by subjecting a naturally aged aluminum alloy material to a short-time spike aging treatment;

[0008] The high-strength and easy-to-form 7xxx aluminum alloy material for the thin plate member includes the following components by mass fraction:

[0009] Zn 5.1~6.8%, Mg 2.1~3.1%, Cu 1.2~2.7%, Mn≤0.35%, Zr ≤0.10%, Ti≤0.10%, impurity element Si≤0.40%, Fe≤0.50%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al;

[0010] The short-time peak aging is carried out by box furnace heating or electromagnetic induction heating.

[0011] The box-type furnace heating treatment comprises: heating the naturally aged aluminum alloy material to 180-240° C. at a heating rate of 2-6° C. / s;

[0012] The electromagnetic induction heating treatment comprises: heating the naturally aged aluminum alloy material to 150-240° C. at a heating rate of 30-60° C. / s, and keeping the temperature for 30-120s.

[0013] Preferably, the high-strength and easy-to-form 7xxx aluminum alloy material for the thin plate member includes the following components in mass fraction:

[0014] Zn 5.5~6.8%, Mg 2.5~3.1%, Cu 1.4~2.7%, Mn≤0.35%, Zr≤0.10%, Ti≤0.10%, impurity element Si≤0.40%, Fe≤0.50%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al.

[0015] Preferably, the set temperature of the box furnace is 410-490° C., and the heating time is 60-240 s.

[0016] The present invention provides a method for preparing a high-strength and easily formable 7xxx aluminum alloy material for a thin plate member as claimed in claim 1, comprising the following steps:

[0017] A) melting and casting the raw materials to obtain ingots;

[0018] B) subjecting the ingot to homogenization treatment, hot rolling, cold rolling, solution treatment and natural aging treatment in sequence to obtain a naturally aged aluminum alloy material;

[0019] C) The naturally aged aluminum alloy material is subjected to short-time spike aging treatment to obtain high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components.

[0020] Preferably, the casting is prepared by a spray deposition method;

[0021] The homogenization process comprises the following steps:

[0022] The ingot is kept at 400°C-450°C for 4-10 hours, and then kept at 460°C-490°C for 10-40 hours, and then air-cooled or wind-cooled to room temperature. The heating rate in the homogenization treatment is 25-75°C / h.

[0023] Preferably, the hot rolling comprises the following steps:

[0024] The homogenized billet is kept at 380-450°C for 3-20h, and then subjected to hot rough rolling and hot finish rolling to 4-8mm, with a final rolling temperature of 250-350°C, cooled to room temperature, and then the 4-8mm thick alloy hot-rolled coil is cold-rolled and curled to obtain a 0.2-3mm cold-rolled coil.

[0025] Preferably, the temperature of the solution treatment is 450-510°C, and the time of the solution treatment is 5-20 minutes;

[0026] The natural aging treatment comprises the following steps:

[0027] The material after the solution treatment is naturally placed at room temperature to obtain a naturally aged aluminum alloy material.

[0028] The present invention provides a thin plate component, which is obtained by cold stamping and baking varnish treatment of 7xxx aluminum alloy material;

[0029] The 7xxx aluminum alloy material is the high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components described above;

[0030] The thickness of the thin plate member is 0.2-3 mm.

[0031] Preferably, the temperature of the paint baking treatment is 160-190° C., and the time of the paint baking treatment is 20-60 min.

[0032] The present invention provides a component, comprising the thin plate member described above.

[0033] The present invention provides a high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components, which is obtained by subjecting a naturally aged aluminum alloy material to a short-time spike aging treatment; the high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components comprises the following components by mass fraction: Zn 5.1-6.8%, Mg 2.1-3.1%, Cu 1.2~2.7%, Mn≤0.35%, Zr≤0.10%, Ti≤0.10%, impurity element Si≤0.40%, Fe≤0.50%, other impurities individually ≤0.05%, other impurities in total ≤0.15%, and the balance is Al; the short-time spike aging adopts box furnace heating treatment or electromagnetic induction heating treatment, and the box furnace heating treatment includes: heating the naturally aged aluminum alloy material to 180~240℃ at a heating rate of 2~6℃ / s; the electromagnetic induction heating treatment includes: heating the naturally aged aluminum alloy material to 150~240℃ at a heating rate of 30~60℃ / s, and keeping it warm for 30s~120s.

[0034] The specific beneficial effects of the technical solution in the present invention are as follows:

[0035] 1. The naturally aged aluminum alloy material (at any time) described in the present invention is suitable for the integrated process of short-time peak aging forming. Not only can the process be used to effectively reduce the material strength before forming to ensure the forming quality, but on the other hand, compared with the rapid heating process equivalent to isothermal heating, the box furnace differential temperature heating method equivalent to non-isothermal aging is used. The material sequentially experiences different temperature ranges from low to high. Under the premise of almost no increase in the yield strength of the material before stamping, a part of the particles can be effectively nucleated during the heating process and precipitated during the subsequent baking process, and finally the baking strength is further improved through the strengthening precipitated phase with higher number density.

[0036] The material strength can reach yield strength>450MPa, tensile strength>500MPa, and elongation>8%, which is significantly better than the 7xxx aluminum alloy material that can be obtained by conventional cold and hot stamping processes;

[0037] 2. The short-time peak aging forming integrated process described in the present invention can be completely implemented based on conventional cold stamping equipment and dies to produce related parts and products, and the equipment procurement cost is significantly lower than that of hot stamping related equipment and dies;

[0038] 3. Compared with hot stamping which requires heating at a temperature above 450°C, the short-time peak aging forming integrated process of the present invention only requires heating the sheet to 180-240°C (actual material temperature) in a box furnace, which significantly reduces production difficulty and energy consumption costs;

[0039] 4. The short-time peak aging forming integrated process described in the present invention can also be carried out by differential heating in a conventional box-type heating furnace, which makes the process more feasible. In addition, linear heating helps to reduce the temperature difference between the surface and the core of the aluminum alloy, and shortens the time the aluminum alloy stays at high temperature, which can effectively avoid the pre-stamping strength from increasing again due to excessive regression;

[0040] 5. The present invention conducts a detailed study on the stability of natural aging clusters of 7xxx series aluminum alloys with different compositions and different initial natural aging states at various temperatures as well as the relationship between remelting and re-precipitation, proposes a short-time peak aging process window for aluminum alloys according to different natural aging cluster precipitation conditions, and clarifies the differences in the preparation process of high-strength aluminum alloy plates with different natural aging states. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0042] Figure 1 This is a photo of a car B-pillar sample of the naturally aged 7xxx series aluminum alloy sheet of Example 1 of the present invention after short-time spike aging forming;

[0043] Figure 2 This is a photograph of the automobile B-pillar sample after the naturally aged 7xxx series aluminum alloy sheet of comparative example 2 of the present invention was formed by short-time spike aging. DETAILED DESCRIPTION

[0044] The present invention provides a high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components, which is obtained by subjecting a naturally aged aluminum alloy material to a short-time spike aging treatment;

[0045] The high-strength and easy-to-form 7xxx aluminum alloy material for the thin plate member includes the following components by mass fraction:

[0046] Zn 5.1~6.8%, Mg 2.1~3.1%, Cu 1.2~2.7%, Mn≤0.35%, Zr ≤0.10%, Ti≤0.10%, impurity element Si≤0.40%, Fe≤0.50%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al;

[0047] The short-time peak aging is carried out by box furnace heating or electromagnetic induction heating.

[0048] The box-type furnace heating treatment comprises: heating the naturally aged aluminum alloy material to 180-240° C. at a heating rate of 2-6° C. / s;

[0049] The electromagnetic induction heating treatment comprises: heating the naturally aged aluminum alloy material to 150-240° C. at a heating rate of 30-60° C. / s, and keeping the temperature for 30s-120s.

[0050] In the present invention, the thin plate member having the following components is matched with the high-strength and easy-to-form naturally aged 7xxx aluminum alloy material and is suitable for the short-time spike aging forming integrated process in the present invention:

[0051] Zn 5.1~6.8%, Mg 2.1~3.1%, Cu 1.2~2.7%, Mn≤0.35%, Zr ≤0.10%, Ti≤0.10%, impurity element Si≤0.40%, Fe≤0.50%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al;

[0052] In the present invention, Zn can be specifically 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, preferably a range value with any of the above values ​​as the upper or lower limit;

[0053] Mg may specifically be 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, preferably a range value with any of the above values ​​as the upper or lower limit;

[0054] Cu can specifically be 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, preferably a range value with any of the above values ​​as the upper or lower limit;

[0055] Preferably, Zn 5.5-6.8%, Mg 2.5-3.1%, Cu 1.4-2.7%, Mn ≤0.35%, Zr ≤0.10%, Ti ≤0.10%, impurity element Si ≤0.40%, Fe ≤0.50%, other impurities individually ≤0.05%, total ≤0.15%, balance Al

[0056] More preferably, Zn 6.1~6.7%, Mg 2.9~3.1%, Cu 2.0~2.6%, Mn ≤0.35%, Zr ≤0.08%, Ti≤0.05%, impurity element Si≤0.30%, Fe≤0.40%, other impurities individually ≤0.05%, total ≤0.15%, and the balance is Al.

[0057] In the present invention, the short-time peak aging adopts box furnace heating treatment or electromagnetic induction heating treatment. In the present invention, the box furnace heating treatment is differential temperature heating, and the heating rate of the box furnace heating is preferably 2~6℃ / s, more preferably 3~4℃ / s, such as 2℃ / s, 3℃ / s, 4℃ / s, 5℃ / s, 6℃ / s, preferably a range value with any of the above values ​​as the upper or lower limit; the box furnace heating treatment is heated to 180~240℃, preferably 200~220℃, such as 180℃, 185℃, 190℃, 195℃, 200℃, 205℃, 210℃, 215℃, 220℃, 225℃, 230℃, 235℃, 240℃, preferably a range value with any of the above values ​​as the upper or lower limit, the temperature refers to aluminum The temperature actually reached by the alloy material, the heating of the aluminum alloy material is stopped after reaching this temperature, and the set temperature of the box furnace is set to 410-490°C, more preferably 430-470°C, such as 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, preferably a range value with any of the above values ​​as the upper or lower limit; the box furnace is set at this temperature, and the naturally aged aluminum alloy material in the furnace is slowly heated from room temperature to the heating temperature at a rate of 2-6°C / s, and the material sequentially experiences different temperature intervals from low to high, which can make a part of the particles effectively nucleate during the heating process and precipitate during the paint baking process without almost increasing the strength, and finally improve the paint baking strength through the strengthening precipitation phase with higher number density. The heating time is preferably 60 to 240 s, more preferably 60 to 100 s, such as 60 s, 70 s, 80 s, 90 s, 100 s, 110 s, 120 s, 130 s, 140 s, 150 s, 160 s, 170 s, 180 s, 190 s, 200 s, 210 s, 220 s, 230 s, 240 s, preferably a range value with any of the above values ​​as the upper or lower limit.

[0058] In the present invention, the electromagnetic induction heating is an isothermal heating device, and the heating rate of the electromagnetic induction heating is preferably 30-60°C / s, more preferably 40-50°C / s, such as 30°C / s, 35°C / s, 40°C / s, 45°C / s, 50°C / s, 55°C / s, 60°C / s, preferably the upper or lower limit of any of the above numerical values; the holding temperature of the electromagnetic induction heating is preferably 150-240°C, more preferably 1 The temperature of the mixture is preferably 80-220°C, such as 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, preferably a range value with the above arbitrary numerical value as the upper or lower limit; the insulation time is preferably 30-120s, more preferably 30-60s, more preferably 40-50s, such as 30s, 35s, 40s, 45s, 50s, 55s, 60s, 70s, 80s, 90s, 100s, 110s, 120s, preferably a range value with the above arbitrary numerical value as the upper or lower limit.

[0059] The naturally aged plate in the present invention is softened and nucleated synchronously by short-time spike aging, and the material is subjected to baking varnish treatment after being formed. The yield strength of the final plate is greater than 450MPa, the tensile strength is greater than 500MPa, and the elongation is greater than 8%.

[0060] The present invention also provides a method for preparing the high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components as described above, comprising the following steps:

[0061] The naturally aged aluminum alloy material is subjected to a short-time peak aging treatment, then stamped into shape, and then subjected to a baking varnish treatment to obtain a high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components.

[0062] In the present invention, the thickness of the naturally aged aluminum alloy material is preferably a naturally aged plate with a thickness of 0.2 to 3.0 mm, and is preferably prepared according to the following steps:

[0063] A) melting and casting the raw materials to obtain ingots;

[0064] B) subjecting the ingot to homogenization treatment, hot rolling, cold rolling, solution treatment and natural aging treatment in sequence to obtain a naturally aged aluminum alloy material.

[0065] In the present invention, the raw materials can be selected from corresponding pure metal or alloy raw materials according to the composition and content of the high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components described above, and the present invention will not be repeated here.

[0066] In the present invention, the smelting temperature is preferably 700-745°C, more preferably 710-735°C, such as 700°C, 705°C, 710°C, 715°C, 720°C, 725°C, 730°C, 735°C, 740°C, 745°C, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit; the ingot is preferably manufactured by industrial semi-continuous ingot casting, preferably prepared by spray deposition; the casting temperature is preferably 690-710°C, more preferably 700-705°C, such as 690°C, 695°C, 700°C, 705°C, 710°C, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit.

[0067] In the present invention, the homogenization treatment preferably includes the following two stages:

[0068] The ingot is kept at 400℃~450℃ for 4~10h, then kept at 460℃~490℃ for 10~40h, and then air-cooled or wind-cooled to room temperature.

[0069] In the present invention, the insulation temperature of the first stage is preferably 400-450°C, more preferably 420-430°C, such as 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit; the insulation time of the first stage is preferably 4-10 hours, more preferably 6-8 hours; the insulation temperature of the second stage is preferably 460-490°C, more preferably 480-485°C, such as 460°C, 465°C, 470°C, 475°C, 480°C, 485°C, 490°C, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit; the insulation time of the second stage is preferably 10-40 hours, more preferably 20-30 hours.

[0070] In the present invention, the heating rate in the homogenization process is preferably 25-75°C / h, more preferably 30-70°C / h, such as 25°C / h, 30°C / h, 35°C / h, 40°C / h, 45°C / h, 50°C / h, 55°C / h, 60°C / h, 65°C / h, 70°C / h, preferably a range value with any of the above values ​​as the upper or lower limit.

[0071] After the homogenization treatment is completed, the present invention performs hot rolling, cold rolling and curling on the homogenized blank to obtain a coil.

[0072] In the present invention, the homogenized billet is preferably first subjected to heat preservation treatment, and then subjected to hot rough rolling and hot finish rolling in sequence to 4-8 mm, and then air-cooled to room temperature after coiling to obtain a hot-rolled coil, and then the hot-rolled coil is cold-rolled and coiled to obtain a plate (strip, foil) material with a thickness of 0.2-3 mm.

[0073] In the present invention, the temperature of the heat preservation treatment after homogenization is preferably 380-450°C, more preferably 400-420°C, such as 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, preferably a range value with any of the above values ​​as the upper or lower limit; the time of the heat preservation treatment is preferably 3-20 hours, more preferably 5-15 hours.

[0074] In the present invention, the finishing temperature is preferably 250-350°C, more preferably 280-320°C, such as 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, preferably a range value with any of the above values ​​as the upper or lower limit.

[0075] After obtaining the plate (strip, foil) material, the present invention performs rapid solution treatment on the strip, and the temperature of the solution treatment is preferably 450-510°C, more preferably 460-500°C, such as 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, preferably a range value with any of the above values ​​as the upper or lower limit; the time of the solution treatment is preferably 5-20min, more preferably 10-15min.

[0076] After the solution treatment is completed, water cooling is carried out, and then the coil is subjected to natural aging treatment, that is, it is naturally parked for any period of time at room temperature (between 0 and 40°C) to obtain a naturally aged aluminum alloy material.

[0077] The present invention preferably subjects the naturally aged aluminum alloy material to a short-time spike aging treatment, followed by stamping and forming, and then subjecting it to a baking varnish treatment to obtain a high-strength and easily formable 7xxx aluminum alloy material for thin plate components.

[0078] In the present invention, the short-time spike aging treatment is consistent with the short-time spike aging treatment described above, and the present invention will not be repeated here.

[0079] The present invention also provides a thin plate component, which is obtained by cold stamping and painting a 7xxx aluminum alloy material; the 7xxx aluminum alloy material is the high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components described above.

[0080] In the present invention, the cold stamping is a commonly used forming method in the art, which can be implemented using conventional cold stamping equipment and molds, and the present invention will not be repeated here. In the present invention, the cold stamping refers to stamping at a conventional room temperature, such as 0-40°C.

[0081] In the present invention, the temperature of the baking varnish treatment is preferably 160-190° C., more preferably 170-180° C., and the time of the baking varnish treatment is preferably 20-60 min, more preferably 20-50 min.

[0082] The present invention further provides a component, comprising the thin-walled component described above. In the present invention, the component can be applied to the fields of automobile, aerospace, 3C, etc.

[0083] The present invention is based on the characteristics of the short-time spike aging forming integrated process. The naturally aged alloy sheet has the ability to dissolve clusters under short-time heating conditions. The sheet completes solid solution treatment and natural aging during the preparation process. The clusters precipitated during the natural aging process are fully dissolved by short-time spike aging and nucleated to a certain extent. The material is then formed and further subjected to baking varnish treatment. The final sheet has a yield strength of >450MPa, a tensile strength of >500MPa, and an elongation of >8%, which are higher than the corresponding performance of conventional cold and hot stamping and baking varnish sheets. The sheet provided by the present invention has both formability and high strength, and is suitable for the preparation of high-strength complex thin-walled aluminum alloy components required in the fields of automobiles, aerospace, 3C, etc.

[0084] In order to further illustrate the present invention, a high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components provided by the present invention, its preparation method and application are described in detail below in combination with embodiments, but it should not be understood as limiting the scope of protection of the present invention.

[0085] Example 1

[0086] The alloy ingots were prepared according to the composition ratio in Table 1, and the ingots were prepared by industrial semi-continuous casting;

[0087] After the alloy ingot is prepared, a two-stage homogenization treatment is carried out: the homogenization process is to keep the alloy ingot at 425±25℃ for 7±1h, then keep it at 480±10℃ for 25±5h, and then heat it up at a rate of 50±10℃ / h, and then air cool it or wind cool it to room temperature. After the homogenized billet is kept at 415±35℃ for 12±2h, it is hot rough rolled and hot finish rolled to 6±2mm, and the final rolling temperature is 300±50℃, then coiled, and the alloy hot rolled coil is air cooled to room temperature. The 4-8mm thick alloy hot rolled coil is cold rolled and coiled to obtain a 2mm thick alloy cold rolled sheet. The 2mm thick cold rolled coil is solution treated, and the solution treatment temperature is 480±30℃. After rapid solution treatment for 15±5min (the process production uses online continuous solution treatment), it is water cooled to obtain a 2mm thick cold rolled coil after solution treatment. After solution treatment, the steel was left to stand for 2 weeks at room temperature (20±5°C) to obtain a naturally aged cold rolled coil with a thickness of 2 mm. The alloy composition and thickness are shown in Table 1.

[0088] The short-time spike aging forming process is: using a box furnace for differential heating, the box furnace temperature is set to 460℃, the heating rate is 3℃ / s, and the actual temperature of the sample is 200℃. After heating for 60s, the sample temperature reaches 200℃ and then it is taken out of the furnace and transferred to the cold stamping die for stamping. The sample has a good forming effect and does not crack. Finally, it is strengthened by a 185℃, 30min baking paint process, and the performance is shown in Table 2.

[0089] Example 2

[0090] The aluminum alloy plate was prepared according to the steps in Example 1. The difference from Example 1 is that the heating method is different. The sample is heated by electromagnetic induction at a heating rate of 40°C / s to quickly heat to 200°C and then keep warm for about 60s.

[0091] Example 3

[0092] The difference from Example 1 is that: the alloy composition is slightly different, see Table 1 for details; the heating process before forming is different, the sample is heated by electromagnetic induction heating at a heating rate of 40°C / s to quickly heat to 180°C and then keep warm for about 120s.

[0093] Example 4

[0094] The difference from Example 1 is that the alloy composition is different, see Table 1 for details.

[0095] Example 5

[0096] The difference from Example 1 is that: the alloy composition is slightly different, see Table 1 for details; the heating process before forming is different: a box furnace is used for differential heating, the box furnace temperature is set to 460°C, the heating rate is 3°C / s, and the actual temperature of the sample is 240°C. After heating for 75s, it is taken out of the furnace.

[0097] Example 6

[0098] The difference from Example 1 is that: the alloy composition is slightly different, see Table 1 for details; the heating process before forming is different: a box furnace is used for differential temperature heating, the box furnace temperature is set to 460°C, the heating rate is 3°C / s, and the actual temperature of the sample is 220°C. After heating for 65s, it is taken out of the furnace.

[0099] Example 7

[0100] The difference from Example 1 is that: the alloy composition is slightly different, the foil thickness is 0.3 mm, see Table 1 for details; the heating process before forming is different: a box furnace is used for differential heating, the box furnace temperature is set to 460°C, the heating rate is 3°C / s, and the actual temperature of the sample is 180°C. After heating for 60s, it is taken out of the furnace.

[0101] Embodiment 8-9

[0102] The difference from Example 1 is that: the alloy composition is different, see Table 1 for details; the ingot is prepared by injection molding.

[0103] Comparative Example 1

[0104] The difference from Example 1 is that the alloy composition is different, see Table 1 for details.

[0105] Comparative Example 2

[0106] The difference from Example 1 is that: the alloy composition is slightly different, see Table 1 for details; the short-time spike aging process is different: the sample is heated by electromagnetic induction heating at a heating rate of 40°C / s to 250°C and then kept warm for about 20s.

[0107] Comparative Example 3

[0108] The difference from Example 1 is that: the alloy composition is slightly different, see Table 1 for details; the short-time spike aging process is different: a box furnace is used for differential heating, the box furnace temperature is set to 460°C, the heating rate is 3°C / s, and the actual temperature of the sample is about 120°C. After heating for 0.5 minutes, it is taken out of the furnace.

[0109] Table 1 Plate composition (wt%), thickness, state and short-time spike aging process

[0110]

[0111] Table 2 Measured data of comparative examples and embodiments

[0112]

[0113] As can be seen from Table 2, the alloys of the embodiments of the present invention all have good mechanical properties and are well compatible with the short-time spike aging forming integrated process. After forming and baking varnish treatment, the plates of the embodiments all reach a yield strength of >450MPa, a tensile strength of >500MPa, and an elongation of >8%. Among them, the short-time spike aging treatment can not only redissolve the natural aging clusters that are unfavorable to stamping into smaller clusters or even solute atoms, but also form a certain number of nucleation particles in the matrix, so that they can be quickly converted into strengthening precipitation phases in the subsequent baking varnish process, thereby improving the baking varnish response of the material.

[0114] Specifically:

[0115] In Examples 1 to 3, the performance of the formed components is good, and they are well adapted to the integrated process based on the box-type furnace and the electromagnetic induction short-time spike aging forming. The formed plates still maintain good elongation indicators.

[0116] In Example 4, the strength gradually increases after the alloying degree is increased, but it is still well adapted to the short-time spike aging forming integrated process, and the plate still maintains a good elongation index after forming.

[0117] Embodiments 5 and 6 use different short-time peak aging processes before forming, and the process window is relatively wide, which is convenient for various component processing plants to perform process screening.

[0118] Example 7 is a 0.3 mm thick foil prepared by a natural aging + short-time spike aging forming integrated process to achieve aluminum performance. This thickness of foil is suitable for 3C electronic products such as mobile phones.

[0119] The ingots of Examples 8 and 9 were prepared by injection molding, and the performance of the formed plates was significantly improved compared with the ingots produced by conventional semi-continuous casting.

[0120] The alloy composition of Comparative Example 1 does not fall within the scope of the present invention, and is insufficiently compatible with the short-time spike aging forming integrated process in the present application, resulting in insufficient strength of the sheet after forming.

[0121] The short-time spike aging process in Comparative Examples 2 and 3 does not fall within the scope of the present invention, and cracking occurs during the sheet forming process.

[0122] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components, obtained by subjecting a naturally aged aluminum alloy material to a short-time spike aging treatment; The high-strength and easy-to-form 7xxx aluminum alloy material for the thin plate member includes the following components by mass fraction: Zn 5.1~6.8%, Mg 2.1~3.1%, Cu 1.2~2.7%, Mn≤0.35%, Zr ≤0.10%, Ti≤0.10%, impurity element Si≤0.40%, Fe≤0.50%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al; The short-time peak aging is carried out by box furnace heating or electromagnetic induction heating. The box-type furnace heating treatment comprises: The naturally aged aluminum alloy material is heated to 180-240°C at a heating rate of 2-6°C / s; The electromagnetic induction heating treatment comprises: heating the naturally aged aluminum alloy material to 150-240° C. at a heating rate of 30-60° C. / s, and keeping the temperature for 30-120s.

2. The high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components according to claim 1, characterized in that: The high-strength and easy-to-form 7xxx aluminum alloy material for the thin plate member includes the following components by mass fraction: Zn 5.5~6.8%, Mg 2.5~3.1%, Cu 1.4~2.7%, Mn≤0.35%, Zr≤0.10%, Ti≤0.10%, impurity element Si≤0.40%, Fe≤0.50%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al.

3. The high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components according to claim 1, characterized in that: The set temperature of the box furnace is 410-490° C., and the heating time is 60-240 s.

4. A method for preparing the high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components as claimed in claim 1, comprising the following steps: A) melting and casting the raw materials to obtain ingots; B) subjecting the ingot to homogenization treatment, hot rolling, cold rolling, solution treatment and natural aging treatment in sequence to obtain a naturally aged aluminum alloy material; C) The naturally aged aluminum alloy material is subjected to short-time spike aging treatment to obtain high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components.

5. The preparation method according to claim 4, characterized in that: The casting is prepared by a spray deposition method; The homogenization process comprises the following steps: The ingot is kept at 400°C-450°C for 4-10 hours, and then kept at 460°C-490°C for 10-40 hours, and then air-cooled or wind-cooled to room temperature. The heating rate in the homogenization treatment is 25-75°C / h.

6. The preparation method according to claim 4, characterized in that: The hot rolling comprises the following steps: The homogenized billet is kept at 380-450°C for 3-20h, and then subjected to hot rough rolling and hot finish rolling to 4-8mm, with a final rolling temperature of 250-350°C, cooled to room temperature, and then the 4-8mm thick alloy hot-rolled coil is cold-rolled and curled to obtain a 0.2-3mm cold-rolled coil.

7. The preparation method according to claim 4, characterized in that: The temperature of the solution treatment is 450-510°C, and the time of the solution treatment is 5-20 minutes; The natural aging treatment comprises the following steps: The material after the solution treatment is naturally placed at room temperature to obtain a naturally aged aluminum alloy material.

8. A thin plate member obtained by cold stamping and baking varnish treatment of 7xxx aluminum alloy material; The 7xxx aluminum alloy material is the high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components according to any one of claims 1 to 3 or the high-strength and easy-to-form 7xxx aluminum alloy material for thin plate components prepared by the preparation method according to any one of claims 4 to 7; The thickness of the thin plate member is 0.2-3 mm.

9. The thin plate member according to claim 8, characterized in that The temperature of the paint baking treatment is 160-190° C., and the time of the paint baking treatment is 20-60 minutes.

10. A component comprising the thin plate member according to claim 8 or 9.