Stretching bath lotion for wet spinning, preparation method of stretching bath lotion and application of stretching bath lotion in preparation of conductive acrylic fibers

By using copper source, vulcanizing agent and permeable dispersant in the spinning liquid, conducting conductive modification during the fiber stretching process, the mechanical properties of the conductive fibers and the antistatic effect are solved. The problem of durability has achieved efficient and durable conductive performance improvement.

CN118895570APending Publication Date: 2024-11-05QINGDAO UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411191723.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The addition of antistatic agents or conductive agents to the spinning liquid of the existing conductive fibers leads to a decrease in the mechanical properties of the fibers, and the antistatic effect of the surface modification method is not durable and difficult to maintain in a low-humidity environment.

Method used

Wet spinning stretching bath solution, including copper source, vulcanizing agent and permeable dispersant, is used to conduct conductive modification during fiber stretching, and the coordination complexing of copper ions and polyacrylonitrile macromolecules is used. Improve the conductivity of the fibers and maintain mechanical properties.

Benefits of technology

It achieves the improvement of the efficient durability and mechanical properties of conductive fibers, avoids the problem of uneven distribution of fiber structure, and is suitable for special textiles such as anti-static work clothes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895570A_ABST
    Figure CN118895570A_ABST
Patent Text Reader

Abstract

The invention discloses a stretching bath lotion for wet spinning. The stretching bath lotion is prepared from the following raw materials in parts by weight: 10-55 parts of a copper source; 10-65 parts of a vulcanizing agent; 5-8 parts of a permeation dispersant; and 100 to 500 parts of deionized water. The invention also discloses application of the stretching bath lotion for wet spinning in preparation of conductive acrylic fibers. In the spinning solution stage, no antistatic agent, conductive agent or conductive material and auxiliary agent is added, so that the problems of dispersion and agglomeration caused by the addition of the antistatic agent, conductive agent or conductive material and auxiliary agent are avoided, and the influence of uneven distribution on the acrylic fiber quality is avoided; meanwhile, by utilizing the existing technical route of spinning polyacrylonitrile fibers by a wet method, the fibers are subjected to conductive modification by adopting a stretching bath in a fiber stretching forming stage, so that the intrinsic performance of the fibers is not influenced, and the conductive or antistatic performance of the fibers is also improved. The conductive acrylic fiber has obvious social value and economic benefit, is endowed with conductive performance in the process of preparing the acrylic fiber, greatly reduces the production cost, and is suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive acrylic fibers, and in particular relates to a stretching bath for wet spinning, a preparation method and application in the preparation of conductive acrylic fibers. Background Art

[0002] Acrylic fiber, also known as polyacrylonitrile fiber, has high elasticity, strength, heat resistance, light resistance and corrosion resistance, and is widely used in the textile industry. Due to its bright color, light and soft texture, and its appearance and feel are similar to wool, it is called "synthetic wool". The polyacrylonitrile (PAN) macromolecules in acrylic fiber contain a large number of hydrophobic groups, which makes acrylic fiber highly hydrophobic and extremely poor in hygroscopicity. Acrylic fiber, known as synthetic wool, is often used in autumn and winter, so it is very easy to generate static electricity. Static electricity is easily generated by friction and induction during the production, processing and use of textiles. During the use of acrylic textiles, the accumulation of static electricity can easily cause dust to adhere, causing clothing to entangle limbs, easily causing adhesion discomfort, and can cause physiological changes such as increased blood pH, all of which greatly reduce the wearing performance of acrylic textiles. In addition, the higher potential generated by static electricity may also cause electric shock to the human body, and may also break down electronic components and cause damage to electronic components; the electromagnetic radiation generated by electrostatic discharge can cause electromagnetic interference to various electronic equipment and information systems. In order to eliminate static electricity in acrylic fibers and their products, promote the rapid development of acrylic production, and meet people's growing demand for high-quality fibers and fabrics, people began to seek methods to modify the conductive properties of acrylic fibers to enhance their antistatic properties and improve their wearing comfort.

[0003] Antistatic technology for textile materials is mainly divided into three categories:

[0004] (1) Surface treatment method: Use surfactant to hydrophilize fibers or fabrics to improve the hygroscopicity of fibers, thereby reducing the resistivity of textiles and accelerating charge dissipation. However, the antistatic effect of this method is difficult to preserve for a long time, and it is easy to cause acrylic fibers to have poor washing resistance, and they do not show antistatic properties in low humidity environments;

[0005] (2) Blending spinning method: Antistatic fibers are prepared by blending, copolymerizing, or grafting fiber-forming polymers to introduce hydrophilic polar groups, or by adding antistatic agents into the fibers. Antistatic fibers prepared by this method have a significant impact on the original spinning formation of the fibers, as well as the mechanical properties and functional products of the formed fibers, due to the excessive addition of antistatic components to the spinning solution, which is not conducive to the preparation of high-quality fibers.

[0006] (3) Research and development of conductive fibers. The research on conductive fibers mainly includes the research on uniform conductive fibers made of conductive materials such as metal fibers, carbon fibers, and conductive polymers; or the research on coated conductive fibers obtained by coating the outer layer of synthetic fibers with conductive materials such as carbon black. According to research, the resistivity of conductive fibers obtained by composite spinning of carbon black or metal compounds and fiber-forming polymers is generally less than 10 7 Ω·cm, even as small as 10 4 ~10 5 Ω·cm. The development and application of conductive fibers make the antistatic effect of the textiles made significant, and the conductive effect is durable and not affected by the environmental humidity. It can also be used in special functional textiles such as antistatic work clothes.

[0007] However, after the conductive additives used in the existing conductive fibers are applied to textiles, additives such as carbon black are generally insoluble in solvents, and the polyacrylonitrile solution prepared during spinning has a high viscosity. Therefore, when preparing the polyacrylonitrile solution, the conductive additives tend to clump together, which further leads to uneven dispersion of the additives in the final formed fibers. At the same time, the added additives will make the molecular chains in the fibers rigid, which ultimately leads to low strength, brittleness, easy breakage and other problems in the finished fibers, making it impossible to use the fibers for downstream finished products.

[0008] For example, Chinese patent CN103255634A has developed a polyacrylonitrile / polyaniline composite micro-nano conductive fiber. In this scheme, polyaniline and polyethylene glycol are used as raw materials, and wet spinning technology is used for synthesis. The purpose of adding polyethylene glycol is to use the water solubility of polyethylene glycol to produce micropores on the fiber, and then aniline is polymerized on the micropores to finally obtain conductive fibers. Although this method has obtained fibers with good electrical conductivity, acrylic fibers have structural defects due to the presence of micropores, making the fiber strength lower and the cost higher. For example, the document "The influence of polyethylene glycol-modified polymer spinning solution on the cross-sectional morphology and crystalline structure of wet-spun polyacrylonitrile primary fibers" also discloses the influence of polyethylene glycol on increasing the hydrophilicity of the fiber. This method uses wet spinning to produce acrylic fibers. Although good electrical conductivity is obtained, there is still a problem of uneven fiber structure distribution leading to defective performance. Chinese patent CN111088528A discloses a method for preparing a polyacrylonitrile conductive spinning solution, which effectively improves the phenomenon of agglomeration that is easy to occur during the production process and improves the conductive properties of acrylic fibers by adding a segment softener and an acid-doped polyaniline conductive agent to the polyacrylonitrile spinning solution. However, the inventors did not discuss whether the addition of the conductive agent to the spinning solution affects the original elasticity, strength, heat resistance, light resistance and other properties of acrylic fibers.

[0009] To sum up, how to avoid the defect of reduced physical and mechanical properties caused by the addition of antistatic agents, conductive agents and other functional additives in the spinning solution, which affects the purity of polyacrylonitrile polymer due to the addition of other components, and solve the problem of poor conductive durability of acrylic fibers caused by conventional surface modification, while giving the fibers excellent conductive properties, has become a difficult problem that technicians in the field of conductive acrylic fibers urgently need to solve. Summary of the invention

[0010] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a stretching bath for wet spinning, a preparation method and an application in the preparation of conductive acrylic fibers, which can effectively impart antistatic or conductive functionality to fibers, greatly improve the conductive durability and ensure that the fibers have good mechanical properties.

[0011] In order to solve the above technical problems, the technical solution adopted by the present invention is: a stretching bath for wet spinning, characterized in that it is composed of the following raw materials in parts by weight:

[0012]

[0013] In the above-mentioned wet spinning stretching bath, the copper source is copper sulfate and / or copper chloride.

[0014] In the above-mentioned stretching bath for wet spinning, the vulcanizing agent is any one or more of sodium thiosulfate and sodium sulfate.

[0015] In the above-mentioned stretching bath for wet spinning, the penetrating dispersant is any one or more of fatty alcohol polyoxyethylene ether, octyl phosphate, ethylene oxide, and sodium secondary alkyl sulfonate.

[0016] A method for preparing a stretching bath for wet spinning comprises dissolving a copper source, a sulfiding agent and a penetrating dispersant in deionized water according to the weight parts respectively, and dispersing the mixture uniformly by mixing and stirring to obtain the wet spinning stretching bath.

[0017] The above-mentioned wet spinning stretching bath is used in the preparation of conductive acrylic fibers.

[0018] A method for preparing conductive acrylic fiber by wet spinning, comprising the following steps:

[0019] 1. Preparation of spinning solution:

[0020] (1) Prepare acrylic fiber spinning solution required for wet spinning and set aside;

[0021] 2. Obtaining primary fiber:

[0022] (2) the acrylic fiber spinning solution prepared in step (1) is accurately metered by a metering pump and ejected from a spinneret to form a thin stream;

[0023] (3) The thin stream enters the coagulation bath for solidification to form a tow.

[0024] (4) the filament bundle is preheated and stretched in a preheating bath to obtain wet-spun acrylic primary fibers;

[0025] 3. Conductive modification:

[0026] (5) the spun fibers enter a stretching bath, and the spun fibers are soaked and stretched by the stretching bath to obtain conductive acrylic fibers;

[0027] 4. Post-processing:

[0028] (6) Washing, oiling and drying the conductive acrylic fiber obtained in step (5) to obtain the desired conductive acrylic fiber.

[0029] In the above-mentioned method for preparing conductive acrylic fiber by wet spinning, in the step (4), the preheating bath is a copper source solution with a mass fraction of 5-20%, and the bath temperature is 60-65°C.

[0030] In the above-mentioned method for preparing conductive acrylic fiber by wet spinning, in the step (5), the temperature of the stretching bath is 90-98° C., and the immersion time is 15-60 min.

[0031] In the above-mentioned method for preparing conductive acrylic fiber by wet spinning, the copper source in the copper source solution is copper sulfate and / or copper chloride.

[0032] The advantages of the stretching bath for wet spinning, the preparation method and the application in preparing conductive acrylic fibers of the present invention are: while the polyacrylonitrile nascent fibers are being stretched in the stretching bath, the conductive bath is used to perform a conductive modification treatment on the fibers. During the stretching of the nascent fibers in the stretching bath, the polyacrylonitrile molecular chains are orderly oriented and arranged, and the conductive modification treatment is performed in this process. At this time, the orientation degree of the macromolecular chains has not been completed. Compared with the polyacrylonitrile fibers with a higher orientation degree, the copper ions and sulfur atoms in the conductive bath are more likely to enter the interior of the nascent fiber molecules, which is beneficial to the improvement of the conductive performance. The present invention avoids adding functional additives such as antistatic agents and conductive agents to the spinning solution through the conductive modification treatment in the wet spinning stretching stage. Thus, the influence of the addition of other components on the purity of the polyacrylonitrile polymer is avoided. The coordination and complexation of the coordinated metal ions with the polyacrylonitrile macromolecules is used to solve the problem of poor durability of conventional surface modification. The conductive effect is durable and is not affected by the environmental humidity, and can be applied to special functional textiles such as antistatic work clothes. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a physical comparison diagram of polyacrylonitrile filaments without conductive modification and after conductive modification;

[0034] Figure 2This is the SEM electron microscope photo of unmodified polyacrylonitrile filament;

[0035] Figure 3 This is a SEM electron microscope photograph of the conductive polyacrylonitrile filament prepared in Example 2 of the present invention;

[0036] Figure 4 This is a surface element analysis diagram of the conductive polyacrylonitrile filament prepared in Example 2 of the present invention;

[0037] Figure 5 The mechanical properties test diagram of polyacrylonitrile filament before and after modification;

[0038] Figure 6 Schematic diagram of the test process for the washability of modified polyacrylonitrile fiber. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0040] In the present invention, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the attached drawings; while "inside" and "outside" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order. The term "plurality" means "two or more".

[0041] A stretching bath for wet spinning is composed of the following raw materials in parts by weight: 10-55 parts of a copper source; 10-65 parts of a vulcanizing agent; 5-8 parts of a penetrating dispersant; and 100-500 parts of deionized water. The preparation method of the stretching bath for wet spinning is as follows: the copper source, the vulcanizing agent, and the penetrating dispersant are respectively dissolved in deionized water according to the parts by weight, and dispersed uniformly by mixing and stirring. The copper source is copper sulfate and / or copper chloride. The vulcanizing agent is any one or more of sodium thiosulfate and sodium sulfate. The penetrating dispersant is any one or more of fatty alcohol polyoxyethylene ether, octyl phosphate, ethylene oxide, and sodium secondary alkyl sulfonate.

[0042] The wet spinning stretching bath is applied to the preparation of conductive acrylic fibers. Specifically, a method for preparing conductive acrylic fibers by wet spinning comprises the following steps:

[0043] 1. Preparation of spinning solution:

[0044] (1) Prepare acrylic fiber spinning solution required for wet spinning and set aside;

[0045] 2. Obtaining primary fiber:

[0046] (2) the acrylic fiber spinning solution prepared in step (1) is accurately metered by a metering pump and ejected from a spinneret to form a thin stream;

[0047] (3) The thin stream enters the coagulation bath for solidification to form a tow.

[0048] (4) the filament bundle is preheated and stretched in a preheating bath to obtain wet-spun acrylic primary fibers;

[0049] 3. Conductive modification:

[0050] (5) the spun fibers enter a stretching bath, and the spun fibers are soaked and stretched by the stretching bath to obtain conductive acrylic fibers;

[0051] 4. Post-processing:

[0052] (6) Washing, oiling and drying the conductive acrylic fiber obtained in step (5) to obtain the desired conductive acrylic fiber.

[0053] Wherein, in step (4), the preheating bath is a copper source solution with a mass fraction of 5-20%, the bath temperature is 60-65°C, and the copper source in the copper source solution is copper sulfate and / or copper chloride. In step (5), the temperature of the stretching bath is 90-98°C, and the immersion time is 15-60 minutes.

[0054] The present invention firstly utilizes a preheating bath to treat the tow before stretching modification. In the preheating bath, a copper source solution is used to allow the copper ions in the solution to be pre-adsorbed on the surface of the polyacrylonitrile primary fiber. In the subsequent stretching bath, based on the molecular diffusion effect, the copper ions are more conducive to the diffusion of the inside of the polyacrylonitrile fiber. Through the conductive modification treatment in the wet spinning stretching stage, the addition of functional additives such as antistatic agents and conductive agents to the spinning solution is avoided. Thus, the influence of the addition of other components on the purity of the polyacrylonitrile polymer is avoided. The coordination and complexation of the coordinated metal ions and the polyacrylonitrile macromolecules is utilized to solve the problem of poor durability of conventional surface modification. The method utilizes the process characteristics of preparing polyacrylonitrile fibers by the current wet spinning technology, and conducts conductive modification on the fibers in the filament stretching stage, which maximizes the high quality of the raw materials and gives the fibers antistatic or conductive functionality, and is an efficient and convenient rapid modification technology.

[0055] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0056] Example 1

[0057] A stretching bath for wet spinning is composed of the following raw materials in parts by weight: 10 parts of a copper source; 10 parts of a vulcanizing agent; 5 parts of a penetrating dispersant; and 100 parts of deionized water. The preparation method of the stretching bath for wet spinning is as follows: the copper source, the vulcanizing agent, and the penetrating dispersant are respectively dissolved in deionized water according to the parts by weight, and the mixture is uniformly dispersed by mixing and stirring to obtain the stretching bath.

[0058] The copper source is copper sulfate, the vulcanizing agent is sodium thiosulfate, and the penetrating dispersant is fatty alcohol polyoxyethylene ether.

[0059] The wet spinning stretching bath is applied to the preparation of conductive acrylic fibers. Specifically, the method for preparing conductive acrylic fibers by wet spinning comprises the following steps:

[0060] 1. Preparation of spinning solution:

[0061] (1) Prepare acrylic fiber spinning solution required for wet spinning and set aside;

[0062] 2. Obtaining primary fiber:

[0063] (2) the acrylic fiber spinning solution prepared in step (1) is accurately metered by a metering pump and ejected from a spinneret to form a thin stream;

[0064] (3) The thin stream enters the coagulation bath for solidification to form a tow.

[0065] (4) the filament bundle is preheated and stretched in a preheating bath, wherein the preheating bath is a 5% by mass copper source solution, the bath temperature is 60° C., and the copper source in the copper source solution is copper sulfate and / or copper chloride, to obtain wet-spun acrylic primary fibers;

[0066] 3. Conductive modification:

[0067] (5) the spun fibers enter a stretching bath, and are soaked and stretched by a stretching bath liquid, the temperature of the stretching bath liquid is 90° C., and the soaking time is 15 min, thereby obtaining conductive acrylic fibers;

[0068] 4. Post-processing:

[0069] (6) Washing, oiling and drying the conductive acrylic fiber obtained in step (5) to obtain the desired conductive acrylic fiber.

[0070] Example 2

[0071] A stretching bath for wet spinning is composed of the following raw materials in parts by weight: 30 parts of a copper source; 40 parts of a vulcanizing agent; 6 parts of a penetrating dispersant; and 300 parts of deionized water. The preparation method of the stretching bath for wet spinning is as follows: the copper source, the vulcanizing agent, and the penetrating dispersant are dissolved in deionized water according to the parts by weight, and the mixture is uniformly dispersed by mixing and stirring to obtain the stretching bath. The copper source is copper sulfate and copper chloride, the vulcanizing agent is sodium sulfate, and the penetrating dispersant is ethylene oxide.

[0072] The wet spinning stretching bath is applied to the preparation of conductive acrylic fibers. Specifically, the method for preparing conductive acrylic fibers by wet spinning comprises the following steps:

[0073] 1. Preparation of spinning solution:

[0074] (1) Prepare acrylic fiber spinning solution required for wet spinning and set aside;

[0075] 2. Obtaining primary fiber:

[0076] (2) the acrylic fiber spinning solution prepared in step (1) is accurately metered by a metering pump and ejected from a spinneret to form a thin stream;

[0077] (3) The thin stream enters the coagulation bath for solidification to form a tow.

[0078] (4) the filament bundle is preheated and stretched in a preheating bath, wherein the preheating bath is a copper source solution having a mass fraction of 13%, the bath temperature is 63° C., and the copper source in the copper source solution is copper sulfate and / or copper chloride, to obtain wet-spun acrylic primary fibers;

[0079] 3. Conductive modification:

[0080] (5) the spun fibers enter a stretching bath, and are soaked and stretched by the stretching bath liquid for modification. The temperature of the stretching bath liquid is 95° C., and the soaking time is 35 min, thereby obtaining conductive acrylic fibers.

[0081] 4. Post-processing:

[0082] (6) Washing, oiling and drying the conductive acrylic fiber obtained in step (5) to obtain the desired conductive acrylic fiber.

[0083] Example 3

[0084] A stretching bath for wet spinning is composed of the following raw materials in parts by weight: 55 parts of a copper source; 65 parts of a sulfiding agent; 8 parts of a penetrating dispersant; and 500 parts of deionized water. The preparation method of the stretching bath for wet spinning is as follows: the copper source, the sulfiding agent, and the penetrating dispersant are respectively dissolved in deionized water according to the parts by weight, and the mixture is uniformly dispersed by mixing and stirring to obtain the stretching bath.

[0085] The copper source is copper chloride, the sulfiding agent is sodium thiosulfate and sodium sulfate, and the penetrating dispersant is sodium secondary alkyl sulfonate.

[0086] The wet spinning stretching bath is applied to the preparation of conductive acrylic fibers. Specifically, the method for preparing conductive acrylic fibers by wet spinning comprises the following steps:

[0087] 1. Preparation of spinning solution:

[0088] (1) Prepare acrylic fiber spinning solution required for wet spinning and set aside;

[0089] 2. Obtaining primary fiber:

[0090] (2) the acrylic fiber spinning solution prepared in step (1) is accurately metered by a metering pump and ejected from a spinneret to form a thin stream;

[0091] (3) The thin stream enters the coagulation bath for solidification to form a tow.

[0092] (4) the filament bundle is preheated and stretched in a preheating bath, wherein the preheating bath is a 20% by mass copper source solution, the bath temperature is 65° C., and the copper source in the copper source solution is copper sulfate and / or copper chloride, to obtain wet-spun acrylic primary fibers;

[0093] 3. Conductive modification:

[0094] (5) the spun fibers enter a stretching bath, and are soaked and stretched by the stretching bath liquid for modification. The temperature of the stretching bath liquid is 98° C., and the soaking time is 60 min, thereby obtaining conductive acrylic fibers.

[0095] 4. Post-processing:

[0096] (6) Washing, oiling and drying the conductive acrylic fiber obtained in step (5) to obtain the desired conductive acrylic fiber.

[0097] The performance test results of the conductive acrylic fiber prepared by using the wet spinning stretching bath in the wet spinning process in Example 2 of the present invention are as follows:

[0098] 1. Appearance structure characterization analysis

[0099] like Figure 1 As shown, (a) is a polyacrylonitrile filament without conductive modification, and (b) is a polyacrylonitrile filament with conductive modification. After being modified by the conductive stretching bath of the present invention, the appearance structure of the fiber is compared with the polyacrylonitrile fiber that has not been modified by the conductive stretching bath. The fiber color changes from white to dark green (copper green) with a metallic luster, indicating that after the conductive stretching bath modification of the present invention, the copper element is adsorbed into the fiber to bring about conductive properties and change the fiber color.

[0100] from Figure 2 and Figure 3 Comparing the SEM electron microscope photos of the unmodified and conductively modified fiber surfaces, it can be found that the surface of the unmodified polyacrylonitrile filament is smooth and flat, while the surface of the conductively modified polyacrylonitrile filament has evenly distributed micro-nanoparticles.

[0101] Furthermore, after Figure 4 Elemental analysis of the surface of the polyacrylonitrile filament after conductive modification revealed that the main components of the micro-nanoparticles evenly distributed on the surface were sulfur and copper, indicating that the copper source and sulfur in the conductive stretching bath were successfully adsorbed onto the surface of the polyacrylonitrile filament.

[0102] The above characterization and analysis indicate that the technical route proposed by the present invention is feasible to achieve the conductive properties of the fiber by utilizing the existing wet-spinning polyacrylonitrile fiber process and using a stretching bath to perform conductive modification on the fiber during the fiber stretching and forming stage.

[0103] 2. Mechanical properties

[0104] like Figure 5 As shown, it is a comparison of mechanical performance parameters of polyacrylonitrile filaments before and after modification, wherein the light gray curve is the polyacrylonitrile fiber sample before modification; the dark blue is the polyacrylonitrile fiber sample after modification. The results show that the conductive modification of polyacrylonitrile by the technical route of the present invention is carried out. According to the principle that the orientation degree of the polyacrylonitrile macromolecular chain has not been completed during the drawing process of the primary fiber in the stretching bath, the copper ions and sulfur atoms in the conductive bath are more likely to enter the interior of the primary fiber molecules, and the tensile breaking strength of the obtained conductive polyacrylonitrile fiber is better than that before modification. It can be seen that the present invention avoids the influence of traditional functional additives such as antistatic agents and conductive agents on the mechanical properties of polyacrylonitrile fibers by adding antistatic agents, conductive agents, etc. to the spinning solution, and re-modification after fiberization, etc. through the conductive modification treatment in the wet spinning stretching stage. While giving the fiber antistatic or conductive functionality, it maximizes and improves the high quality of the raw materials. It is an efficient and convenient rapid modification technology.

[0105] 3. Conductive properties

[0106] According to the test, the surface resistance of the conductive polyacrylonitrile filament prepared by the present invention can reach 10 2 ~10 3 Ωcm; the surface resistance of the polyacrylonitrile filaments without conductive modification is very large, and basically no data can be measured. It can be seen that the conductive polyacrylonitrile filaments modified by stretching of the present invention have excellent conductive properties.

[0107] 4. Washability

[0108] like Figure 6As shown, in order to determine the stability and washing durability of the conductive layer on the surface of the conductive polyacrylonitrile fiber, we conducted a washing test. The washing test conditions refer to the AATCC 61 test standard, the washing temperature is 40°C, the standard washing liquid content is 0.37%, the washing time is 45 minutes, and then the fiber is taken out to dry and the resistance is measured. Six tests were carried out, and the surface resistance was tested after washing. It was found that the surface resistance of the fiber was still maintained at the same order of magnitude, which shows that the conductive modification treatment method described in the present invention performs conductive modification on the fiber during the stretching process, and copper ions and sulfur atoms are more likely to enter the interior of the primary fiber molecules, which is beneficial to the improvement of the conductive performance. Through the conductive modification treatment in the wet spinning stretching stage, the coordination and complexation of the coordinated metal ions and the polyacrylonitrile macromolecules is utilized to solve the problem of poor durability of conventional surface modification.

[0109] In summary, in order to ensure the quality of the polyacrylonitrile fiber after spinning, the present invention does not add any antistatic agent, conductive agent or conductive material and auxiliary agent in the spinning solution stage, thereby avoiding the dispersion and agglomeration problems caused by their addition, as well as the influence of uneven distribution on the quality of acrylic fiber; at the same time, the existing wet-spinning polyacrylonitrile fiber technology route is used, and the fiber is modified for conductivity by using a stretching bath in the fiber stretching and forming stage, which does not affect the intrinsic properties of the fiber and increases its conductivity or antistatic properties. It has obvious social value and economic benefits, and gives it conductive properties in the process of preparing acrylic fiber, greatly reducing production costs, and is suitable for industrial applications.

[0110] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention should fall within the protection scope of the present invention.

Claims

1. A stretching bath for wet spinning, characterized in that: It is composed of the following raw materials in parts by weight:

2. The stretching bath for wet spinning according to claim 1, characterized in that: The copper source is copper sulfate and / or copper chloride.

3. The wet spinning stretching bath according to claim 1, characterized in that: The vulcanizing agent is any one or more of sodium thiosulfate and sodium sulfate.

4. The stretching bath for wet spinning according to claim 1, characterized in that: The penetrating dispersant is any one or more of fatty alcohol polyoxyethylene ether, octyl phosphate, ethylene oxide, and sodium secondary alkyl sulfonate.

5. A method for preparing the wet spinning stretching bath according to any one of claims 1 to 4, characterized in that: The copper source, the sulfiding agent and the infiltration dispersant are respectively dissolved in deionized water according to the weight parts, and dispersed evenly by mixing and stirring to obtain the product.

6. Use of the wet spinning stretching bath according to any one of claims 1 to 4 in the preparation of conductive acrylic fibers.

7. A method for preparing conductive acrylic fiber by wet spinning, characterized in that: The steps include:

1. Preparation of spinning solution: (1) Prepare acrylic fiber spinning solution required for wet spinning and set aside; 2. Obtaining primary fiber: (2) the acrylic fiber spinning solution prepared in step (1) is accurately metered by a metering pump and ejected from a spinneret to form a thin stream; (3) The thin stream enters the coagulation bath for solidification to form a tow. (4) the filament bundle is preheated and stretched in a preheating bath to obtain wet-spun acrylic primary fibers; 3. Conductive modification: (5) the spun fibers enter a stretching bath, and the spun fibers are soaked and stretched by the stretching bath to obtain conductive acrylic fibers; 4. Post-processing: (6) Washing, oiling and drying the conductive acrylic fiber obtained in step (5) to obtain the desired conductive acrylic fiber.

8. The method for preparing conductive acrylic fiber by wet spinning according to claim 7, characterized in that: In the step (4), the preheating bath is a copper source solution with a mass fraction of 5-20%, and the bath temperature is 60-65°C.

9. The method for preparing conductive acrylic fiber by wet spinning according to claim 7, characterized in that: In the step (5), the temperature of the stretching bath is 90-98° C., and the immersion time is 15-60 min.

10. The method for preparing conductive acrylic fiber by wet spinning according to claim 8, characterized in that: In the copper source solution, the copper source is copper sulfate and / or copper chloride.

Citation Information

Patent Citations

  • Conductive spinning solution, preparation method and application of conductive spinning solution to preparation of conductive acrylic fibers

    CN111088528A

  • Method for modifying orlon

    CN101603270A

  • Electrically conductive fiber and production method thereof

    JP2010144306A

  • Method of making electrically conducting fibers

    US4336028A

  • Method of making electrically conducting fiber

    US4364739A