Monte Carlo method-based method for predicting slurry curing profile in ceramic material increasing process

The Monte Carlo method predicts the curing profile of the ceramic slurry, which solves the problem of increasing curing width and reducing depth of the ceramic slurry during the photocuring process, and improves the accuracy and efficiency of ceramic additive manufacturing.

CN118899052APending Publication Date: 2024-11-05SHENYANG INST OF AUTOMATION - CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410941775.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

During the photocuring process of ceramic slurry, due to the scattering of laser energy by ceramic powder, the curing width increases and the curing depth decreases, affecting the accuracy of ceramic green body manufacturing.

Method used

Using the Monte Carlo method to predict the curing profile of the slurry during ceramic additive process, the laser is simulated by obtaining laser parameters, calculating ceramic slurry, measuring the particle size distribution of ceramic powder and the refractive index of photosensitive resin. The propagation process in ceramic slurry calculates the laser energy absorption density function, thereby predicting the curing profile.

Benefits of technology

It improves the accuracy of ceramic additive manufacturing, reduces printing defects, guides the reasonable selection of process parameters such as laser power and scanning speed, and improves production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899052A_ABST
    Figure CN118899052A_ABST
Patent Text Reader

Abstract

A method for predicting a slurry curing profile in a ceramic additive manufacturing process based on a Monte Carlo method relates to the technical field of ceramic additive manufacturing, and comprises the following steps: firstly, acquiring physical parameters and proportions of components of ceramic slurry and process parameters in the ceramic additive manufacturing process, inputting the acquired parameters into a simulation program, and simulating the slurry curing profile in the ceramic additive manufacturing process; a laser energy absorption density function is obtained, and then an actual curing profile curve is solved according to curing conditions of photosensitive resin in photochemical reaction. According to the method, the dynamic state of photochemical reaction is combined, and the actual curing profile curve is finally obtained by solving the curing condition of the photosensitive resin. The curve reflects the form change in the slurry curing process, and is crucial for ensuring the structural integrity of the final ceramic green body. According to the method, the accuracy and reliability of ceramic additive manufacturing are improved, technical support is provided for parameter optimization and quality control in the manufacturing process, the production efficiency and the product quality are effectively improved, and the method has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic additive manufacturing, and in particular to a method for predicting a slurry solidification profile in a ceramic additive manufacturing process based on a Monte Carlo method. Background Art

[0002] Ceramics is a general term for all inorganic non-metallic solid materials. Ceramics is a material with a long history. As early as the early Neolithic Age, humans had mastered the technology of pottery making. With the development of technology, the connotation of ceramics has become more and more extensive. Today, ceramic materials are no longer limited to traditional daily necessities and decorations, but have developed into indispensable materials in many key fields such as power electronics, biomedicine, energy and power. Unlike traditional ceramics made of quartz, clay and feldspar, modern ceramic materials are usually high-purity metal or non-metal oxides, carbides, nitrides, etc. Modern ceramic materials can be divided into structural ceramics and functional ceramics according to their different uses. Structural ceramics refer to ceramics with excellent mechanical properties and are often used in various structural components. Functional ceramics are ceramics with unique physical properties in a certain aspect, such as piezoelectric ceramics, electro-optical ceramics, etc.

[0003] Ceramic materials are widely used in various fields of industry due to their excellent mechanical, thermal and chemical properties such as high temperature resistance, wear resistance, high hardness, high strength and low toxicity. In the field of aerospace, the blades of aircraft engines work in high temperature, high speed and high pressure environment. Ceramic-based fiber-reinforced composite materials have the characteristics of high specific strength and high temperature resistance, and are ideal structural materials for the hot end components of aircraft engines. The corrosion resistance of ceramics makes them widely used in the chemical industry, and they are used to manufacture reaction vessels that need to work in strong acid and alkali environments and utensils used under extreme conditions such as high-temperature crucibles. In addition, ceramic materials also have good insulation properties and are indispensable materials in the power electronics industry. They are used to manufacture insulators in high-voltage transmission lines and key electronic components such as capacitors in circuits. In daily life, ceramic products are widely used in tableware and sanitary ware for their beautiful and durable characteristics. In the field of biomedicine, high-purity ceramics are used as artificial bones and teeth. Therefore, ceramic materials are not only the cornerstone of industrial production, but also key materials to promote scientific and technological innovation and improve the quality of human life.

[0004] SLA (Stereolithography Appearance) is a revolutionary manufacturing technology that uses a ceramic slurry made of a mixture of photosensitive resin and ceramic powder, and solidifies the resin by irradiating it with a light source of a specific wavelength, thereby building a complex ceramic structure layer by layer. Stereolithography was proposed by Charles W Hull in 1984, and the first commercial SLA 3D printer was built in 1988. It is one of the earliest 3D printing technologies proposed and commercially applied. This technology uses ultraviolet lasers to scan layer by layer in the shape of the cross section of the object in the liquid photosensitive resin to solidify it. The platform then drops and continues to print the next layer, gradually building a three-dimensional object. SLA technology was originally mainly used for photosensitive resin materials. However, over time, researchers began to explore the application of this technology to more types of materials. In 1995, Griffith, Halloran and others first used SLA technology for the manufacture of ceramic parts. In the following decades, with the advancement of materials science, lasers, and servo systems, SLA ceramic additive manufacturing technology has made leaps and bounds. This significantly improves the accuracy and efficiency of the printing process, making it possible to produce parts with more complex shapes. Compared with other ceramic processes, SLA ceramic 3D printing technology has great advantages in preparing complex shapes and high-precision large parts.

[0005] However, in the process of photocuring ceramic green body forming, since the ceramic slurry usually has a high solid content of ceramics and the refractive index difference between ceramics and photosensitive resin is large, the propagation of light in the ceramic slurry will be strongly scattered. This phenomenon will cause the curing width of the slurry to increase and the curing depth to decrease during the curing process. Summary of the invention

[0006] In the process of curing ceramic slurry by ultraviolet irradiation to form ceramic green body, the scattering of laser energy by ceramic powder leads to an increase in curing width and a decrease in curing depth, thus affecting the manufacturing accuracy of ceramic green body. In view of this technical problem, the present invention provides a method for predicting the curing profile of slurry in the process of ceramic additive manufacturing based on the Monte Carlo method. The method can accurately predict the curing profile of slurry with different parameters in the process of photocuring, improve printing accuracy, reduce printing defects, and guide the selection of appropriate process parameters, such as laser power and scanning speed. Thereby improving the printing accuracy and reducing printing defects, it has guiding significance for the reasonable selection of process parameters such as laser power and scanning speed.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A method for predicting a slurry solidification profile in a ceramic additive process based on a Monte Carlo method comprises the following steps:

[0009] Step 1, obtaining the spot diameter, pulse frequency, laser wavelength of the laser used in the ceramic additive process, and the power and scanning speed set by the laser during the process;

[0010] Step 2, calcining the ceramic slurry, so that the organic matter in the ceramic slurry is fully pyrolyzed and removed, and the ceramic powder contained therein is retained;

[0011] Step 3, using a laser particle size analyzer to obtain a particle size distribution histogram of the ceramic powder obtained in step 2;

[0012] Step 4, according to the mass change before and after the calcination process in step 2, the ratio between the ceramic powder and the photosensitive resin in the ceramic slurry is calculated;

[0013] Step 5, obtaining the photosensitive resin without ceramic particles in the ceramic slurry by centrifugation, and thereby obtaining the refractive index and extinction coefficient of the photosensitive resin and ceramic powder in the ceramic slurry at the laser wavelength of the laser obtained in step 1;

[0014] Step 6, obtaining the molar concentration and molar extinction coefficient of the photoinitiator used in the measured ceramic slurry at the laser wavelength of the laser obtained in step 1;

[0015] Step 7, calculating the particle size distribution function, average volume and average radius of the ceramic powder contained in the ceramic slurry according to the experimental data obtained in step 3;

[0016] Step 8, calculating the number of ceramic particles contained in a unit volume of the ceramic slurry according to the ratio of the ceramic slurry obtained in step 4 and the average volume of the ceramic powder obtained in step 7;

[0017] Step 9, calculating the probability density function of the distance between two ceramic particles in the ceramic slurry according to the number of ceramic particles contained in the unit volume of the ceramic slurry obtained in step 8;

[0018] Step 10, calculating the reflectivity of the ceramic slurry to the laser energy according to the refractive index and extinction coefficient of the photosensitive resin obtained in step 5;

[0019] Step 11, calculating the absorption coefficient of the ceramic slurry according to the molar concentration and molar extinction coefficient of the photoinitiator in the ceramic slurry obtained in step 6;

[0020] Step 12: According to the parameters obtained in steps 1 to 11, the propagation process of the laser in the ceramic slurry is simulated and calculated using the Monte Carlo method to obtain a Monte Carlo point cloud;

[0021] Step 13, using the kernel function probability density estimation method to obtain the laser energy absorption density function of the Monte Carlo point cloud obtained in step 12;

[0022] Step 14: Solve the laser energy absorption density function obtained in step 13 according to the curing conditions of the photosensitive resin to obtain a curing profile curve of the ceramic slurry.

[0023] Furthermore, the calcination in step 2 is performed by calcining the ceramic slurry in an air atmosphere at a temperature of 600° C. for 24-48 hours using a box furnace to ensure complete removal of all organic substances.

[0024] Furthermore, the measurement of the particle size distribution function in step 3 requires the use of anhydrous ethanol as a dispersant, and ultrasonic treatment for 10-15 minutes before measurement to avoid possible powder agglomeration.

[0025] Furthermore, the mass before and after the calcination process in step 4 needs to be measured using an analytical balance to ensure sufficient accuracy. At the same time, light protection is required during the measurement process to prevent ambient light from causing photochemical reactions and thus interfering with the measurement results.

[0026] Furthermore, the refractive index of the photosensitive resin in step 5 needs to be measured at 35°C using an Abbe refractometer. Do not add a photoinitiator during measurement to avoid polymerization of the photosensitive resin during the measurement process, thereby interfering with the measurement results. When centrifuging the photosensitive resin and ceramic particles in the ceramic slurry, a centrifugal operation of 10,000 r / min for more than 15 minutes is required.

[0027] Furthermore, the extinction coefficient is measured by an ultraviolet spectrophotometer in step 6. The molar concentration of the contained photoinitiator is measured by measuring the attenuation of the light intensity after the laser passes through a certain thickness of photosensitive resin.

[0028] Further, the particle size distribution function in step 7 is fitted by the particle size distribution histogram obtained in step 3. A ceramic particle sample with a number of more than 1,000,000 is obtained by using a rejection method according to the particle size distribution function. The radius of the ceramic particles of the sample is averaged to obtain the average radius of the ceramic particles. The volume of the ceramic particles of the sample is averaged to obtain the average volume of the ceramic particles.

[0029] Furthermore, in step 8, the volume of ceramic particles contained in a unit volume of the ceramic slurry is calculated according to the proportion of the ceramic slurry obtained in step 4. Furthermore, the number of ceramic particles contained in a unit volume of the ceramic slurry is calculated according to the average volume of the ceramic powder obtained in step 7.

[0030] Furthermore, the number of ceramic particles contained in a unit volume of the ceramic slurry in step 9 is substituted into the probability density function of the mean free path.

[0031] Furthermore, in step 10, the refractive index and extinction coefficient of the ceramic slurry are substituted into the Fresnel equation in combination with the refractive index of air to obtain the reflection of the ceramic slurry-air interface in the non-polarized state.

[0032] Furthermore, in step 12, a simulation program compiled by matlab is used to perform solution calculations.

[0033] Furthermore, the method of kernel function probability density estimation described in step 13 is used to estimate the obtained Monte Carlo particle point cloud, thereby obtaining an energy absorption density function.

[0034] Furthermore, the curing condition of the photosensitive resin in step 14 is that the energy density is greater than 20×10 -12 J / μm 3 .

[0035] Compared with the prior art, the present invention has the following advantages:

[0036] 1. This paper proposes a prediction model for the curing behavior of ceramic slurry based on the Monte Carlo method and conducts experimental verification. Based on the Mie scattering theory, the effects of particle size distribution, ceramic content and different ceramic types on the curing behavior are considered, and the possible reasons are analyzed.

[0037] 2. The present invention is based on physical modeling, with clear principles and physical meanings, and does not contain any empirical parameters. It can predict the curing profile curve of ceramic slurry more accurately under different types of ceramic powders, ceramic slurries with different ceramic contents, and photosensitive resins with different proportions, and has good applicability.

[0038] 3. In terms of numerical calculation, the simulation speed of the present invention is fast and easy to expand, and physical equations can be conveniently implanted. The use of parallel computing improves the running speed, and the use of the continued fraction algorithm to solve the Mie scattering phase function improves the numerical stability in the solution process.

[0039] 4. The method of the present invention not only improves the accuracy and reliability of ceramic additive manufacturing, but also provides technical support for parameter optimization and quality control in the manufacturing process, effectively improving production efficiency and product quality, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Schematic diagram of slurry solidification in ceramic additive manufacturing process;

[0041] Figure 2 The refractive index and extinction coefficient of the aluminum oxide and the photoinitiator 819 used in the present invention;

[0042] Figure 3Three different kernel functions used for kernel function probability density estimation of the present invention;

[0043] Figure 4 is a histogram of particle size distribution of ceramic powder in an embodiment of the present invention;

[0044] Figure 5 is a Monte Carlo point cloud in an embodiment of the present invention;

[0045] Figure 6 is the energy distribution density function in an embodiment of the present invention;

[0046] Figure 7 A comparison diagram of the simulation prediction results and the actual results in the embodiment of the present invention;

[0047] Figure 8 It is a simulation program flowchart of the present invention. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0049] Example

[0050] A method for predicting a slurry solidification profile in a ceramic additive process based on a Monte Carlo method comprises the following steps:

[0051] Slurry curing in ceramic additive manufacturing Figure 1 The flowchart of the entire simulation process is shown in Figure 8 shown.

[0052] Step 1: Use anhydrous ethanol as a solvent to immerse alumina powder (average particle size is about 0.47 μm), and then add oleic acid with a mass fraction of 1 wt % as a dispersant.

[0053] Step 2: After ball milling the alumina powder suspension for 4 hours, place it in a vacuum oven and dry it at 150° C. for 24 hours.

[0054] Step 3: After taking out, crush the dried and compacted alumina with a mortar, and then pass it through a 100-mesh sieve to obtain surface-modified alumina powder.

[0055] Step 4: using 60 vol% of 1,6-hexanediol diacrylate (HDDA), 20 vol% of trimethylolpropane triacrylate (TMPTA) as photosensitive resin monomers and 20 vol% of PEG-200 as a plasticizer.

[0056] Step 5: Add 1 wt % of photoinitiator 819 and mix in a magnetic stirrer at room temperature for 30 minutes to obtain a resin premix.

[0057] Step 6: Then, the surface-modified alumina powder is added to the resin premix in batches, and the mixture is ball-milled for 4 hours between two additions and for 24 hours after the last addition, with the ball mill speed being 500 r / min, so as to prepare a ceramic slurry with good dispersibility.

[0058] Step 7: The prepared ceramic slurry was filtered through a 100-mesh sieve to remove impurities, and then placed in a vacuum defoaming device for 2 hours to eliminate bubbles. The prepared ceramic slurry was placed in a black plastic bucket at room temperature and kept away from light. Before use, the slurry was mixed with a three-roller for 30 minutes to prevent uneven slurry content caused by ceramic powder sedimentation.

[0059] Step 8: The spot diameter of the laser is 35 μm, the rated power is 3 W, the output power is 90%, the pulse frequency is 150 kHz, the laser wavelength is 355 nm, and the scanning speed is 5000 mm / s.

[0060] Step 9: Use a laser particle size analyzer to obtain a particle size distribution histogram of the alumina powder in the ceramic slurry, such as Figure 4 shown.

[0061] Step 10, calcining the ceramic slurry at 600°C for 24 hours, and calculating the mass change before and after calcination to obtain a mass ratio of alumina powder to photosensitive resin (mixture of HDDA and TMPTA) in the ceramic slurry of 7:3, and a volume ratio of 62:38.

[0062] Step 11: The refractive index of the photosensitive resin (mixture of HDDA and TMPTA) measured by Abbe refractometer is 1.45, and the extinction coefficient can be ignored. The refractive index and extinction coefficient of the alumina powder are as follows: Figure 2 shown.

[0063] Step 12: According to the mass of the photoinitiator 819 added in step 5 and the molecular weight of the photoinitiator 819, the molar concentration of the photoinitiator 819 is 0.026 mol / L. The molar extinction coefficient of the photoinitiator 819 is as follows: Figure 2 shown.

[0064] Step 13: Fit the particle size distribution function according to the particle size distribution histogram of the alumina powder obtained in step 9, and use the rejection method to obtain a sample of alumina particles with a number of more than 1,000,000 according to the particle size distribution function, average the particle radius of the sample to obtain the average radius of the particles, and average the volume of the particles of the sample to obtain the average volume of the particles. Specifically, the average volume of the alumina powder is 1.7465×10 -16 m 3 and the average radius is 1.9703×10 -6 m.

[0065] Step 14: According to the data of step 10 and step 13, the number of alumina particles contained in the unit volume of the ceramic slurry is 2.2221×10 15 pcs / m 3 .

[0066] Step 15: According to the amount of alumina particles contained in the unit volume of the ceramic slurry in step 14, the mean free path of the alumina particles is obtained to be 14.6 μm.

[0067] Step 16: According to the refractive index and extinction coefficient of the photosensitive resin obtained in step 11, the reflectivity of the ceramic slurry to the laser energy is calculated to be 0.09.

[0068] Step 17: Calculate the absorption coefficient of the ceramic slurry as 0.0215 based on the molar concentration and molar extinction coefficient of the photoinitiator 819 used in the ceramic slurry obtained in step 12.

[0069] Step 18: Use the Monte Carlo method to simulate the propagation process of the laser in the ceramic slurry and obtain the Monte Carlo point cloud as shown in Figure 5 shown.

[0070] Step 19: The Monte Carlo point cloud obtained in step 18 is used to obtain the laser energy absorption density function using the kernel function probability density estimation method, such as Figure 6 The three different kernel functions used in kernel function probability density estimation are as follows: Figure 3 shown.

[0071] Step 20: The laser energy absorption density function obtained in step 19 is used to solve the curing profile curve of the ceramic slurry according to the curing conditions of the photosensitive resin, such as Figure 7 shown.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for predicting the curing profile of slurry in ceramic additive process based on Monte Carlo method, characterized in that The following steps are involved: Step 1, obtaining the spot diameter, pulse frequency, laser wavelength of the laser used in the ceramic additive process, and the power and scanning speed set by the laser during the process; Step 2, calcining the ceramic slurry to fully pyrolyze and remove the organic matter in the ceramic slurry, and retain the ceramic powder contained therein; Step 3, obtaining a particle size distribution histogram of the ceramic powder in step 2; Step 4, calculating the ratio between the ceramic powder and the photosensitive resin of the ceramic slurry according to the mass change before and after the calcination process in step 2; Step 5, obtaining the photosensitive resin without ceramic particles in the ceramic slurry by centrifugation, and thereby obtaining the refractive index and extinction coefficient of the photosensitive resin and the ceramic material in the ceramic slurry at the laser wavelength of the laser obtained in step 1; Step 6, obtaining the molar concentration and molar extinction coefficient of the photoinitiator at the laser wavelength of the laser obtained in step 1; Step 7, calculating the particle size distribution function, average volume and average radius of the ceramic powder in the ceramic slurry according to the experimental data obtained in step 3; Step 8, calculating the number of ceramic particles contained in a unit volume of the ceramic slurry according to the ratio of the ceramic powder obtained in step 4 to the photosensitive resin and the average volume of the ceramic powder obtained in step 7; Step 9, calculating the probability density function of the distance between two ceramic particles in the ceramic slurry according to the number of ceramic particles contained in the unit volume of the ceramic slurry measured in step 8; Step 10, calculating the reflectivity of the ceramic slurry to the laser energy according to the refractive index and extinction coefficient of the photosensitive resin obtained in step 5; Step 11, calculating the absorption coefficient of the ceramic slurry according to the molar concentration and molar extinction coefficient of the photoinitiator obtained in step 6; Step 12: According to the parameters obtained in steps 1 to 11, the propagation process of the laser in the ceramic slurry is simulated and calculated using the Monte Carlo method to obtain a Monte Carlo point cloud; Step 13, using the kernel function probability density estimation method to obtain the laser energy absorption density function of the Monte Carlo point cloud obtained in step 12; Step 14: The laser energy absorption density function obtained in step 13 is used to solve the curing profile curve of the ceramic slurry according to the curing conditions of the photosensitive resin.

2. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that The calcination in step 2 is carried out at a temperature of 600°C for 24-48 hours to ensure complete removal of all organic matter.

3. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that The measurement of the particle size distribution function in step 3 requires the use of anhydrous ethanol as a dispersant and ultrasonic treatment for 10-15 minutes before measurement to avoid possible powder agglomeration.

4. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that The refractive index of the photosensitive resin in step 5 needs to be measured at 35°C using an Abbe refractometer, and no photoinitiator is added during the measurement to avoid polymerization of the photosensitive resin during the measurement process and thus interference with the measurement results; when centrifuging the photosensitive resin and ceramic particles in the ceramic slurry, a centrifugal operation of 10,000 r / min for more than 15 minutes is required; In step 6, the extinction coefficient is measured by an ultraviolet spectrophotometer; the molar concentration of the contained photoinitiator is measured by measuring the attenuation of the light intensity after the laser passes through a certain thickness of photosensitive resin.

5. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that The particle size distribution function in step 7 is fitted by the particle size distribution histogram obtained in step 3, and a ceramic particle sample with a quantity of more than 1,000,000 is obtained by using a rejection method according to the particle size distribution function; the radius of the ceramic particles of the sample is averaged to obtain the average radius of the ceramic particles; the volume of the ceramic particles of the sample is averaged to obtain the average volume of the ceramic particles.

6. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that In step 8, the volume of ceramic particles contained in unit volume of ceramic slurry is calculated according to the ratio of ceramic slurry obtained in step 4; the number of ceramic particles contained in unit volume of ceramic slurry is calculated according to the average volume of ceramic powder obtained in step 7.

7. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that In step 9, the number of ceramic particles contained in a unit volume of the ceramic slurry is substituted into the probability density function of the mean free path.

8. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that Step 10: Substituting the refractive index and extinction coefficient of the ceramic slurry into the Fresnel equation in combination with the refractive index of air can obtain the reflection of the ceramic slurry-air interface in the non-polarized state.

9. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that Step 12 uses the simulation program compiled by Matlab to perform solution calculations.

10. The method for predicting the slurry solidification profile in the ceramic additive process based on the Monte Carlo method according to claim 1, characterized in that The method of using kernel function probability density estimation described in step 13 estimates the obtained Monte Carlo particle point cloud to obtain an energy absorption density function; The curing condition of the photosensitive resin in step 14 is that the energy density is greater than 20×10 -12 J / μm 3 .

Citation Information

Patent Citations

  • A nanosecond laser ablation microgroove section profile prediction method

    CN109948288A