Method for improving corrosion resistance of stainless steel through electric pulse treatment in medium

By using sodium nitrite solution in the autoclave for alternating electrical pulse treatment, the problems of large energy consumption and limited corrosion resistance improvement in the existing stainless steel surface nitriding technology are solved, and the corrosion resistance and hardness of the stainless steel surface are improved. Large-scale promotion.

CN118895540APending Publication Date: 2024-11-05NORTHEASTERN UNIV CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410821530.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing stainless steel surface nitriding technology has problems such as large energy consumption, low production efficiency, high cost and limited improvement in corrosion resistance. In particular, traditional nitriding methods require high temperature treatment, which limits their large-scale promotion and use.

Method used

Alternating electrical pulse treatment is performed using sodium nitrite solution in the autoclave. By filling nitrogen into the autoclave, it is pressurized, and the alternating electrical pulses are applied to electrochemical nitriding of the stainless steel surface to form a nitriding layer to improve its resistance. corrosion performance.

Benefits of technology

It significantly improves the corrosion resistance of stainless steel, and improves its hardness and friction wear performance, reduces processing costs and time, and is suitable for large-scale promotion and use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895540A_ABST
    Figure CN118895540A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving corrosion resistance of stainless steel through electric pulse treatment in a medium, and relates to the technical field of stainless steel surface modification. The method comprises the following steps: placing stainless steel in an electrolyte of a high-pressure kettle as a working electrode, arranging an auxiliary electrode in the electrolyte, filling nitrogen into the high-pressure kettle to pressurize the high-pressure kettle, and performing electrochemical nitriding on the surface of the stainless steel under an alternating pulse electric field by applying alternating electric pulses to the working electrode and the auxiliary electrode. According to the method, the high-pressure autoclave is pressurized by filling nitrogen into the high-pressure autoclave, electrochemical nitriding on the surface of the stainless steel is carried out in the alternating pulsed electric field, and the corrosion resistance of the stainless steel is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stainless steel surface modification, in particular to a method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium. Background Art

[0002] Stainless steel has excellent corrosion resistance, but the service environment it faces is becoming more and more complex, and it is still restricted by problems such as insufficient hardness and poor corrosion resistance. A large number of studies have shown that nitrogen is a highly efficient austenite stabilizer. Adding nitrogen to steel not only improves the mechanical properties of steel, but also improves the corrosion resistance of stainless steel to a certain extent. Various methods have been developed to nitriding the surface of stainless steel to improve its comprehensive performance, including chemical heat treatment processes such as liquid nitriding, gas nitriding, ion nitriding, etc., which use specific media and certain temperature conditions in traditional surface nitriding technology to allow nitrogen to penetrate into the surface of the workpiece to form a thin layer of nitride.

[0003] In addition, electrochemical nitriding is currently also a treatment method to improve the comprehensive performance of stainless steel. This treatment technology mostly uses long-term constant potential polarization to nitride the surface of stainless steel in a nitrate solution.

[0004] The existing traditional nitriding technologies such as liquid nitriding, gas nitriding and ion nitriding need to be processed in a closed container at a high temperature. This preparation technology has the disadvantages of high energy consumption, low production efficiency, high processing cost and long process cycle. The dependence on equipment also limits its large-scale promotion and use. The surface hardness and friction and wear properties of stainless steel after treatment are greatly improved, but its corrosion resistance is slightly improved. The electrochemical nitriding method reduces the production cost, but still has the disadvantages of long processing time and limited improvement in corrosion resistance. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.

[0006] To this end, the present invention provides a method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium, comprising: placing the stainless steel in an electrolyte of an autoclave as a working electrode, arranging an auxiliary electrode in the electrolyte, filling nitrogen into the autoclave to pressurize the autoclave, and applying alternating electric pulses to the working electrode and the auxiliary electrode to electrochemically nitridate the surface of the stainless steel under an alternating pulse electric field.

[0007] Furthermore, the electrolyte is a sodium nitrite solution.

[0008] Furthermore, the electrolyte is a 6-8 mol / L sodium nitrite solution with a pH of 11-14.

[0009] Furthermore, the pressure of the autoclave is controlled to be 5-9 MPa.

[0010] Furthermore, the pressure of the autoclave is controlled to be 6-8 MPa.

[0011] Furthermore, the stainless steel includes 316L stainless steel, 321 stainless steel, 2101 stainless steel or single crystal FeCr15Ni15Mo2.

[0012] Furthermore, the method of electrochemically nitriding the stainless steel surface under an alternating pulse electric field comprises:

[0013] When the stainless steel is 316L stainless steel, 2101 stainless steel or single crystal FeCr15Ni15Mo2, set the anode potential E + is the open circuit potential, and the cathode potential E is set - Relative to the Ag / AgCl reference electrode, it is -0.8 to -1.6 V. In one cycle, the anode treatment time is 40 to 90 seconds, the cathode treatment time is 200 to 300 seconds, and the total electrochemical nitriding time is 70 to 140 minutes.

[0014] When the stainless steel is 321 stainless steel, set the anode potential E + The cathode potential E is set to 0.8-1.2 V relative to the Ag / AgCl reference electrode. - Relative to the Ag / AgCl reference electrode, it is -0.8 to -1.6 V. In one cycle, the treatment time of the anode is 40 to 90 s, the treatment time of the cathode is 200 to 300 s, and the total electrochemical nitriding time is 70 to 140 min.

[0015] Furthermore, the method of electrochemically nitriding the stainless steel surface under an alternating pulse electric field comprises:

[0016] When the stainless steel is 316L stainless steel, 2101 stainless steel or single crystal FeCr15Ni15Mo2, set the anode potential E + is the open circuit potential, and the cathode potential E is set - Relative to the Ag / AgCl reference electrode, it is -0.9 to -1.2 V. In one cycle, the anode treatment time is 50 to 70 seconds, the cathode treatment time is 250 to 280 seconds, and the total electrochemical nitriding time is 90 to 120 minutes.

[0017] When the stainless steel is 321 stainless steel, set the anode potential E + The cathode potential E is set to 0.9-1.1 V relative to the Ag / AgCl reference electrode. -Relative to the Ag / AgCl reference electrode, the voltage is -0.9 to -1.2 V. In one cycle, the treatment time of the anode is 50 to 70 s, the treatment time of the cathode is 250 to 280 s, and the total electrochemical nitriding time is 90 to 120 min.

[0018] Furthermore, the temperature in the autoclave is controlled to be 60-100°C.

[0019] Furthermore, the temperature in the autoclave was controlled to be 70-90°C.

[0020] Compared with the prior art, the present invention has at least the following beneficial effects:

[0021] The present invention provides a method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium. Nitrogen is filled into an autoclave to pressurize the autoclave, and electrochemical nitriding is performed on the surface of the stainless steel in an alternating pulse electric field to modify the passivation film and form a nitriding layer on the surface of the stainless steel, thereby greatly improving the corrosion resistance of the stainless steel; and the hardness and friction and wear properties of the stainless steel after treatment are improved to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the potentiodynamic polarization curves of Comparative Example 1, Example 1 and Comparative Example 5 of the present application in 3.5 wt.% NaCl solution.

[0023] Figure 2 These are electrochemical impedance diagrams of Comparative Example 1 and Example 1 of the present application when immersed in a 3.5 wt. % NaCl solution for different time periods.

[0024] Figure 3 Schematic diagram of polarization resistance of Comparative Example 1 and Example 1 of the present application when immersed in 3.5wt.% NaCl solution for different time periods.

[0025] Figure 4 It is a schematic diagram of the Mott-Schottky curves of Comparative Example 1 and Example 1 of the present application in 3.5 wt. % NaCl solution.

[0026] Figure 5 This is a friction coefficient curve diagram of comparative example 1 and embodiment 1 of the present application.

[0027] Figure 6 Schematic diagram of the potentiodynamic polarization curves of Comparative Example 2 and Example 2 of the present application in 3.5 wt. % NaCl solution.

[0028] Figure 7 It is a schematic diagram of the potentiodynamic polarization curves of Comparative Example 3 and Example 3 of the present application in 3.5 wt. % NaCl solution.

[0029] Figure 8Schematic diagram of the potentiodynamic polarization curves of Comparative Example 4 and Example 4 of the present application in 3.5 wt. % NaCl solution. DETAILED DESCRIPTION

[0030] In order to better understand the above technical solution, the technical solution of the present invention is described in detail below through specific embodiments.

[0031] An embodiment of the present invention provides a method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium, comprising: placing the stainless steel in an electrolyte of an autoclave as a working electrode, arranging an auxiliary electrode in the electrolyte, filling the autoclave with nitrogen to pressurize the autoclave, and applying alternating electric pulses to the working electrode and the auxiliary electrode to electrochemically nitridate the surface of the stainless steel under an alternating pulse electric field.

[0032] The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium provided by an embodiment of the present invention comprises the following steps: nitrogen is filled into an autoclave to pressurize the autoclave, and electrochemical nitriding is performed on the surface of the stainless steel in an alternating pulse electric field to modify the passivation film on the surface of the stainless steel and form a nitriding layer on the surface of the stainless steel, thereby greatly improving the corrosion resistance of the stainless steel; and the hardness and friction and wear properties of the stainless steel after treatment are improved to a certain extent.

[0033] It can be understood that electrochemical nitriding of the stainless steel surface under an alternating pulse electric field is to apply alternating electric pulses to the working electrode and the auxiliary electrode so that the working electrode and the auxiliary electrode alternately become the anode and the cathode, forming a nitriding layer on the stainless steel surface.

[0034] In some embodiments, the electrolyte is a sodium nitrite solution. Preferably, the electrolyte is a 6-8 mol / L sodium nitrite solution with a pH of 11-14.

[0035] In this technical solution, the principle of selecting the electrolyte solution is that under the action of the electric field, the nitrogen-containing substances in the solution can generate active nitrogen atoms, so sodium nitrite solution is selected. -Under the action of the electric field, the following reactions mainly occur, as shown in the following formulas (1) and (2). Once active nitrogen atoms are generated, they will combine with each other to form nitrogen gas. In order to obtain active nitrogen atoms to the greatest extent, in addition to the hydrogen evolution reaction, there is also a reaction in which nitrogen-containing substances are transformed into active nitrogen atoms under the action of the electric field. Increasing the pH can effectively reduce the proportion of hydrogen evolution reaction and increase the proportion of active nitrogen atom generation reaction, thereby enriching active nitrogen atoms on the surface of stainless steel. By adding sodium hydroxide to the sodium nitrite solution, the pH of the sodium nitrite solution is controlled at 11-14. By combining theoretical calculations with experiments, it is found that when the electrolyte solution is 6-8 mol / L sodium nitrite solution and the pH is 11-14, the corrosion resistance of stainless steel is significantly improved after electrochemical nitriding treatment. When the pH is lower than 11 or higher than 14, the corrosion resistance of stainless steel is not significantly improved, and even reduced.

[0036] NO2 - +4H + +3e - → N ad +2H2O (1)

[0037]

[0038] In some embodiments, the pressure of the autoclave is controlled to be 5-9 MPa. Preferably, the pressure of the autoclave is controlled to be 6-8 MPa.

[0039] In this technical solution, by applying nitrogen partial pressure, the conversion of active nitrogen atoms generated in the nitrous acid solution into nitrogen gas can be effectively suppressed. Once active nitrogen atoms are generated, they will combine with each other to form nitrogen gas. Since the N≡N bond energy is very large, the speed of reaction (2) is very fast. If the nitrogen pressure is too low, this will lead to a large consumption of active nitrogen atoms, and it will be difficult to increase the concentration gradient on the metal surface. Increasing the partial pressure of the product N2 will lead to a change in the equilibrium constant, which can reverse the equilibrium of reaction (2), N ad The concentration can be increased by one order of magnitude, which can effectively increase the nitrogen atoms N ad The concentration gradient is favorable for the active nitrogen atoms N ad Diffusion to the metal surface, thereby further realizing the low-temperature electrochemical nitriding process, thereby greatly improving the corrosion resistance of stainless steel and its surface hardness and friction and wear performance. Through multiple experiments, it was found that filling the autoclave with nitrogen to pressurize the autoclave and controlling the pressure of the autoclave to 5-9MPa, preferably 6-8MPa, can effectively increase the nitrogen atoms N ad concentration gradient.

[0040] In some embodiments, the stainless steel includes 316L stainless steel, 321 stainless steel, 2101 stainless steel, or single crystal FeCr15Ni15Mo2.

[0041] The method of electrochemically nitriding the stainless steel surface under an alternating pulse electric field comprises:

[0042] When the stainless steel is 316L stainless steel, 2101 stainless steel or single crystal FeCr15Ni15Mo2, set the anode potential E + The cathode potential E- is set to be -0.8 to -1.6 V relative to the Ag / AgCl reference electrode. In one cycle, the anode treatment time is 40 to 90 seconds, the cathode treatment time is 200 to 300 seconds, and the total electrochemical nitriding time is 70 to 140 minutes. Preferably, when the stainless steel is 316L stainless steel, 2101 stainless steel or single crystal FeCr15Ni15Mo2, the anode potential E- is set to be -0.8 to -1.6 V relative to the Ag / AgCl reference electrode. In one cycle, the anode treatment time is 40 to 90 seconds, the cathode treatment time is 200 to 300 seconds, and the total electrochemical nitriding time is 70 to 140 minutes. + is the open circuit potential, and the cathode potential E is set - Relative to the Ag / AgCl reference electrode, the voltage is -0.9 to -1.2 V. In one cycle, the treatment time of the anode is 50 to 70 s, the treatment time of the cathode is 250 to 280 s, and the total electrochemical nitriding time is 90 to 120 min.

[0043] When the stainless steel is 321 stainless steel, set the anode potential E + The cathode potential E- is set to 0.8 to 1.2 V relative to the Ag / AgCl reference electrode, and the cathode potential E- is set to -0.8 to -1.6 V relative to the Ag / AgCl reference electrode. In one cycle, the anode treatment time is 40 to 90 seconds, the cathode treatment time is 200 to 300 seconds, and the total electrochemical nitriding time is 70 to 140 minutes. Preferably, when the stainless steel is 321 stainless steel, the anode potential E is set to + The cathode potential E- is set to 0.9-1.1 V relative to the Ag / AgCl reference electrode, and the cathode potential E- is set to -0.9--1.2 V relative to the Ag / AgCl reference electrode. In one cycle, the anode treatment time is 50-70 s, the cathode treatment time is 250-280 s, and the total electrochemical nitriding time is 90-120 min.

[0044] It is understandable that the treatment conditions for different stainless steels are not exactly the same. Experiments have confirmed that under the above conditions, the same electrochemical nitriding parameters can be used for 316L stainless steel, 2101 stainless steel and single crystal FeCr15Ni15Mo2 stainless steel, where the anode potential E is set to + It is an open circuit potential, but no potential is applied to the anode; 321 stainless steel can achieve the same effect by adjusting the anode potential.

[0045] The specific electrochemical nitriding parameters are mainly determined by studying the electrochemical thermodynamics and kinetics of stainless steel materials in nitrite solutions. The E-pH diagram and cathode polarization test curve are used to determine the influence of different pH values ​​of the solution during the electrochemical nitriding of stainless steel materials, as well as the stable state of each substance at different potentials, so as to select the best potential setting, and conduct experiments to verify the theoretical feasibility. Then, through experimental tests with different time gradients, the cathode treatment time, the anode treatment time and the total time are determined. If the treatment time is too short, the proportion of active nitrogen atoms generated by the cathode reaction in the electrolyte solution will be reduced, and a higher nitrogen concentration gradient cannot be effectively formed on the metal surface, thereby failing to improve the passivation film, and failing to achieve the diffusion of nitrogen atoms to a certain depth of the metal layer to improve the corrosion resistance of stainless steel; if the treatment time is too long, the corrosion resistance of stainless steel cannot be further improved, and the treatment efficiency will be reduced. After theoretical and experimental optimization, the above-mentioned electrochemical nitriding parameters are determined, which can maximize the corrosion resistance of stainless steel materials.

[0046] It is understandable that before the electrochemical nitriding treatment, the surface of the sample to be treated is pretreated, and the pretreatment includes cutting, grinding, polishing, rinsing and drying of the stainless steel. Specifically, it can be polished with 80 mesh, 240 mesh, 400 mesh, 600 mesh, 1000 mesh and 2000 mesh silica sandpaper in sequence, polished with diamond grinding paste, and cleaned in ethanol solution using an ultrasonic cleaner.

[0047] In some embodiments, the temperature in the autoclave is controlled at 60-100°C, preferably, the temperature in the autoclave is controlled at 70-90°C.

[0048] In this technical solution, the temperature in the autoclave is controlled at 60-100°C, preferably 70-90°C. It can be understood that the temperature needs to be controlled within a certain range. If the temperature is too high, the surface of the treated sample will turn yellow and the roughness will increase, and the corrosion resistance will be reduced. If the temperature is too low, the reaction rate will decrease, which is not conducive to the generation of active nitrogen atoms and the diffusion process to the metal surface, and thus the corrosion resistance of the experimental material cannot be effectively improved.

[0049] Example 1: An electric pulse treatment method for 316L stainless steel

[0050] A method for preparing a 316L stainless steel low-temperature surface pressurized electrochemical nitriding film comprises the following steps:

[0051] Step 1), cut 316L stainless steel into samples of 10 mm × 10 mm × 10 mm by wire cutting.

[0052] Step 2), the 316L stainless steel sample was polished with 80 mesh, 240 mesh, 400 mesh, 600 mesh, 1000 mesh and 2000 mesh silica sandpaper in sequence, then polished with diamond grinding paste, and finally cleaned in ethanol solution with an ultrasonic cleaner for 10 minutes and then dried to obtain a 316L stainless steel sample.

[0053] Step 3), prepare 6-8 mol / L sodium nitrite solution, and adjust the pH to 11-14 with sodium hydroxide solution to obtain an electrolyte solution.

[0054] Step 4), connecting the electrolyte solution, the 316L stainless steel sample obtained in step 2) and a high-voltage electrochemical test kettle to form a working circuit.

[0055] Step 5), nitrogen is charged into the autoclave to control the pressure of the autoclave at 8 MPa.

[0056] Step 6), heat the high-voltage electrochemical test kettle and control the solution in the kettle at 80°C.

[0057] Step 7), set up the electrochemical test program, E + =OCP (no potential applied), E - =-1.0124V Ag / AgCl In one cycle, the cathode and anode treatment times were 277s and 56s respectively. The power was turned on and the test kettle was treated for 120min. The surface of the 316L stainless steel sample was electrochemically nitrided.

[0058] Step 8), rinse the treated samples with alcohol and blow dry for subsequent testing and characterization.

[0059] Example 2: An electric pulse treatment method for 2101 stainless steel

[0060] The electric pulse treatment of 2101 stainless steel was carried out according to the method of Example 1.

[0061] Example 3: An electric pulse treatment method for 321 stainless steel

[0062] The electric pulse treatment of 321 stainless steel was carried out according to the method of Example 1.

[0063] The difference from Example 1 is that the electrochemical test procedure anode potential E + The settings are different. + =+1.0676V Ag / AgCl , E - =-1.0124V Ag / AgCl In one cycle, the cathode and anode treatment times were 277s and 56s respectively. The power was turned on and the test kettle was treated for 120min. The surface of the 321 stainless steel sample was electrochemically nitrided.

[0064] Example 4: An electric pulse treatment method for single crystal FeCr15Ni15Mo2 stainless steel

[0065] The surface of the single crystal FeCr15Ni15Mo2 workpiece was subjected to pressure electrochemical nitriding treatment according to the method of Example 1.

[0066] Comparative Example 1

[0067] The 316L stainless steel sample of Comparative Example 1 is not subjected to electric pulse treatment, wherein the preparation method of the 316L stainless steel sample includes:

[0068] Step 1): Cut 316L stainless steel into samples of 10 mm × 10 mm × 10 mm using wire cutting.

[0069] Step 2): The 316L stainless steel sample was polished with 80 mesh, 240 mesh, 400 mesh, 600 mesh, 1000 mesh and 2000 mesh silica sandpaper in sequence, and then polished with diamond grinding paste. Finally, it was cleaned in an ethanol solution with an ultrasonic cleaner for 10 minutes and then dried to obtain a 316L stainless steel sample.

[0070] Comparative Example 2

[0071] The 2101 stainless steel sample of Comparative Example 2 is not subjected to electric pulse treatment, wherein the preparation method of the 2101 stainless steel sample includes:

[0072] Step 1): Cut 2101 stainless steel into samples of 10 mm × 10 mm × 10 mm using wire cutting.

[0073] Step 2): The 2101 stainless steel sample was polished with 80 mesh, 240 mesh, 400 mesh, 600 mesh, 1000 mesh and 2000 mesh silica sandpaper in sequence, then polished with diamond grinding paste, and finally cleaned in an ethanol solution with an ultrasonic cleaner for 10 minutes and then dried to obtain a 2101 stainless steel sample.

[0074] Comparative Example 3

[0075] The 321 stainless steel sample of Comparative Example 3 is not subjected to electric pulse treatment, wherein the preparation method of the 321 stainless steel sample includes:

[0076] Step 1): Cut 321 stainless steel into samples of 10 mm × 10 mm × 10 mm using wire cutting.

[0077] Step 2): The 321 stainless steel sample was polished with 80 mesh, 240 mesh, 400 mesh, 600 mesh, 1000 mesh and 2000 mesh silica sandpaper in sequence, then polished with diamond grinding paste, and finally cleaned in an ethanol solution with an ultrasonic cleaner for 10 minutes and then dried to obtain a 321 stainless steel sample.

[0078] Comparative Example 4

[0079] The single crystal FeCr15Ni15Mo2 sample of comparative example 4 is not subjected to electric pulse treatment, wherein the preparation method of the single crystal FeCr15Ni15Mo2 sample includes:

[0080] Step 1): Cut the single crystal FeCr15Ni15Mo2 into samples of 10mm×10mm×10mm by wire cutting.

[0081] Step 2): The single crystal FeCr15Ni15Mo2 sample is polished with 80 mesh, 240 mesh, 400 mesh, 600 mesh, 1000 mesh and 2000 mesh silica sandpaper in sequence, and then polished with diamond grinding paste. Finally, it is cleaned in an ethanol solution with an ultrasonic cleaner for 10 minutes and then blown dry to obtain a single crystal FeCr15Ni15Mo2 sample.

[0082] Comparative Example 5: A method for treating 316L stainless steel with electric pulses in a medium

[0083] A method for preparing a low-temperature surface electrochemical nitriding film of 316L stainless steel comprises the following steps:

[0084] Step 1), cut 316L stainless steel into samples of 10 mm × 10 mm × 10 mm by wire cutting.

[0085] Step 2), the 316L stainless steel sample was polished with 80 mesh, 240 mesh, 400 mesh, 600 mesh, 1000 mesh and 2000 mesh silica sandpaper in sequence, then polished with diamond grinding paste, and finally cleaned in ethanol solution with an ultrasonic cleaner for 10 minutes and then dried to obtain a 316L stainless steel sample.

[0086] Step 3), prepare 6-8 mol / L sodium nitrite solution, and adjust the pH to 11-14 with sodium hydroxide solution to obtain an electrolyte solution.

[0087] Step 4), connecting the electrolyte solution, the 316L stainless steel sample obtained in step 2) and a high-voltage electrochemical test kettle to form a working circuit.

[0088] Step 5), control the pressure of the autoclave to 0.1 MPa at normal pressure.

[0089] Step 6), heat the high-voltage electrochemical test kettle and control the solution in the kettle at 80°C.

[0090] Step 7), set up the electrochemical test program, E + =OCP, E - =-1.0124V Ag / AgCl In one cycle, the cathode and anode treatment times were 277s and 56s respectively. The power was turned on and the test kettle was treated for 120min. The surface of the 316L stainless steel sample was electrochemically nitrided.

[0091] Step 8), rinse the treated samples with alcohol and blow dry for subsequent testing and characterization.

[0092] The difference between Comparative Example 5 and Example 1 is that in step (5), nitrogen is not charged into the autoclave, and the pressure of the autoclave is controlled at normal pressure 0.1 MPa.

[0093] Results and Discussion

[0094] from Figure 1 It can be clearly seen that after the surface pressurized electrochemical nitriding treatment, the passivation range of Example 1 is significantly enlarged and the corrosion resistance is significantly improved. Table 1 shows the electrochemical parameters obtained from the potentiodynamic polarization curve.

[0095] Table 1 Electrochemical parameters of Comparative Example 1, Example 1 and Comparative Example 5

[0096]

[0097] Table 1 shows the E before and after pressurized electrochemical nitriding treatment corr 、E b,100 with I corr The self-corrosion current density of Comparative Example 1 is 1.01×10 -7 μA·cm -2 Down to 2.94×10 -8 μA·cm -2, that is, the self-corrosion current density of 316L stainless steel after electric pulse treatment is reduced by one order of magnitude compared with the 316L stainless steel substrate without electric pulse treatment. The pitting breakdown potential of Example 1 after electric pulse (pressurized electrochemical nitriding) treatment is 1008.37mV, which is about 578mV higher than the pitting breakdown potential of Comparative Example 1 of 430.89mV. The pitting breakdown potential is greatly improved, and the corrosion resistance is greatly improved. As for Comparative Example 5, after electric pulse (normal pressure electrochemical nitriding) treatment at normal pressure of 0.1Mpa, the self-corrosion current density and pitting breakdown potential are compared with Example 1. Example 1 has more excellent pitting resistance, indicating that the application of nitrogen partial pressure has an important influence on the electrochemical nitriding process. The potentiodynamic polarization curve can only represent the short-term corrosion resistance of stainless steel, and the long-term corrosion resistance still needs further testing.

[0098] from Figure 2 It can be seen that the Nyquist diagrams of both Comparative Example 1 and Example 1 are single capacitive reactance arcs, and the radius of the capacitive reactance arc of Example 1 is significantly increased; in the Bode diagram, the impedance film of Example 1 is increased compared with Comparative Example 1; the combined results of the Nyquist diagram and the Bode diagram show that the stability of the passivation film on the surface of Example 1 is gradually enhanced, the corrosion rate is reduced, and the corrosion resistance is improved.

[0099] from Figure 3 It can be seen that during the long-term immersion process, the polarization resistance value of Example 1 is always one to two orders of magnitude higher than the resistance value of Comparative Example 1, that is, in the long-term corrosion resistance test, the corrosion resistance of Example 1 is still better than that of Comparative Example 1.

[0100] from Figure 4 It can be seen that the comparative example 1 has larger passivation film defects than the example 1. Table 2 shows the donor density of the comparative example 1 and the example 1 obtained from the Mott-Schottky curve.

[0101] Table 2 Donor density of comparative example 1 and example 1

[0102]

[0103] Table 2 shows the donor density N before and after pressurized electrochemical nitriding treatment D Value, N of Comparative Example 1 D 87.53(10 24 cm 3 ), while Example 1 dropped to 8.87 (10 24 cm 3 ), the donor density N of Example 1 after pressurized electrochemical nitriding treatment DCompared with comparative example 1, it is greatly reduced, which shows that the pressurized electrochemical nitriding treatment can reduce the defects of the passivation film, improve the stability of the passivation film, and greatly improve the corrosion resistance of the stainless steel.

[0104] The microhardness measurement results of Example 1 and Comparative Example 1 are shown in Table 3. It can be seen from Table 3 that the microhardness of Example 1 after pressurized electrochemical nitriding treatment is also improved compared with Comparative Example 1.

[0105] Table 3 Microhardness of comparative examples and embodiments

[0106]

[0107] from Figure 5 The friction coefficient curve diagram shows that in the friction and wear test conducted under a constant load of 10N, the friction coefficients of Example 1 and Comparative Example 1 both drop rapidly in the initial stage and enter a stable stage thereafter. The friction coefficient of Comparative Example 1 fluctuates stably around 0.60, and the friction coefficient of Example 1 is stable at around 0.50, which is significantly lower than the friction coefficient of the untreated sample. In addition, the friction coefficient of Example 1 is relatively stable without large fluctuations. This indicates that the friction coefficient of Example 1 after pressurized electrochemical nitriding treatment has greater advantages in both size and stability.

[0108] Table 4 Comparative Examples and Examples Friction and Wear Test Weight Loss Results

[0109]

[0110] Table 4 shows the weight loss results of friction and wear experiments of Comparative Example 1 and Example 1. From the data in Table 4, it can be seen that the weight loss of Example 1 after pressurized electrochemical nitriding treatment is 0.5 mg, which is lower than the weight loss of Comparative Example 1.

[0111] The comprehensive friction coefficient and weight loss test results show that the surface wear resistance of Example 1 treated with pressurized electrochemical nitriding is significantly better than that of Comparative Example 1 which is not treated, and the microhardness of Example 1 is higher.

[0112] In summary, the present invention utilizes low-temperature pressurized electrochemical nitriding to modify the passivation film layer of 316L stainless steel and form a nitriding layer of a certain depth. The treated 316L stainless steel has good corrosion resistance, and the surface wear resistance and hardness are also improved to a certain extent.

[0113] from Figure 6 It can be seen that after surface electrochemical nitriding treatment, the passivation range of Example 2 is significantly increased compared with that of Comparative Example 2, and the current density is reduced by nearly an order of magnitude, and the pitting breakdown potential is increased by 500 mV, indicating that the pitting corrosion resistance of Example 2 after treatment is significantly improved.

[0114] from Figure 7 It can be seen that in the potentiodynamic polarization test of Example 3 after the pressurized electrochemical nitriding treatment, the pitting breakdown potential and the passivation range are greatly improved, and the current density is reduced by two orders of magnitude, indicating that the pitting corrosion resistance of the 321 stainless steel treated in Example 3 is significantly improved.

[0115] from Figure 8 It can be seen that the single crystal FeCr15Ni15Mo2 treated by pressurized electrochemical nitriding in Example 4 has an increased corrosion potential in the potentiodynamic polarization curve and an increased passivation interval compared to the untreated test sample, and the potential required for pitting breakdown under the same conditions is also significantly higher than that of the untreated sample in Comparative Example 4. Therefore, it can be concluded that the treated sample has high pitting resistance compared to the untreated sample.

[0116] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed. The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application. The above are only preferred implementation methods of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.

Claims

1. A method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium, characterized in that: include: Stainless steel is placed in the electrolyte of an autoclave as a working electrode, and an auxiliary electrode is set in the electrolyte. Nitrogen is filled into the autoclave to pressurize the autoclave. By applying alternating electric pulses to the working electrode and the auxiliary electrode, the stainless steel surface is electrochemically nitrided under an alternating pulse electric field.

2. The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium according to claim 1, characterized in that: The electrolyte is sodium nitrite solution.

3. The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium according to claim 2, characterized in that: The electrolyte is a 6-8 mol / L sodium nitrite solution with a pH of 11-14.

4. The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium according to claim 3, characterized in that: The pressure of the autoclave was controlled to be 5-9 MPa.

5. The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium according to claim 4, characterized in that: The pressure of the autoclave was controlled at 6-8 MPa.

6. The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium according to claim 4 or 5, characterized in that: The stainless steel includes 316L stainless steel, 321 stainless steel, 2101 stainless steel or single crystal FeCr15Ni15Mo2.

7. The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium according to claim 6, characterized in that: The method of electrochemically nitriding the stainless steel surface under an alternating pulse electric field comprises: When the stainless steel is 316L stainless steel, 2101 stainless steel or single crystal FeCr15Ni15Mo2, set the anode potential E + is the open circuit potential, and the cathode potential E is set - Relative to the Ag / AgCl reference electrode, it is -0.8 to -1.6 V. In one cycle, the anode treatment time is 40 to 90 seconds, the cathode treatment time is 200 to 300 seconds, and the total electrochemical nitriding time is 70 to 140 minutes. When the stainless steel is 321 stainless steel, set the anode potential E + The cathode potential E is set to 0.8-1.2 V relative to the Ag / AgCl reference electrode. - Relative to the Ag / AgCl reference electrode, it is -0.8 to -1.6 V. In one cycle, the treatment time of the anode is 40 to 90 s, the treatment time of the cathode is 200 to 300 s, and the total electrochemical nitriding time is 70 to 140 min.

8. The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium according to claim 7, characterized in that: The method of electrochemically nitriding the stainless steel surface under an alternating pulse electric field comprises: When the stainless steel is 316L stainless steel, 2101 stainless steel or single crystal FeCr15Ni15Mo2, set the anode potential E + is the open circuit potential, and the cathode potential E is set - Relative to the Ag / AgCl reference electrode, it is -0.9 to -1.2 V. In one cycle, the anode treatment time is 50 to 70 seconds, the cathode treatment time is 250 to 280 seconds, and the total electrochemical nitriding time is 90 to 120 minutes. When the stainless steel is 321 stainless steel, set the anode potential E + The cathode potential E is set to 0.9-1.1 V relative to the Ag / AgCl reference electrode. - Relative to the Ag / AgCl reference electrode, the voltage is -0.9 to -1.2 V. In one cycle, the treatment time of the anode is 50 to 70 s, the treatment time of the cathode is 250 to 280 s, and the total electrochemical nitriding time is 90 to 120 min.

9. The method for improving the corrosion resistance of stainless steel by electric pulse treatment in a medium according to claim 8, characterized in that: The temperature in the autoclave was controlled at 60-100°C.