Anti-ultraviolet aging synergistic flame-retardant paper and preparation method thereof

By introducing sodium para-aminobenzenesulfonate between the hydrotalcite layer, combined with an expansion-based flame retardant, an anti-UV aging coating was formed, which solved the problem of the degradation of the performance of the expansion-based flame retardant paper under ultraviolet light, and achieved efficient flame retardant and machinery 性能提升,适用于多功能纸制品。

CN118895686APending Publication Date: 2024-11-05SOUTH CHINA UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411277022.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing expansion-based flame retardant paper has reduced flame retardant properties and mechanical strength under long-term ultraviolet irradiation, limiting its application in home decoration, food packaging, construction and other industries.

Method used

Sodium p-aminobenzenesulfonate is introduced between the hydrotalcite layers, and modified hydrotalcite is used together with an expansion-based flame retardant to form an anti-ultraviolet aging coating and is coated on the surface of the paper to enhance its flame retardant and mechanical properties.

Benefits of technology

It significantly improves the paper's UV aging resistance and flame retardant properties, extends its service life, meets flame retardant standards, and reduces production costs, making it suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention belongs to the technical field of flame-retardant paper, and discloses anti-ultraviolet aging synergistic flame-retardant paper and a preparation method thereof. The method comprises the following steps: 1) dispersing hydrotalcite in water to obtain hydrotalcite dispersion liquid; the preparation method comprises the following steps: dissolving p-aminobenzene sulfonate in water to obtain a p-aminobenzene sulfonate solution; adding the hydrotalcite dispersion liquid into a p-aminobenzene sulfonate solution, adjusting the pH value to 6.5-7.5, reacting at 70-85 DEG C, and drying to obtain modified hydrotalcite; 2) mixing the modified hydrotalcite with a styrene-acrylic emulsion to obtain an anti-ultraviolet aging coating; 3) coating two surfaces of the raw paper with the flame-retardant coating, drying, coating one surface of the raw paper with the anti-ultraviolet aging coating, drying, and curing to obtain the anti-ultraviolet aging synergistic flame-retardant paper.The method is simple, the prepared flame-retardant paper has remarkable anti-ultraviolet aging capability, and meanwhile, the flame-retardant property and the mechanical property of the flame-retardant paper are synergistically improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame-retardant paper and relates to anti-ultraviolet aging synergistic flame-retardant paper and a preparation method thereof. Background Art

[0002] Cellulose paper is mostly made of plant fibers. The strong flammability of plant fibers determines the flammability of paper and paper products. Most fires in daily life are caused by paper products, especially interior decoration materials such as wallpaper. Therefore, the research on flame retardant paper has received widespread attention.

[0003] Most flame-retardant papers are made by adding flame retardants to the surface of the paper by coating or spraying. Among them, intumescent flame retardants are a commonly used type of halogen-free acid source, gas source and carbon source flame retardant, such as ammonium polyphosphate and melamine. However, the physical properties and chemical structure of intumescent flame retardants will change when they are exposed to ultraviolet light for a long time. For example, flame-retardant paper coated with ammonium polyphosphate will decompose after long-term ultraviolet light exposure to produce phosphoric acid, which reduces the pH value of the paper, causing the paper to age, and the flame retardancy and mechanical strength of the paper will decrease. This limits the application of intumescent flame retardant paper in home decoration, food packaging, construction and other industries.

[0004] The invention introduces sodium p-aminobenzenesulfonate between hydrotalcite layers, so that the hydrotalcite coated paper has significant anti-ultraviolet aging ability, and synergistically improves its flame retardant ability, thereby preparing anti-ultraviolet aging synergistic flame retardant paper with excellent performance. Summary of the invention

[0005] In order to overcome the shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide an anti-ultraviolet aging synergistic flame retardant paper and a preparation method thereof. The present invention solves the technical problem that the flame retardant effect and mechanical strength of nitrogen-phosphorus flame retardant paper are drastically reduced, and obtains flame retardant paper with excellent anti-ultraviolet aging, improved flame retardant performance and strength.

[0006] To achieve the above object, the present invention provides the following technical solutions: A method for preparing anti-ultraviolet aging synergistic flame retardant paper comprises the following steps: 1) dispersing hydrotalcite in water to obtain a hydrotalcite dispersion; dissolving p-aminobenzenesulfonate in water to obtain a p-aminobenzenesulfonate solution; adding the hydrotalcite dispersion to the p-aminobenzenesulfonate solution, adjusting the pH to 6.5-7.5, then reacting at 70-85° C., and drying to obtain a modified hydrotalcite; 2) Mixing the modified hydrotalcite with styrene acrylic emulsion to obtain an anti-ultraviolet aging coating; 3) Applying the flame retardant coating on both sides of the base paper and drying; applying the anti-ultraviolet aging coating on one side of the base paper, drying, and curing to obtain anti-ultraviolet aging synergistic flame retardant paper.

[0007] The sulfanilic acid salt in step 1) is one or more of sodium sulfanilic acid and potassium sulfanilic acid.

[0008] The hydrotalcite is one or more of magnesium-aluminum hydrotalcite, zinc-aluminum hydrotalcite and magnesium-zinc hydrotalcite.

[0009] The mass ratio of the p-aminobenzenesulfonate to the hydrotalcite in step (1) is 1:(1.5-2.5).

[0010] The mass ratio of hydrotalcite to water in the hydrotalcite dispersion is 1:(25~40).

[0011] The hydrotalcite dispersion is obtained by placing the hydrotalcite in water, breaking it, dispersing it, and washing it with water. The breaking refers to grinding it with a wall-breaking machine for 1 min to 2 min, and dispersing it by ultrasonic dispersion for 10 min to 45 min.

[0012] The reaction is carried out under stirring conditions; the stirring speed is 600rpm~800rpm.

[0013] The reaction time is 20 to 30 hours.

[0014] The drying refers to removing part of the water by rotary evaporation, freezing, and freeze drying. The freezing temperature is -40°C.

[0015] The powder particle size of the modified hydrotalcite is between 350nm and 500nm.

[0016] Adding the hydrotalcite dispersion into the p-aminobenzenesulfonate solution means adding by dropping; the dropping speed is 40 drops / min to 60 drops / min.

[0017] The mass ratio of p-aminobenzenesulfonate to water in the p-aminobenzenesulfonate solution is 1:(30~40).

[0018] The absolute dry mass ratio of the modified hydrotalcite in step 2) to the styrene-acrylic emulsion is (0.9-1.1):1.

[0019] In step 2), when preparing the anti-ultraviolet aging coating, water can be added to adjust the concentration. After adding water, the concentration of the modified hydrotalcite in the anti-ultraviolet aging coating is 5-30wt%.

[0020] The flame retardant coating in step 3) is obtained by mixing the intumescent flame retardant with the coating emulsion; the mixing is stirring, the stirring temperature is 23°C~25°C, and the rotation speed is 600rpm~800rpm.

[0021] The intumescent flame retardant is one or more of ammonium polyphosphate, melamine and pentaerythritol; the coating emulsion is one or more of styrene acrylic emulsion and acrylic resin emulsion.

[0022] The absolute dry mass ratio of the intumescent flame retardant to the coating emulsion is 1:(0.9-1.5).

[0023] During the preparation of the flame retardant coating, water can be added to adjust the concentration of the flame retardant coating to prevent the concentration from being too high. After adding water, the concentration of the flame retardant in the flame retardant coating is 5-20wt%.

[0024] The base paper in step 3) can be made of hardwood kraft bleached pulp, the main component of which is hardwood fiber.

[0025] The amount of the flame retardant coating on each side in step 3) is 10-14% of the mass of the base paper; after the flame retardant coating is applied on one side, it is dried at 100-110° C. for 5-15 minutes and cooled to room temperature.

[0026] The amount of the anti-ultraviolet aging flame retardant coating in step 3) is 5% to 30% of the base paper mass, preferably 9-11%; the coated paper is naturally dried in the shade at 100 to 110° C. for 10 to 15 minutes and cured for 3 to 7 minutes.

[0027] After the aminobenzenesulfonate is introduced between the hydrotalcite layers, the ultraviolet absorption performance is significantly improved, and the energy of the absorbed ultraviolet light can be dissipated and released in the form of fluorescence. The modified hydrotalcite of the present application not only makes the flame retardant paper have significant anti-ultraviolet aging ability but also improves the flame retardancy and mechanical properties of the flame retardant paper.

[0028] The synergistic flame retardant principle of the present invention: during combustion, the ammonium polyphosphate in the intumescent flame retardant acts as an acid source and foaming agent, reacting with cellulose (carbon source) to form an expanded carbon layer. The modified hydrotalcite absorbs a large amount of heat during the combustion process, and thermally decomposes on the surface of the expanded carbon layer to produce mixed metal oxides, forming a regular porous carbon layer. The double carbon layer structure has better toughness and thermal stability, and greatly plays the role of oxygen barrier, flame retardant, heat insulation and inhibition of combustible gas generation. At the same time, melamine and modified hydrotalcite are used as gas sources to produce non-combustible gases such as ammonia during the combustion process, which dilutes the oxygen concentration and further inhibits combustion. In addition, Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention successfully prepared green multifunctional flame-retardant paper with high requirements for anti-ultraviolet aging performance, flame retardant performance, and mechanical properties. Due to the excellent ultraviolet barrier performance of the modified hydrotalcite coating, it can effectively reduce the performance loss of the intumescent flame-retardant paper under long-term ultraviolet irradiation. After coating it on the surface of the intumescent flame-retardant paper, a functional paper with excellent anti-ultraviolet aging performance, flame retardant performance, and mechanical properties is obtained.

[0029] (2) The present invention has the characteristics of simple and easy availability of raw materials and equipment, low cost, green and pollution-free production, and easy industrial mass production.

[0030] (3) The minimum oxygen index of the anti-ultraviolet aging flame retardant paper of the present invention is 31.8%, which has reached the flame retardant standard, and the vertical and horizontal burning performance far exceeds the national standard, and it has excellent mechanical and physical properties.

[0031] (4) The anti-ultraviolet aging synergistic hydrotalcite coating provided by the present invention can significantly reduce the loss of mechanical properties and flame retardant properties after aging. The anti-ultraviolet aging synergistic flame retardant paper was placed in a UV aging box for 7 days, and the flame retardant effect and mechanical and physical properties were effectively retained, and the vertical and horizontal burning reached the national standard. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 FT-IR images of the modified hydrotalcite prepared in Example 1 and Comparative Example 4 of the present invention and the original hydrotalcite; Figure 2 It is a tensile index graph of Examples 1-2 of the present invention, Comparative Examples 1-3, and a blank control group; Figure 3 The tear index graphs of Examples 1-2 of the present invention, Comparative Examples 1-3 and a blank control group are shown; Figure 4 This is a SEM image of the surface layer of the anti-ultraviolet synergistic flame retardant coating of SPL-PASS-LDH-15 flame retardant paper prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific examples, but the embodiments of the present invention are not limited thereto.

[0034] Elemental analysis: Elemental analysis is a chemical analysis method that studies the elemental composition of organic compounds. It is used to identify which elements are contained in organic compounds and to determine the percentage of these elements in organic compounds.

[0035] Anti-ultraviolet aging performance: Put the corresponding paper samples into the ultraviolet aging box, use 4 40W UV340 ultraviolet lamps to carry out ultraviolet aging on the paper samples for 7 consecutive days, and measure the flame retardant performance and mechanical strength of the corresponding paper samples before and after aging.

[0036] Flame retardant properties: According to the standard GB / T14656-2009, the paper prepared in each embodiment and comparative example was cut into 21cmx7cm samples, and the flame afterburning time, burning time and carbonization length were measured by a flame retardant paper and paperboard combustion tester. The shorter the flame afterburning time, the shorter the burning time and the shorter the carbonization length, the better the flame retardant properties of the flame retardant paper.

[0037] Mechanical strength performance measurement: According to the standard GB / T 12914-2018, the paper prepared in each embodiment and comparative example was cut into 15 cm × 1.5 cm specifications, and its tensile strength was measured using a tensile strength tester. According to the standard GB / T 455-2002, the paper prepared in each embodiment and comparative example was cut into 6.3 cm × 5.2 cm (vertical) specimens, and its tear strength was measured using a tear strength tester.

[0038] Oxygen index determination: According to ASTM-D2863, the limiting oxygen index test was carried out on a sample with a size of 60mm×140mm×0.30mm on an oxygen index tester. The limiting oxygen index can directly reflect the flame retardant properties of the material. The higher the limiting oxygen index, the better the flame retardant properties of the flame retardant paper.

[0039] Embodiment 1: A method for preparing anti-ultraviolet aging synergistic flame retardant paper comprises the following steps: (1) Preparation of flame-retardant coating by physical blending: 3 parts by weight of ammonium polyphosphate crystals, 1 part by weight of melamine powder and 4 parts by weight of styrene-acrylic emulsion were blended on an absolute dry basis, deionized water was added to make the concentration of the flame-retardant coating 15%, ultrasonic treatment was performed to prevent the solution from being too concentrated, and stirring was performed at room temperature for 1 hour to obtain a flame-retardant coating; (2) Preparation of flame-retardant paper by coating: Coat the base paper (the basis weight of the paper can be 80g / m 2 ), and then the coated paper is dried at 105°C for 10 minutes and cooled to room temperature; the flame retardant coating is coated on the other side of the base paper in an amount of 12% of the base paper mass to obtain a flame retardant paper named SPL; (3) Modified hydrotalcite: 5 parts by weight of sodium p-aminobenzenesulfonate was dissolved in 175 parts by weight of deionized water to obtain a sodium p-aminobenzenesulfonate solution; 10 parts by weight of hydrotalcite (magnesium aluminum hydrotalcite MgAl2(CO3)(OH) 16 ·4H2O) in 100 parts by weight of deionized water, crushed with a wall-breaking machine at low power for 1 minute, then ultrasonically dispersed for 10 minutes, and rinsed with deionized water to obtain a hydrotalcite dispersion, in which the amount of water in the dispersion is 325 parts; the hydrotalcite dispersion is slowly added dropwise to the sodium p-aminobenzenesulfonate solution, the pH is adjusted to 7±0.2, mechanically stirred at 80°C for 24 hours, taken out, rotary evaporated with a rotary evaporator, placed in an ultra-low temperature refrigerator for 48 hours (freezing temperature is -40°C), freeze-dried for 72 hours (freeze-dried temperature is -40°C), and finally a solid powder is obtained to obtain an anti-ultraviolet aging flame retardant, named 7-PASS-LDHs; (4) Preparation of anti-ultraviolet aging coating: 1 part by weight of 7-PASS-LDH was mixed with 1 part by weight of styrene acrylic emulsion on an absolute dry basis, and deionized water was added to make the concentration of the anti-ultraviolet aging coating 10%. Ultrasonication was performed to prevent the solution from being too concentrated, and stirring was performed at room temperature for 1 hour. (5) Preparation of anti-ultraviolet aging synergistic flame retardant paper by coating method: spray the anti-ultraviolet aging coating at a dosage of 10 wt% of the base paper mass on one side of the flame retardant paper, then dry the sprayed paper naturally in a windproof environment, and then dry it at 105 °C for 10 min, cure it for 5 min, and cool it to room temperature to obtain anti-ultraviolet aging synergistic flame retardant paper, named SPL-PASS-LDH-10.

[0040] Embodiment 2: The difference from Example 1 is that the amount of the anti-ultraviolet aging coating in step (5) is 15wt% of the base paper, and an anti-ultraviolet aging synergistic flame retardant paper is obtained, which is named SPL-PASS-LDH-15.

[0041] Figure 4 This is a SEM image of the surface layer of the anti-ultraviolet synergistic flame retardant coating of SPL-PASS-LDH-15 flame retardant paper prepared in Example 2 of the present invention.

[0042] Comparative Example 1: The method is basically the same as Example 1, except that steps (3), (4) and (5) are omitted, and a flame retardant paper named SPL is obtained.

[0043] Comparative Example 2: The method is basically the same as Example 1, except that: instead of modifying the hydrotalcite by the ion exchange method in step (3), the unmodified original hydrotalcite is directly used to prepare the coating in step (4), thereby obtaining the unmodified hydrotalcite flame retardant paper, which is named SPL-LDH-10.

[0044] Comparative Example 3: The method is basically the same as Comparative Example 2, except that the amount of the hydrotalcite coating in step (5) is 15 wt % of the base paper, and is named SPL-LDH-15.

[0045] Comparative Example 4: The method is basically the same as Example 2, except that in step (4), the pH is adjusted to 10±0.2, and the obtained anti-ultraviolet aging hydrotalcite is named 10-PASS-LDHs.

[0046] Characterization Tests: 1. Three types of hydrotalcites, namely, unmodified hydrotalcite and hydrotalcite 7-PASS-LDH prepared in Example 1 S , hydrotalcite 10-PASS-LDH prepared in Comparative Example 4 S FT-IR and elemental analysis were performed.

[0047] (1) FT-IR analysis: FT-IR of hydrotalcite Figure 1 As shown in the graph, the spectrum shows that the peak of hydroxyl (-OH) stretching vibration near 3450 in the three types of hydrotalcites is the peak of interlayer hydroxyl (-OH) stretching vibration, and the strong peak at 1360 is the characteristic infrared absorption peak of CO3. S and 10-PASS-LDH S The two absorption peaks 1188 and 1038 in 7-PASS-LDH are the bending vibration absorption peak of amino group and the characteristic absorption peak of sulfonate stretching vibration. S The peak values ​​are all greater than 10-PASS-LDH S The peak of 7-PASS-LDH S and 10-PASS-LDH S It was determined that the aminobenzenesulfonic acid anion successfully replaced CO3 through ion exchange, and had a better replacement effect at pH=7 during the reaction. Figure 1 FT-IR images of the modified hydrotalcite prepared in Example 1 and Comparative Example 4 of the present invention and the original hydrotalcite.

[0048] (2) Elemental analysis: Table 1 Elemental analysis results The elemental analysis results of the three hydrotalcites are shown in Table 1, which further confirms the anion content of p-aminobenzenesulfonic acid in the anti-ultraviolet aging hydrotalcite. S 、10-PASS-LDH S and 7-PASS-LDH S The N molar mass fractions of the hydrotalcites are 0%, 0.12% and 0.72% respectively, and the S elements are 0%, 0.23% and 0.47% respectively, indicating the presence of amino and sulfonic acid groups in the anti-ultraviolet aging hydrotalcites. In addition, the molar mass fractions of the C elements are 5.23%, 6.70% and 13.1% respectively, confirming the introduction of benzene rings rich in carbon elements. Elemental analysis proves that the hydrotalcite is successfully modified and the pH value during the reaction is kept at 7, which is more conducive to the ion exchange reaction. Therefore, in the preparation process, the pH value of Examples 1 and 2 is 7, which is more conducive to the preparation of anti-ultraviolet aging synergistic flame retardants.

[0049] 2. Flame retardant performance test and strength comparison before and after UV irradiation: (1) Flame retardant properties: According to the standard GB / T 14656-2009, the papers prepared in the embodiments and comparative examples and the blank control paper were cut into 21 cm x 7 cm samples before and after ultraviolet light irradiation, and combustion tests were performed respectively. The test results are shown in Table 2.

[0050] Table 2 Flame retardant performance test results Through the flame retardant performance measurement, through the data of Examples 1-2, Comparative Example 1 and the blank control group, it was found that the blank experimental group was completely burned out, Comparative Example 1 reached the flame retardant standard, and the average carbonization length of Comparative Example 1 was longer after ultraviolet irradiation. The average carbonization lengths of Examples 1 and 2 were both less than Comparative Example 1, indicating that the flame retardant effect was enhanced after the anti-ultraviolet synergistic flame retardant coating was applied. The higher the coating amount of the anti-ultraviolet synergistic flame retardant material, the better the flame retardant effect, and after 7 days of ultraviolet irradiation, the flame retardant effect decreased less and still reached the flame retardant standard. And under the comparison of the same amount of hydrotalcite coating, that is, Example 1 and Comparative Example 2, Example 2 and Comparative Example 3, after ultraviolet aging, the carbonization length growth value (carbonization length after ultraviolet irradiation-carbonization length without ultraviolet irradiation) is also much smaller than the comparative example, indicating that the anti-ultraviolet synergistic flame retardant coating is better than the unmodified hydrotalcite coating in anti-ultraviolet synergistic flame retardant effect.

[0051] (2) Strength properties: According to the standards GB / T 12914-2018 and GB / T 455-2002, the tensile strength and tear strength of the papers prepared in Examples 1-2 and Comparative Examples 1-3 were measured by tensile strength and tear strength testers, respectively, and quantitatively converted into tensile index and tear index. The test results are shown in Figure 2 and 3 shown. Figure 2 It is a tensile index graph of Examples 1-2 of the present invention, Comparative Examples 1-3, and a blank control group; Figure 3 The tearing index graphs of Examples 1-2 of the present invention, Comparative Examples 1-3 and a blank control group are shown.

[0052] Depend on Figure 2 , 3 It can be seen that after 7 days of ultraviolet irradiation, the tensile index and tear index of SPL decreased seriously. Although the tensile index and tear index of Examples 1 and 2 decreased, the degree of decrease was much less than that of Comparative Examples 2 and 3, which shows that after the anti-ultraviolet synergistic flame retardant hydrotalcite was coated on paper, the ultraviolet aging of paper fibers was reduced, and a considerable amount of mechanical strength was retained for the paper. In addition, considering the flame retardancy and cost of the comprehensive examples, the dosage of the anti-ultraviolet aging coating is controlled at 10%, which is the best, that is, Example 1 is the best.

[0053] (3) Oxygen index determination: On the premise that the dosage of anti-ultraviolet coating is determined to be 10%, the limiting oxygen index of SPL of comparative example 1, SPL-LDH-10 of comparative example 2, and SPL-PASS-LDH-10 of embodiment 1 were measured, and the results were 27.1%, 29.3%, and 31.8%, respectively. It was found that after coating with modified hydrotalcite, not only the mechanical properties were extremely well retained, but also the flame retardant effect was better. Compared with flame retardant paper, the flame retardant performance of SPL was significantly improved, reaching the flame retardant level.

Claims

1. A method for preparing anti-ultraviolet aging synergistic flame retardant paper, characterized in that: The following steps are involved: 1) dispersing hydrotalcite in water to obtain a hydrotalcite dispersion; dissolving p-aminobenzenesulfonate in water to obtain a p-aminobenzenesulfonate solution; adding the hydrotalcite dispersion to the p-aminobenzenesulfonate solution, adjusting the pH to 6.5-7.5, then reacting at 70-85° C., and drying to obtain a modified hydrotalcite; 2) Mixing the modified hydrotalcite with styrene acrylic emulsion to obtain an anti-ultraviolet aging coating; 3) Applying the flame retardant coating on both sides of the base paper and drying; applying the anti-ultraviolet aging coating on one side of the base paper, drying, and curing to obtain anti-ultraviolet aging synergistic flame retardant paper.

2. The method for preparing the anti-ultraviolet aging synergistic flame retardant paper according to claim 1, characterized in that: The mass ratio of the aminobenzenesulfonate to the hydrotalcite in step 1) is 1:(1.5-2.5); The absolute dry mass ratio of the modified hydrotalcite in step 2) to the styrene-acrylic emulsion is (0.9-1.1):

1.

3. The method for preparing the anti-ultraviolet aging synergistic flame retardant paper according to claim 1, characterized in that: The amount of the anti-ultraviolet aging coating in step 3) is 5% to 30% of the mass of the base paper.

4. The method for preparing the anti-ultraviolet aging synergistic flame retardant paper according to claim 3, characterized in that: The amount of the anti-ultraviolet aging coating in step 3) is 9% to 11% of the mass of the base paper.

5. The method for preparing the anti-ultraviolet aging synergistic flame retardant paper according to claim 1, characterized in that: The sulfanilic acid salt in step 1) is one or more of sodium sulfanilic acid and potassium sulfanilic acid; The hydrotalcite is one or more of magnesium-aluminum hydrotalcite, zinc-aluminum hydrotalcite and magnesium-zinc hydrotalcite; The flame retardant coating in step 3) is obtained by mixing an intumescent flame retardant with a coating emulsion; The amount of the flame retardant coating on each side in step 3) is 10-14% of the mass of the base paper.

6. The method for preparing the anti-ultraviolet aging synergistic flame retardant paper according to claim 5, characterized in that: The intumescent flame retardant is one or more of ammonium polyphosphate, melamine and pentaerythritol; the coating emulsion is one or more of styrene acrylic emulsion and acrylic resin emulsion; The mass ratio of the intumescent flame retardant to the absolute dry mass of the coating emulsion is 1:(0.9-1.5).

7. The method for preparing the anti-ultraviolet aging synergistic flame retardant paper according to claim 1, characterized in that: During the preparation of the flame retardant coating, water is added to adjust the concentration of the flame retardant coating. After adding water, the concentration of the flame retardant in the flame retardant coating is 5-20wt%; The base paper in step 3) is made from hardwood kraft bleached pulp, and its main component is hardwood fiber; Step 3) After the flame retardant coating is applied on one side, it is dried at 100-110°C for 5-15 minutes and cooled to room temperature; In step 2), when preparing the anti-ultraviolet aging coating, water is added to adjust the concentration. After adding water, the concentration of the modified hydrotalcite in the anti-ultraviolet aging coating is 5-30wt%; In step 3), the coated paper is naturally dried in the shade, dried at 100-110° C. for 10-15 minutes, and cured for 3-7 minutes.

8. The method for preparing the anti-ultraviolet aging synergistic flame retardant paper according to claim 1, characterized in that: In step 1), the mass ratio of hydrotalcite to water in the hydrotalcite dispersion is 1:(25-40); The reaction time is 20 to 30 hours; The drying refers to rotary evaporation to remove part of the water, freezing, and freeze drying; The powder particle size of the modified hydrotalcite is between 350nm and 500nm; Adding the hydrotalcite dispersion to the aminobenzenesulfonate solution means adding by dropwise addition; the dropping speed is 40 drops / min to 60 drops / min; The mass ratio of p-aminobenzenesulfonate to water in the p-aminobenzenesulfonate solution is 1:(30~40).

9. The method for preparing the anti-ultraviolet aging synergistic flame retardant paper according to claim 1, characterized in that: The hydrotalcite dispersion is obtained by placing hydrotalcite in water, breaking it, dispersing it, and then washing it with water; The crushing refers to grinding with a wall-breaking machine for 1min~2min, and the dispersion is ultrasonic dispersion, with a dispersion time of 10min~45min; The reaction is carried out under stirring conditions; the stirring speed is 600rpm~800rpm.

10. An anti-ultraviolet aging synergistic flame retardant paper obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Intumescent flame retardant paint based on hydrotalcite for smoke suppression for wood materials

    CN109943157A

  • Coating paper with flame retardant effect and preparation method thereof

    CN110042697A

  • Carbon paper with flame retardant property and preparation method thereof

    CN113389088A

  • Anti-ultraviolet flame retardant, preparation method thereof, anti-ultraviolet flame-retardant composition and product

    CN114753160A

  • Modified hydrotalcite flame retardant and application thereof

    CN115536906A