High-waterproofness fabric
By introducing micro-nano structured fillers and nano zinc oxide modification into textiles, combined with the cross-linking reaction of dihydroxycoumarin derivatives, a highly waterproof coating is constructed, solving the problem of insufficient waterproof performance of waterproof and breathable textiles and achieving high waterproof and breathable properties as well as UV resistance in the fabric.
Patent Information
- Application Number
- CN202410937167.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
Existing waterproof and breathable textiles have insufficient waterproof performance and moisture absorption, resulting in generally poor waterproof and breathable effects.
The structure consists of a waterproof and breathable membrane, a base fabric, and a highly waterproof coating, arranged from the inside out. The coating contains micro-nano structure fillers, tackifying fluorinated modified polyvinyl alcohol, and dihydroxycoumarin derivatives. The hydrophobic properties are improved by constructing a low surface energy rough surface and cross-linking reaction, and the fiber stability is enhanced by nano zinc oxide modification treatment.
It significantly improves the waterproof and breathable properties and UV resistance of the fabric, and the strong adhesion between the coating and the base fabric enhances the stability and hydrophobic properties of the fabric.
Smart Images

Figure BDA0004941684710000101 
Figure BDA0004941684710000111
Abstract
Description
Technical Field
[0001] The present application relates to the field of fabrics, and in particular to a highly waterproof fabric. Background Art
[0002] With the development of science and technology, social progress and improvement of living standards, people's requirements for quality of life are gradually increasing. The functions of textiles have been extended from covering the body to keeping warm to beauty, comfort, fashion and protection. People's consumption concepts have also gradually developed from practicality to health care, environmental protection and multi-function. Various intelligent and functional textiles have received widespread attention, and waterproof and breathable textiles are one of them.
[0003] Waterproof and breathable laminated fabric is formed by laminating a waterproof and breathable membrane with a base fabric. Lamination is a method of applying a layer of adhesive on the base fabric, covering it with a film or other material, and heating and pressurizing it to form a two-layer or more composite fabric. The base fabric layer usually uses a fabric with certain water-repellent properties, but its water-repellent effect is limited, and its own hygroscopicity will increase the wet weight of the fabric, resulting in the fabric's average waterproof and breathable performance, so it needs to be improved. Summary of the invention
[0004] In order to improve the waterproof performance of fabrics, the present application provides a highly waterproof fabric.
[0005] The highly waterproof fabric provided in this application adopts the following technical solution: A highly waterproof fabric, the highly waterproof fabric comprising a waterproof and breathable membrane, a base fabric and a highly waterproof coating arranged in sequence from the inside to the outside, the highly waterproof coating being obtained by coating the highly waterproof coating on a side of the base fabric away from the waterproof and breathable membrane, the highly waterproof coating comprising the following components in parts by mass: 5-10 parts of micro-nano structure filler 4-6 parts of dihydroxycoumarin derivatives 20-30 parts of fluorinated modified polyvinyl alcohol Solvent 100-120 parts.
[0006] Micro-nano structured fillers have micro-nano rough structures. Introducing them into highly waterproof coatings can help construct a rough surface with low surface energy and improve the hydrophobic properties of highly waterproof coatings. Dihydroxycoumarin derivatives can undergo cross-linking reactions with thickening fluorinated modified polyvinyl alcohol. The coumarin groups can undergo dimerization and depolymerization, dissipating the energy of ultraviolet light, giving the coating certain self-healing properties and improving the stability and UV resistance of the highly waterproof coating. Thickening fluorinated modified polyvinyl alcohol has good hydrophobic and adhesion properties, allowing the highly waterproof coating to be firmly bonded to the base fabric, thereby improving the stability and hydrophobic properties of the highly waterproof fabric.
[0007] Preferably, the micro-nano structure filler comprises titanium dioxide nanorods, aluminum oxide nanosheets and a hydrophobic modifier.
[0008] Titanium dioxide nanorods have a rod-like structure, can construct a rough microscopic surface, and have super hydrophobic properties; aluminum oxide nanosheets have high hardness and wear resistance, which can improve the stability and durability of the coating; hydrophobic modifiers modify inorganic fillers to further improve the hydrophobic properties of micro-nanostructure fillers.
[0009] Preferably, the aluminum oxide nanosheets are attached to the surface of the titanium dioxide nanorods to obtain aluminum oxide-attached titanium dioxide, and the raw materials for preparing the aluminum oxide nanosheets include aluminum chloride hexahydrate, polyethylene glycol and carbonamide.
[0010] By hydrothermal reaction of aluminum chloride hexahydrate, polyethylene glycol, carbonamide and titanium dioxide nanorods, aluminum oxide is attached to the surface of titanium dioxide nanorods in a flaky structure, which can further construct a micro-nano structure and improve the hydrophobic property. Aluminum oxide attached to titanium dioxide combines the advantages of aluminum oxide and titanium dioxide, can better absorb and shield ultraviolet rays, and synergize with dihydroxycoumarin derivatives to improve anti-ultraviolet performance.
[0011] Preferably, the mass ratio of aluminum chloride hexahydrate, polyethylene glycol and carbonamide is (0.4-0.6):0.08:1.
[0012] The aluminum oxide nanosheets prepared according to the above mass ratio have good morphology and structure, and can be uniformly attached to the surface of the titanium dioxide nanorods.
[0013] Preferably, the raw materials for preparing the hydrophobic modifier include isocyanatepropyltriethoxysilane and perfluoroalkylethyl acrylate.
[0014] The isocyanate group in isocyanatepropyltriethoxysilane can react with the hydroxyl group in perfluoroalkylethyl acrylate. The modifier obtained by the condensation reaction of the two further grafts the titanium dioxide attached to the alumina, reduces the hydroxyl groups on the surface of the titanium dioxide attached to the alumina, and further improves its hydrophobic properties and system compatibility.
[0015] Preferably, the raw materials for preparing the thickened fluorinated modified polyvinyl alcohol include polyvinyl alcohol, trifluorobenzaldehyde and tannic acid.
[0016] Trifluorobenzaldehyde is used as a hydrophobic monomer to perform hydrophobic modification on polyvinyl alcohol. The introduction of hydrophobic phenyl groups and fluorine atoms into polyvinyl alcohol can improve the hydrophobic properties of polyvinyl alcohol. Tannic acid has a catechol structure and can be firmly adsorbed on the surface of the fabric through hydrogen bonds and electrostatic effects. The use of tannic acid to modify highly hydrophobic coatings can improve the bonding strength between the coating and the fabric. Tannic acid can also capture and quench free radicals, absorb ultraviolet rays, and improve the UV resistance of the coating. It synergizes with micro-nanostructured fillers and dihydroxycoumarin derivatives to effectively improve the UV resistance of the coating through the synergistic effect of absorbing reflected ultraviolet rays, dissipating ultraviolet energy, and quenching free radicals generated by ultraviolet rays.
[0017] Preferably, the base fabric is obtained by blending viscose fiber and nylon fiber.
[0018] The base fabric obtained by blending viscose fiber and nylon fiber has good waterproof and breathable properties. Nylon fiber has good water-repellent properties, and viscose fiber can promote the transport of water vapor out of the fabric. After contacting water vapor, the viscose fiber expands and blocks the pores between fibers, preventing external water vapor from entering, thereby achieving good waterproof and moisture permeability effects.
[0019] Preferably, the waterproof and breathable membrane is obtained by electrostatic spinning, and the waterproof and breathable membrane comprises polyacrylonitrile and polyurethane, and the polyurethane is chain-extended and modified by modified nano zinc oxide.
[0020] The waterproof and breathable membrane obtained by electrospinning polyacrylonitrile and polyurethane has a good three-dimensional network structure, which is conducive to the passage of water vapor and gas molecules, prevents the penetration of moisture, and has good waterproof and breathable properties; by modifying the polyurethane with modified nano zinc oxide, nano zinc oxide particles can be introduced into the polyurethane, so that the fibers of the waterproof and breathable membrane have a rough surface structure, further improving its hydrophobic properties, thereby improving the waterproof properties of the fabric.
[0021] Preferably, the modified nano zinc oxide is prepared by the following steps: Nano zinc oxide and 3-chloropropyltrimethoxysilane were mixed and dispersed in toluene, deionized water was added after stirring, and 1,8-octanediamine was added after stirring in a water bath to react, and stirring in a water bath to react was continued, and the obtained product solution was filtered to obtain a filtrate, and the filtrate was washed with anhydrous ethanol, and the washed filtrate was dried in an oven at 80°C for 6 hours to obtain modified nano zinc oxide.
[0022] Nano zinc oxide is modified by 3-chloropropyltrimethoxysilane and 1,8-octanediamine, and long amino chains are grafted on the surface. The modified nano zinc oxide has good reactivity and system compatibility. It can be used for chain extension modification of polyurethane, improve the stability of spun fibers, promote the formation of rough micro-nano structures on the fiber surface, and thus improve the waterproof and moisture permeability of nanofiber membranes.
[0023] Preferably, the highly waterproof fabric is prepared by the following steps: The viscose fiber and the nylon fiber are blended to obtain a base fabric; an adhesive is coated on the base fabric, a waterproof and breathable membrane is compounded to the side of the base fabric coated with the adhesive, and the fabric is dried and baked to obtain a fabric with a waterproof and breathable membrane; a highly waterproof coating is coated on the side of the fabric with the waterproof and breathable membrane away from the waterproof and breathable membrane to obtain a fabric with a highly waterproof coating, the fabric with the highly waterproof coating is dried and baked to obtain a semi-finished product, and the semi-finished product is washed with water and then air-dried to obtain a highly waterproof fabric.
[0024] The fabric prepared according to the above steps has good waterproof and moisture permeability and UV resistance.
[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. Micro-nano structure fillers have micro-nano rough structures. Introducing them into high waterproof coatings can help construct a rough surface with low surface energy and improve the hydrophobic properties of high waterproof coatings; dihydroxycoumarin derivatives can undergo cross-linking reactions with thickening fluorinated modified polyvinyl alcohol, and the coumarin groups can undergo dimerization and depolymerization, dissipating the energy of ultraviolet light, so that the coating has certain self-healing properties and improves the stability and UV resistance of the high waterproof coating; thickening fluorinated modified polyvinyl alcohol has good hydrophobic and adhesion properties, so that the high waterproof coating can be firmly combined with the base fabric, thereby improving the stability and hydrophobic properties of the high waterproof fabric.
[0026] 2. The synergistic effect of micro-nano structure fillers, dihydroxycoumarin derivatives and tannic acid can effectively improve the anti-ultraviolet performance of the coating through the synergistic effect of absorbing and reflecting ultraviolet rays, dissipating ultraviolet energy and quenching free radicals generated by ultraviolet rays.
[0027] 3. Nano zinc oxide is modified by 3-chloropropyltrimethoxysilane and 1,8-octanediamine, and long amino chains are grafted on the surface. The modified nano zinc oxide has good reactivity and system compatibility. It can be used for chain extension modification of polyurethane, improve the stability of spun fibers, promote the formation of rough micro-nano structures on the fiber surface, and thus improve the waterproof and moisture permeability of nanofiber membranes. DETAILED DESCRIPTION
[0028] The present application discloses a highly waterproof fabric. The raw materials used in the present application can be obtained from commercially available raw materials unless otherwise specified. The present application is further described in detail below in conjunction with the embodiments: Raw materials description: Titanium dioxide nanorods were purchased from Bohuasi Nanotechnology (Ningbo) Co., Ltd., aluminum chloride hexahydrate (CAS No.: 7784-13-6), polyethylene glycol (CAS No.: 25322-68-3), carbonamide (CAS No.: 57-13-6), isocyanate propyl triethoxysilane (CAS No.: 4801-88-5), catalyst is triethylamine (CAS No.: 121-44-8), perfluoroalkyl ethyl acrylate (CAS No.: 65605-70-1), polyvinyl alcohol (CAS No.: 9002-89-5), dimethyl sulfoxide (CAS No.: 67-68-5), p-toluenesulfonic acid (CAS No.: 104-15-4), trifluorobenzaldehyde (CAS No.: 58551-83-0), tannic acid (CAS No.: 1401-55-4), dihydroxycoumarin derivative The raw material is 7,8-dihydroxy-4-phenylcoumarin (CAS No.: 842-01-3), nano zinc oxide was purchased from Haichuang Zinc Technology, 3-chloropropyltrimethoxysilane (CAS No.: 2530-87-2), 1,8-octanediamine (CAS No.: 373-44-4), polyether diol (CAS No.: 9003-11-6), molecular weight is 2000, diphenylmethane diisocyanate (CAS No.: 101-68-6), dibutyltin dilaurate (CAS No.: 77-58-7), the end-capping agent is hydroxyethyl acrylate (CAS No.: 818-61-1), polyacrylonitrile (CAS No.: 25014-41-9), molecular weight is 150000, perfluorodecyltrimethoxysilane (CAS No.: 83048-65-1), and the adhesive was purchased from Dongguan Jiurui Plastic Raw Materials Co., Ltd.
[0029] Example 1 Preparation of micro-nanostructured fillers 20g of titanium dioxide nanorods were ultrasonically washed three times with ethanol, filtered and dried in an oven at 80°C for 6h to obtain washed titanium dioxide nanorods. 15g of washed titanium dioxide nanorods, 2.7g of aluminum chloride hexahydrate, 0.54g of polyethylene glycol and 6.76g of carbonamide were mixed and dispersed in 100mL of 50% ethanol aqueous solution to obtain a mixed dispersion, the mixed dispersion was stirred at a speed of 200rpm for 30min, and then ultrasonicated for 15min, the ultrasonicated mixed dispersion was transferred to a hydrothermal reactor, heated from room temperature to 160°C in the hydrothermal reactor for 2h, and after the hydrothermal reactor was cooled to below 30°C, filtered to obtain a solid product, the solid product was washed three times with deionized water and ethanol respectively, the washed solid product was dried in an oven at 60°C for 8h, the dried solid product was calcined in a nitrogen atmosphere at 600°C for 4h, the calcined solid product was ground and passed through a 1000 mesh sieve to obtain alumina-attached titanium dioxide.
[0030] 10g of isocyanate propyl triethoxysilane and 2mL of catalyst were mixed and dispersed in 100mL of xylene to obtain a silane dispersion, and after heating to 150°C, 3mL of perfluoroalkylethyl acrylate was added to the silane dispersion, stirred at a speed of 200rpm, kept at 150°C for reflux reaction for 8h, and then cooled to 30°C and rotary evaporated to obtain a hydrophobic modifier. 6g of hydrophobic modifier and 10g of alumina-attached titanium dioxide were dispersed in 50mL of xylene to obtain a modified solution, and the modified solution was stirred at a speed of 200rpm, refluxed at 150°C for 6h, and filtered to obtain a precipitate after cooling to 30°C. The precipitate was washed three times with anhydrous ethanol and dried in a blast drying oven at 80°C for 10h to obtain a micro-nano structure filler.
[0031] Preparation of fluorinated polyvinyl alcohol with enhanced viscosity Disperse 50g of polyvinyl alcohol in dimethyl sulfoxide, stir at 200rpm in a 90℃ water bath until completely dissolved to obtain a polyvinyl alcohol solution, add 7.2g of p-toluenesulfonic acid and 12g of trifluorobenzaldehyde to the polyvinyl alcohol solution, stir and react at 200rpm in an 80℃ water bath for 6h, and obtain fluorinated modified polyvinyl alcohol after cooling to below 30℃. Solvent replace the fluorinated modified polyvinyl alcohol in ethanol for 12h to obtain replaced fluorinated polyvinyl alcohol, add 5g of tannic acid to the replaced fluorinated polyvinyl alcohol, stir and react at 200rpm for 1h to obtain a modified polyvinyl alcohol solution, and dry the modified polyvinyl alcohol solution in an oven at 60℃ for 10h to obtain thickened fluorinated modified polyvinyl alcohol.
[0032] Preparation of highly water-resistant coatings 5 g of micro-nano structure filler, 4 g of dihydroxycoumarin derivative, 20 g of thickening fluorinated modified polyvinyl alcohol and 100 g of solvent are mixed to obtain a mixed solution, wherein the solvent is deionized water, and the mixed solution is stirred and reacted for 2 hours in a 60° C. water bath at a speed of 200 rpm under ultraviolet light to obtain a highly waterproof coating.
[0033] Preparation of waterproof and breathable membrane 30 g of nano zinc oxide and 15 g of 3-chloropropyltrimethoxysilane were dispersed in 200 mL of toluene, stirred at 200 rpm for 2 h, then 1.2 mL of deionized water was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., 20 g of 1,8-octanediamine was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., the product solution was filtered to obtain a filtrate, the filtrate was washed with anhydrous ethanol, and the washed filtrate was dried in an oven at 80 ° C. for 6 h to obtain modified nano zinc oxide.
[0034] 200 g of polyether diol, 120 g of diphenylmethane diisocyanate and 2 g of dibutyltin dilaurate were mixed to obtain a reaction system. The reaction system was reacted for 1 hour under a nitrogen atmosphere, an 80° C. water bath and stirring at 200 rpm, and then the temperature was lowered to 30° C. A modified zinc oxide acetone dispersion containing 25 g of modified zinc oxide was added to the reaction system. The reaction was continued for 1 hour under a nitrogen atmosphere, an 80° C. water bath and stirring at 200 rpm. 15 g of a capping agent was added, the temperature was raised to 40° C. and the reaction was continued for 1 hour. The reaction system was rotary evaporated to obtain a polyurethane.
[0035] 200g of polyurethane and 200g of polyacrylonitrile were dispersed in 2L of N,N-dimethylformamide, and stirred at a speed of 200rpm until completely dissolved to obtain a mixed spinning solution. The mixed spinning solution was subjected to electrospinning at a spinning voltage of 50kV, a receiving distance of 18cm, and a drum speed of 70r / min to obtain a fiber membrane. The fiber membrane was dried in an oven at 50°C for 0.5h to obtain a waterproof and moisture-permeable membrane.
[0036] Preparation of highly water-resistant fabrics Viscose fiber and nylon fiber are blended to obtain a base fabric; an adhesive is coated on the base fabric, a waterproof and breathable membrane is compounded to the side of the base fabric coated with the adhesive, the fabric is dried in an oven at 80°C, and baked at 140°C for 2 minutes to obtain a fabric with a waterproof and breathable membrane; a highly waterproof coating is coated on the side of the fabric with the waterproof and breathable membrane away from the waterproof and breathable membrane to obtain a fabric with a highly waterproof coating, the fabric with the highly waterproof coating is dried in an oven at 80°C, and baked at 150°C for 1.5 minutes to obtain a semi-finished product, the semi-finished product is washed with water and then air-dried to obtain a highly waterproof fabric.
[0037] Example 2 Preparation of micro-nanostructured fillers 20g of titanium dioxide nanorods were ultrasonically washed three times with ethanol, filtered and dried in an oven at 80°C for 6h to obtain washed titanium dioxide nanorods. 15g of washed titanium dioxide nanorods, 3.57g of aluminum chloride hexahydrate, 0.48g of polyethylene glycol and 5.95g of carbonamide were mixed and dispersed in 100mL of 50% ethanol aqueous solution to obtain a mixed dispersion, the mixed dispersion was stirred at a speed of 200rpm for 30min, and then ultrasonicated for 15min, the ultrasonicated mixed dispersion was transferred to a hydrothermal reactor, heated from room temperature to 160°C in the hydrothermal reactor for 2h, and after the hydrothermal reactor was cooled to below 30°C, filtered to obtain a solid product, the solid product was washed three times with deionized water and ethanol respectively, the washed solid product was dried in an oven at 60°C for 8h, the dried solid product was calcined in a nitrogen atmosphere at 600°C for 4h, the calcined solid product was ground and passed through a 1000 mesh sieve to obtain alumina-attached titanium dioxide.
[0038] 10g of isocyanate propyl triethoxysilane and 2mL of catalyst were mixed and dispersed in 100mL of xylene to obtain a silane dispersion, and after heating to 150°C, 3mL of perfluoroalkylethyl acrylate was added to the silane dispersion, stirred at a speed of 200rpm, kept at 150°C for reflux reaction for 8h, and then cooled to 30°C and rotary evaporated to obtain a hydrophobic modifier. 6g of hydrophobic modifier and 10g of alumina-attached titanium dioxide were dispersed in 50mL of xylene to obtain a modified solution, and the modified solution was stirred at a speed of 200rpm, refluxed at 150°C for 6h, and filtered to obtain a precipitate after cooling to 30°C. The precipitate was washed three times with anhydrous ethanol and dried in a blast drying oven at 80°C for 10h to obtain a micro-nano structure filler.
[0039] Preparation of fluorinated polyvinyl alcohol with enhanced viscosity Disperse 50g of polyvinyl alcohol in dimethyl sulfoxide, stir at 200rpm in a 90℃ water bath until completely dissolved to obtain a polyvinyl alcohol solution, add 7.2g of p-toluenesulfonic acid and 12g of trifluorobenzaldehyde to the polyvinyl alcohol solution, stir and react at 200rpm in an 80℃ water bath for 6h, and obtain fluorinated modified polyvinyl alcohol after cooling to below 30℃. Solvent replace the fluorinated modified polyvinyl alcohol in ethanol for 12h to obtain replaced fluorinated polyvinyl alcohol, add 5g of tannic acid to the replaced fluorinated polyvinyl alcohol, stir and react at 200rpm for 1h to obtain a modified polyvinyl alcohol solution, and dry the modified polyvinyl alcohol solution in an oven at 60℃ for 10h to obtain thickened fluorinated modified polyvinyl alcohol.
[0040] Preparation of highly water-resistant coatings 10 g of micro-nano structure filler, 6 g of dihydroxycoumarin derivative, 30 g of thickening fluorinated modified polyvinyl alcohol and 120 g of solvent were mixed to obtain a mixed solution, wherein the solvent was deionized water, and the mixed solution was stirred and reacted for 1 hour in a 60° C. water bath at a speed of 200 rpm under ultraviolet light to obtain a highly waterproof coating.
[0041] Preparation of waterproof and breathable membrane 30 g of nano zinc oxide and 15 g of 3-chloropropyltrimethoxysilane were dispersed in 200 mL of toluene, stirred at 200 rpm for 2 h, then 1.2 mL of deionized water was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., 20 g of 1,8-octanediamine was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., the product solution was filtered to obtain a filtrate, the filtrate was washed with anhydrous ethanol, and the washed filtrate was dried in an oven at 80 ° C. for 6 h to obtain modified nano zinc oxide.
[0042] 200 g of polyether diol, 120 g of diphenylmethane diisocyanate and 2 g of dibutyltin dilaurate were mixed to obtain a reaction system. The reaction system was reacted for 1 hour under a nitrogen atmosphere, an 80° C. water bath and stirring at 200 rpm, and then the temperature was lowered to 30° C. A modified zinc oxide acetone dispersion containing 25 g of modified zinc oxide was added to the reaction system. The reaction was continued for 1 hour under a nitrogen atmosphere, an 80° C. water bath and stirring at 200 rpm. 15 g of a capping agent was added, the temperature was raised to 40° C. and the reaction was continued for 1 hour. The reaction system was rotary evaporated to obtain a polyurethane.
[0043] 200g of polyurethane and 200g of polyacrylonitrile were dispersed in 2L of N,N-dimethylformamide, and stirred at a speed of 200rpm until completely dissolved to obtain a mixed spinning solution. The mixed spinning solution was subjected to electrospinning at a spinning voltage of 50kV, a receiving distance of 18cm, and a drum speed of 70r / min to obtain a fiber membrane. The fiber membrane was dried in an oven at 50°C for 0.5h to obtain a waterproof and moisture-permeable membrane.
[0044] Preparation of highly water-resistant fabrics Viscose fiber and nylon fiber are blended to obtain a base fabric; an adhesive is coated on the base fabric, a waterproof and breathable membrane is compounded to the side of the base fabric coated with the adhesive, the fabric is dried in an oven at 80°C, and baked at 140°C for 2 minutes to obtain a fabric with a waterproof and breathable membrane; a highly waterproof coating is coated on the side of the fabric with the waterproof and breathable membrane away from the waterproof and breathable membrane to obtain a fabric with a highly waterproof coating, the fabric with the highly waterproof coating is dried in an oven at 80°C, and baked at 150°C for 1.5 minutes to obtain a semi-finished product, the semi-finished product is washed with water and then air-dried to obtain a highly waterproof fabric.
[0045] Example 3 Preparation of micro-nanostructured fillers 20g of titanium dioxide nanorods were ultrasonically washed three times with ethanol, filtered and dried in an oven at 80°C for 6h to obtain washed titanium dioxide nanorods. 15g of washed titanium dioxide nanorods, 3.16g of aluminum chloride hexahydrate, 0.51g of polyethylene glycol and 6.33g of carbonamide were mixed and dispersed in 100mL of 50% ethanol aqueous solution to obtain a mixed dispersion, the mixed dispersion was stirred at a speed of 200rpm for 30min, and then ultrasonicated for 15min, the ultrasonicated mixed dispersion was transferred to a hydrothermal reactor, heated from room temperature to 160°C in the hydrothermal reactor for 2h, and after the hydrothermal reactor was cooled to below 30°C, filtered to obtain a solid product, the solid product was washed three times with deionized water and ethanol respectively, the washed solid product was dried in an oven at 60°C for 8h, the dried solid product was calcined in a nitrogen atmosphere at 600°C for 4h, the calcined solid product was ground and passed through a 1000 mesh sieve to obtain alumina-attached titanium dioxide.
[0046] 10g of isocyanate propyl triethoxysilane and 2mL of catalyst were mixed and dispersed in 100mL of xylene to obtain a silane dispersion, and after heating to 150°C, 3mL of perfluoroalkylethyl acrylate was added to the silane dispersion, stirred at a speed of 200rpm, kept at 150°C for reflux reaction for 8h, and then cooled to 30°C and rotary evaporated to obtain a hydrophobic modifier. 6g of hydrophobic modifier and 10g of alumina-attached titanium dioxide were dispersed in 50mL of xylene to obtain a modified solution, and the modified solution was stirred at a speed of 200rpm, refluxed at 150°C for 6h, and filtered to obtain a precipitate after cooling to 30°C. The precipitate was washed three times with anhydrous ethanol and dried in a blast drying oven at 80°C for 10h to obtain a micro-nano structure filler.
[0047] Preparation of fluorinated polyvinyl alcohol with enhanced viscosity Disperse 50g of polyvinyl alcohol in dimethyl sulfoxide, stir at 200rpm in a 90℃ water bath until completely dissolved to obtain a polyvinyl alcohol solution, add 7.2g of p-toluenesulfonic acid and 12g of trifluorobenzaldehyde to the polyvinyl alcohol solution, stir and react at 200rpm in an 80℃ water bath for 6h, and obtain fluorinated modified polyvinyl alcohol after cooling to below 30℃. Solvent replace the fluorinated modified polyvinyl alcohol in ethanol for 12h to obtain replaced fluorinated polyvinyl alcohol, add 5g of tannic acid to the replaced fluorinated polyvinyl alcohol, stir and react at 200rpm for 1h to obtain a modified polyvinyl alcohol solution, and dry the modified polyvinyl alcohol solution in an oven at 60℃ for 10h to obtain thickened fluorinated modified polyvinyl alcohol.
[0048] Preparation of highly water-resistant coatings 7.5 g of micro-nano structure filler, 5 g of dihydroxycoumarin derivative, 25 g of thickening fluorinated modified polyvinyl alcohol and 110 g of solvent were mixed to obtain a mixed solution, wherein the solvent was deionized water, and the mixed solution was stirred and reacted for 1 hour in a 60° C. water bath at a speed of 200 rpm under ultraviolet light to obtain a highly waterproof coating.
[0049] Preparation of waterproof and breathable membrane 30 g of nano zinc oxide and 15 g of 3-chloropropyltrimethoxysilane were dispersed in 200 mL of toluene, stirred at 200 rpm for 2 h, then 1.2 mL of deionized water was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., 20 g of 1,8-octanediamine was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., the product solution was filtered to obtain a filtrate, the filtrate was washed with anhydrous ethanol, and the washed filtrate was dried in an oven at 80 ° C. for 6 h to obtain modified nano zinc oxide.
[0050] 200 g of polyether diol, 120 g of diphenylmethane diisocyanate and 2 g of dibutyltin dilaurate were mixed to obtain a reaction system. The reaction system was reacted for 1 hour under a nitrogen atmosphere, an 80° C. water bath and stirring at 200 rpm, and then the temperature was lowered to 30° C. A modified zinc oxide acetone dispersion containing 25 g of modified zinc oxide was added to the reaction system. The reaction was continued for 1 hour under a nitrogen atmosphere, an 80° C. water bath and stirring at 200 rpm. 15 g of a capping agent was added, the temperature was raised to 40° C. and the reaction was continued for 1 hour. The reaction system was rotary evaporated to obtain a polyurethane.
[0051] 200g of polyurethane and 200g of polyacrylonitrile were dispersed in 2L of N,N-dimethylformamide, and stirred at a speed of 200rpm until completely dissolved to obtain a mixed spinning solution. The mixed spinning solution was subjected to electrospinning at a spinning voltage of 50kV, a receiving distance of 18cm, and a drum speed of 70r / min to obtain a fiber membrane. The fiber membrane was dried in an oven at 50°C for 0.5h to obtain a waterproof and moisture-permeable membrane.
[0052] Preparation of highly water-resistant fabrics Viscose fiber and nylon fiber are blended to obtain a base fabric; an adhesive is coated on the base fabric, a waterproof and breathable membrane is compounded to the side of the base fabric coated with the adhesive, the fabric is dried in an oven at 80°C, and baked at 140°C for 2 minutes to obtain a fabric with a waterproof and breathable membrane; a highly waterproof coating is coated on the side of the fabric with the waterproof and breathable membrane away from the waterproof and breathable membrane to obtain a fabric with a highly waterproof coating, the fabric with the highly waterproof coating is dried in an oven at 80°C, and baked at 150°C for 1.5 minutes to obtain a semi-finished product, the semi-finished product is washed with water and then air-dried to obtain a highly waterproof fabric.
[0053] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that in Example 4, the amount of aluminum chloride hexahydrate is 2.17 g, the amount of polyethylene glycol is 0.58 g, and the amount of carbonamide is 7.25 g.
[0054] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, the amount of aluminum chloride hexahydrate used is 3.93 g, the amount of polyethylene glycol used is 0.45 g, and the amount of carbonamide used is 5.62 g.
[0055] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that in Example 6, the alumina-coated titanium dioxide in the step of preparing the micro-nanostructure filler is replaced by nano-alumina and nano-titania, and the mass ratio of nano-alumina to nano-titania is 0.2:1.
[0056] Example 7 Example 7 is based on Example 3. The only difference between Example 7 and Example 3 is that in Example 7, the hydrophobic modifier in the step of preparing the micro-nanostructure filler is replaced by perfluorodecyltrimethoxysilane.
[0057] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that in Example 8, trifluorobenzaldehyde is not added in the step of preparing the thickened fluorinated modified polyvinyl alcohol.
[0058] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that in Example 9, tannic acid is not added in the step of preparing the thickened fluorinated modified polyvinyl alcohol.
[0059] Example 10 Example 10 is based on Example 3, and the only difference between Example 10 and Example 3 is that the base fabric is replaced with nylon fabric in Example 10.
[0060] Embodiment 11 Example 11 is based on Example 3. The only difference between Example 11 and Example 3 is that in Example 11, the modified nano zinc oxide in the step of preparing the waterproof and moisture-permeable membrane is replaced by nano zinc oxide.
[0061] Example 12 Example 12 is based on Example 3. The only difference between Example 12 and Example 3 is that in Example 12, modified nano zinc oxide is not added in the step of preparing the waterproof and breathable membrane.
[0062] Comparative Example 1 Comparative Example 1 is based on Example 3, and the only difference between Comparative Example 1 and Example 3 is that the micro-nano structure filler in Comparative Example 1 is replaced by titanium dioxide nanorods.
[0063] Comparative Example 2 Comparative Example 2 is based on Example 3, and the only difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, the viscosity-enhancing fluorinated modified polyvinyl alcohol is replaced by polyvinyl alcohol.
[0064] Comparative Example 3 Comparative Example 3 is based on Example 3, and the only difference between Comparative Example 3 and Example 3 is that no dihydroxycoumarin derivative is added in Comparative Example 3.
[0065] Performance testing (1) Select GB / T4744-2013 Testing and Evaluation of Waterproof Performance of Textiles - Hydrostatic Pressure Method as the standard, cut five 10 cm × 10 cm specimens from the fabric, record the pressure value when the third water seepage point appears, test each specimen three times, take the average value after measurement, and fill in the measurement results in Table 1.
[0066] (2) Select "GB / T12704.2-2009 Test method for water vapor permeability of textile fabrics Part 2: Evaporation method" as the standard, cut three samples with a diameter of 70 cm from the fabric, and calculate the water vapor permeability of the samples by the inverted cup method under the conditions of temperature 38°C and humidity 50%. After measurement, take the average value of the three samples and fill in the measurement results in Table 1.
[0067] (3) Select GB / T18830-2009 Evaluation of UV protection performance of textiles as the standard, cut four 10 cm × 10 cm samples from the fabric, record the transmittance between 290 nm and 400 nm, record once every five minutes, calculate the UPF value and UVA transmittance, and record the results in Table 1.
[0068] Table 1 Test results of waterproof and moisture permeability and UV resistance of highly waterproof fabrics As shown in Table 1, the hydrostatic pressure resistance of Examples 1-3 is greater than 153.6 KPa, and the water vapor permeability is greater than 9087 g / (m 2 ·24h), the UPF value is greater than 46.7, and the UVA transmittance is less than 0.44%, which shows that the highly waterproof fabric prepared in the present application has good waterproof and moisture permeability and UV resistance.
[0069] As can be seen from Table 1, the only difference between Examples 4 and 5 and Example 3 is that the mass ratio of aluminum chloride hexahydrate, polyethylene glycol and carbon amide in Example 4 is 0.3:0.08:1, and the mass ratio of aluminum chloride hexahydrate, polyethylene glycol and carbon amide in Example 5 is 0.7:0.08:1. Compared with Example 3, the waterproof and moisture permeability and anti-ultraviolet performance of Examples 4 and 5 are reduced. This is because the mass ratio of aluminum chloride hexahydrate, polyethylene glycol and carbon amide is not within the limited range. When it is not within the optimal ratio range, the morphology of the obtained aluminum oxide nanosheets deteriorates, the surface energy increases, the hydrophobicity decreases, and the synergistic effect of aluminum oxide and titanium dioxide also decreases, thereby reducing the waterproof and moisture permeability and anti-ultraviolet performance.
[0070] As can be seen from Table 1, the only difference between Examples 6 and 7 and Example 3 is that in Example 6, the alumina-coated titanium dioxide in the step of preparing the micro-nano structure filler is replaced by nano alumina and nano titanium dioxide, and in Example 7, the hydrophobic modifier in the step of preparing the micro-nano structure filler is replaced by perfluorodecyltrimethoxysilane. Compared with Example 3, Examples 6 and 7 have reduced waterproof and moisture permeability and anti-ultraviolet performance. This is because if the alumina-coated titanium dioxide is replaced by nano alumina and nano titanium dioxide, the synergistic effect of the two is reduced, the morphology of the constructed micro-nano structure is deteriorated, and the synergistic effect with the dihydroxycoumarin derivative and tannic acid is also reduced; if the hydrophobic modifier is replaced by perfluorodecyltrimethoxysilane, the reactivity and compatibility of the micro-nano structure filler are reduced, so that the waterproof and moisture permeability and anti-ultraviolet performance are reduced.
[0071] As can be seen from Table 1, the only difference between Examples 8 and 9 and Example 3 is that: in Example 8, trifluorobenzaldehyde is not added in the step of preparing the thickened fluorinated modified polyvinyl alcohol, and in Example 9, tannic acid is not added in the step of preparing the thickened fluorinated modified polyvinyl alcohol. Compared with Example 3, Examples 8 and 9 have reduced waterproof and moisture permeability and UV resistance. This is because if trifluorobenzaldehyde is not added, polyvinyl alcohol lacks hydrophobic modification, its hydrophobic property is reduced, and thus the waterproof and moisture permeability is affected; if tannic acid is not added, the bonding force between the high waterproof coating and the fabric is reduced, the stability of the fabric is reduced, and thus the waterproof and moisture permeability and UV resistance are reduced.
[0072] It can be seen from Table 1 that the only difference between Example 10 and Example 3 is that in Example 10, the base fabric is replaced with nylon fabric. Compared with Example 3, the moisture permeability of Example 10 is reduced. This is because the base fabric is replaced with nylon fabric, which lacks relatively hydrophilic viscose fiber, and the moisture absorption and perspiration performance of nylon fabric is reduced, and the fabric is not easy to breathe, so the moisture permeability is reduced.
[0073] As can be seen from Table 1, the only difference between Examples 11 and 12 and Example 3 is that in Example 11, the modified nano zinc oxide in the step of preparing the waterproof and breathable membrane is replaced by nano zinc oxide, and in Example 12, the modified nano zinc oxide is not added in the step of preparing the waterproof and breathable membrane. Compared with Example 3, the waterproof and breathable performance of Examples 11 and 12 is reduced. This is because if the modified nano zinc oxide is replaced by nano zinc oxide, the nano zinc oxide lacks long amino chains, and its reactivity and compatibility are reduced. It cannot react with polyurethane as a chain extender. The surface roughness of the electrospun fiber is only improved by blending and doping, and the stability and hydrophobicity of the waterproof and breathable membrane are reduced; if the modified nano zinc oxide is not added, the stability and hydrophobicity are further reduced, so that the waterproof and breathable performance is reduced.
[0074] As can be seen from Table 1, the only difference between Comparative Example 1 and Example 3 is that the micro-nano structure filler is replaced by titanium dioxide nanorods in Comparative Example 1. Compared with Example 3, the waterproof and moisture permeability performance and the anti-ultraviolet performance of Comparative Example 1 are significantly reduced. This is because the micro-nano structure filler is replaced by titanium dioxide nanorods, and the titanium dioxide nanorods lack the modification treatment of aluminum oxide nanosheets and hydrophobic modifiers, and their surface morphology is deteriorated, and the hydrophobic performance and reaction performance are reduced. The synergistic effect with other components in the coating is weakened, so that the waterproof performance and anti-ultraviolet performance are significantly reduced.
[0075] As can be seen from Table 1, the only difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, the thickened fluorinated modified polyvinyl alcohol is replaced by polyvinyl alcohol. Compared with Example 3, the waterproof and moisture permeability and UV resistance of Comparative Example 2 are significantly reduced. This is because the thickened fluorinated modified polyvinyl alcohol is replaced by polyvinyl alcohol, lacks the introduction of phenyl and fluorine atoms and the modification treatment of tannic acid, the hydrophobicity of polyvinyl alcohol is reduced, the surface energy is increased, the synergistic effect between the components in the coating is weakened, the bonding force between the coating and the surface of the fabric is reduced, and the stability of the fabric is reduced, so that the waterproof and moisture permeability and UV resistance are significantly reduced.
[0076] As can be seen from Table 1, the only difference between Comparative Example 3 and Example 3 is that no dihydroxycoumarin derivative is added in Comparative Example 3. Compared with Example 3, the waterproof and moisture permeability and UV resistance of Comparative Example 3 are significantly reduced. This is because no dihydroxycoumarin derivative is added, the dimerization and depolymerization of the coumarin group are lacking, the UV resistance and stability of the coating are reduced, and thus the waterproof and moisture permeability and UV resistance are significantly reduced.
[0077] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A highly waterproof fabric, characterized in that: The highly waterproof fabric comprises a waterproof and breathable membrane, a base fabric and a highly waterproof coating arranged in sequence from the inside to the outside. The highly waterproof coating is obtained by coating the highly waterproof coating on the side of the base fabric away from the waterproof and breathable membrane. The highly waterproof coating comprises the following components in parts by mass: 5-10 parts of micro-nano structure filler 4-6 parts of dihydroxycoumarin derivatives 20-30 parts of fluorinated modified polyvinyl alcohol Solvent 100-120 parts.
2. A highly waterproof fabric according to claim 1, characterized in that: The micro-nano structure filler comprises titanium dioxide nanorods, aluminum oxide nanosheets and a hydrophobic modifier.
3. A highly waterproof fabric according to claim 2, characterized in that: The aluminum oxide nanosheets are attached to the surface of the titanium dioxide nanorods to obtain aluminum oxide-attached titanium dioxide. The raw materials for preparing the aluminum oxide nanosheets include aluminum chloride hexahydrate, polyethylene glycol and carbonamide.
4. A highly waterproof fabric according to claim 3, characterized in that: The mass ratio of aluminum chloride hexahydrate, polyethylene glycol and carbonamide is (0.4-0.6):0.08:
1.
5. The highly waterproof fabric according to claim 2, characterized in that: The raw materials for preparing the hydrophobic modifier include isocyanate propyl triethoxysilane and perfluoroalkyl ethyl acrylate.
6. The highly waterproof fabric according to claim 1, characterized in that: The raw materials for preparing the viscosity-enhancing fluorinated modified polyvinyl alcohol include polyvinyl alcohol, trifluorobenzaldehyde and tannic acid.
7. The highly waterproof fabric according to claim 1, characterized in that: The base fabric is obtained by blending viscose fiber and nylon fiber.
8. The highly waterproof fabric according to claim 1, characterized in that: The waterproof and breathable film is obtained by electrostatic spinning, and comprises polyacrylonitrile and polyurethane, and the polyurethane is chain-extended and modified by modified nano zinc oxide.
9. A highly waterproof fabric according to claim 8, characterized in that: The modified nano zinc oxide is prepared by the following steps: Nano zinc oxide and 3-chloropropyltrimethoxysilane were mixed and dispersed in toluene, deionized water was added after stirring, and 1,8-octanediamine was added after stirring in a water bath to react, and stirring in a water bath to react was continued, and the obtained product solution was filtered to obtain a filtrate, and the filtrate was washed with anhydrous ethanol, and the washed filtrate was dried in an oven at 80°C for 6 hours to obtain modified nano zinc oxide.
10. The highly waterproof fabric according to claim 1, characterized in that: The highly waterproof fabric is prepared by the following steps: The viscose fiber and the nylon fiber are blended to obtain a base fabric; an adhesive is coated on the base fabric, a waterproof and breathable membrane is compounded to the side of the base fabric coated with the adhesive, and the fabric is dried and baked to obtain a fabric with a waterproof and breathable membrane; a highly waterproof coating is coated on the side of the fabric with the waterproof and breathable membrane away from the waterproof and breathable membrane to obtain a fabric with a highly waterproof coating, the fabric with the highly waterproof coating is dried and baked to obtain a semi-finished product, and the semi-finished product is washed with water and then air-dried to obtain a highly waterproof fabric.