Preparation method of silver grid transparent conductive film
By using chemical silver plating and laser direct writing technology to prepare silver mesh transparent conductive films, the problems of high cost and complex processes of existing methods have been solved, enabling low-cost, mass production of silver mesh transparent conductive films with good optoelectronic properties and flexibility.
Patent Information
- Application Number
- CN202411218230.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-02
AI Technical Summary
Existing methods for preparing transparent conductive films suffer from high costs, complex processes, and unsuitability for mass production. In particular, methods for manufacturing metal meshes, such as photolithography and electro-hydraulic inkjet printing, suffer from low precision and slow speed.
A transparent conductive silver mesh film was prepared by combining chemical silver plating with laser direct writing technology. Silver nano islands and stacks of silver nanoparticles were formed on a PET substrate by chemical silver plating, and pattern design was realized by combining laser direct writing technology, avoiding the use of masks, simplifying the process and improving production efficiency.
A low-cost, high-volume production of silver mesh transparent conductive film has been achieved. It has good optoelectronic properties and flexibility. The laser direct writing technology is highly flexible, the pattern parameters are adjustable, and the cost is low and suitable for industrial production.
Smart Images

Figure CN118899124A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive films, and in particular relates to a method for preparing a silver grid transparent conductive film. Background Art
[0002] With the rapid development of optoelectronic devices, such as transparent heaters, solar thin-film batteries, smart windows and other flexible transparent conductive films as important components of optoelectronic devices, the requirements for optoelectronic performance are getting higher and higher. The traditional transparent conductive material is In2O3 (ITO), which has excellent optoelectronic properties, but with the rapid development of the economy, due to the brittleness, high production cost, poor stability and shortage of indium elements, researchers are developing a new generation of transparent conductive materials to replace traditional ITO.
[0003] At present, the research directions of transparent conductive films mainly include transparent conductive oxides (TCO), carbon-based materials, conductive polymers, metal nanowires and metal grids. The metal grid lines form a conductive path, and the inside of the grid plays a role in light transmission. The metal grid can adjust the size, line width, pattern and other parameters of the metal grid according to application requirements to adjust the optoelectronic performance. As a new generation of transparent conductive film, the metal grid has excellent comprehensive optoelectronic performance and good flexibility, becoming the most promising new generation of flexible transparent conductive film.
[0004] The manufacturing methods of metal mesh include photolithography, electro-hydrodynamic inkjet printing, laser direct writing, and nano-imprinting technology. The manufacture of high-performance metal mesh by photolithography and nano-imprinting technology usually requires the prefabrication of high-precision templates, and the overall process flow is complicated and cumbersome, and the cost is high. It needs to be further processed by PVD methods such as magnetron sputtering or evaporation. Electro-hydrodynamic inkjet printing technology is to use an electric field to drive the flow of droplets of nanoparticle ink to print a mesh on a flexible substrate. The metal mesh produced is often of high precision, but the preparation speed is slow, and it needs to be combined with annealing or low-temperature sintering and other processes in the later stage. It is not suitable for mass production of metal meshes.
[0005] Therefore, in view of the above technical problems, it is necessary to provide a method for preparing a silver grid transparent conductive film.
[0006] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a silver grid transparent conductive film, which can adopt chemical silver plating combined with laser direct writing technology to prepare a metal grid. Chemical silver plating has low cost and can achieve mass production. Laser direct writing technology has the advantages of fast speed and simple process. It does not require a mask plate and computer pattern drawing, and the metal grid pattern can be flexibly designed.
[0008] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0009] A method for preparing a silver grid transparent conductive film comprises the following steps:
[0010] S1. Roughening treatment: soak the release PET in the roughening liquid, and after the roughening treatment, rinse with deionized water;
[0011] S2. Sensitization treatment: transfer the roughened release PET to the sensitization solution for immersion. After sensitization, rinse the silver-plated surface with deionized water and dry it with an air compressor.
[0012] S3, chemical silver plating: after the sensitized PET completed in step S2 is peeled off, a silver plating solution is prepared, and after being mixed evenly, it is poured into a plastic container containing PET, and after the surface of the PET turns black, it is left to stand, and then heating is started;
[0013] S4, drying treatment: after the silver plating is completed, pour out the reaction solution, wash with deionized water 2-3 times, and blow dry with an air compressor until the surface appears silvery white, and then peel off the silver-plated PET;
[0014] S5. Laser direct writing: Draw the grid pattern shape and the number of arrays in advance, and then perform laser direct writing and etching on the silver-coated PET to successfully obtain a silver grid flexible transparent conductive film.
[0015] In one or more embodiments of the present invention, the specific steps of S3 are:
[0016] S31, peeling; transferring the sensitized PET into a plastic container, peeling off the back PET, so that the tape is directly bonded to the wall of the plastic container to prevent the PET from floating;
[0017] S32, prepare a silver plating solution; first, add 1 ml of silver nitrate solution to a 10 ml centrifuge tube, then add the diluted ammonia solution, stop adding when the mixture becomes clear, then add deionized water until the volume rises to 8 ml, then add 2 ml of glucose solution. Quickly shake the 10 ml centrifuge tube to obtain a silver plating solution;
[0018] S33, heating; after the silver plating solution is evenly mixed, pour it into a plastic container containing PET, and transfer the plastic container to the center of the heating table, shake the plastic container until the surface of the PET turns black and then stop, and heat it on the heating table for reaction.
[0019] In one or more embodiments of the present invention, the temperature of the heating stage in step S3 is set to 50° C., and the heating time of the heating stage is 15-30 min.
[0020] In one or more embodiments of the present invention, the roughening solution in step S1 includes concentrated sulfuric acid.
[0021] In one or more embodiments of the present invention, the method for preparing the roughening solution is: diluting concentrated sulfuric acid in deionized water to obtain the roughening solution. The volume ratio of the concentrated sulfuric acid to the deionized water is 1:1.
[0022] In one or more embodiments of the present invention, the concentration of the silver nitrate solution in step S32 is 17 g / L-20 g / L.
[0023] In one or more embodiments of the present invention, the method for preparing the diluted ammonia solution in step S32 is to dilute the concentrated ammonia solution in deionized water, and the volume ratio of the concentrated ammonia solution to deionized water is 1:80.
[0024] In one or more embodiments of the present invention, the concentration of the glucose solution in step S32 is 80-160 g / L.
[0025] In one or more embodiments of the present invention, the soaking time in step S1 is 20-50 minutes. The soaking time in step S2 is 6-8 minutes.
[0026] In one or more embodiments of the present invention, the sensitizing solution in step S2 includes a stannous chloride solution, and the concentration of the stannous chloride solution is 10-30 g / L.
[0027] Compared with the prior art, the method for preparing a silver grid transparent conductive film of the present invention has the following advantages:
[0028] 1) The release PET film is used to effectively prevent the contamination of the back of the PET during the pretreatment and chemical silver plating process, and the tape and the container are effectively bonded to prevent the floating of the PET, so that the chemical silver plating of the PET single side by solution method can be realized.
[0029] 2) The whole process is simple, no complicated operation is required, the laser direct writing speed is fast, the pattern flexibility is high, and the pattern parameters can be adjusted at will without being restricted by the mask. The preparation cost is low.
[0030] 3) Chemical silver plating, the silver layer is stacked in the form of silver nano-islands and silver nano-particles. The surface of the silver nano-particles has a plasma resonance effect, and a characteristic absorption peak is realized in the blue-violet light wavelength range of 400-600nm, achieving the silver grid transparent conductive film with potential application background in blue-violet light protection display. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 This is a flow chart of preparing a silver grid in one embodiment of the present invention; DETAILED DESCRIPTION
[0033] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0034] like Figure 1 As shown, a method for preparing a silver grid transparent conductive film in one embodiment of the present invention comprises the following steps:
[0035] S1. Roughening treatment: Soak the release PET in the roughening liquid for 20-50 minutes. After the roughening treatment, rinse with deionized water. The roughening treatment improves the wettability of the PET surface and produces hydrophilic groups, which is beneficial to the sensitization treatment of complexed stannous ions.
[0036] Furthermore, the roughening liquid includes concentrated sulfuric acid. The method for preparing the roughening liquid is: diluting the concentrated sulfuric acid in deionized water to obtain the roughening liquid. The volume ratio of the concentrated sulfuric acid to the deionized water is 1:1.
[0037] Preferably, the PET is immersed in the roughening liquid for 30 minutes.
[0038] S2. Sensitization treatment: transfer the roughened release PET to the sensitization solution and soak it for 6-8 minutes. After the sensitization, rinse the silver-plated surface with deionized water and blow dry it with an air compressor.
[0039] Furthermore, the sensitizing solution includes a stannous chloride solution, the concentration of the stannous chloride solution is 10-30 g / L, and preferably, the concentration of the stannous chloride solution is 20 g / L.
[0040] Preferably, the roughened release PET is transferred to the sensitizing solution and immersed for 7 minutes.
[0041] S3, chemical silver plating: after the sensitized PET completed in step S2 is peeled off, a silver plating solution is prepared, and after being mixed evenly, it is poured into a plastic container containing PET, and after the surface of the PET turns black, it is left to stand, and then heating is started;
[0042] S4, drying treatment: after the silver plating is completed, pour out the reaction solution, wash with deionized water 2-3 times, and blow dry with an air compressor until the surface appears silvery white, and then peel off the silver-plated PET;
[0043] S5. Laser direct writing: Draw the grid pattern shape and the number of arrays in advance, and then perform laser direct writing and etching on the silver-coated PET to successfully obtain a silver grid flexible transparent conductive film.
[0044] Among them, the specific steps of S3 are:
[0045] S31, peeling; transferring the sensitized PET into a plastic container, peeling off the back PET, so that the tape is directly bonded to the wall of the plastic container to prevent the PET from floating;
[0046] Among them, the size of the plastic container is preferably 54×54×20 mm3.
[0047] S32, prepare a silver plating solution; first, drop 1 ml of silver nitrate solution into a 10 ml centrifuge tube, then drop the diluted ammonia solution, it can be found that the mixed solution first becomes turbid and then becomes clear as the drop continues, stop dropping after it becomes clear, then drop deionized water until it rises to 8 ml, then drop 2 ml of glucose solution. Quickly shake the 10 ml centrifuge tube to obtain a silver plating solution;
[0048] Wherein, the concentration of the silver nitrate solution in step S32 is 17 g / L-20 g / L. Preferably, the concentration of the silver nitrate solution is 17 g / L.
[0049] It should be noted that the concentration range of chemical silver plating solution is 17g / L-20g / L. If the concentration of the plating solution is too high, the thicker the silver plating layer will be, and the nanoparticles will be splashed to a great extent due to phase explosion and plasma impact during the laser direct writing process. If the silver plating concentration is too low, the thinner the silver layer will be, and the microscopic continuity will be poor, which is not conducive to the improvement of conductivity. The method for preparing the diluted ammonia solution in step S32 is to dilute the concentrated ammonia solution in deionized water, and the volume ratio of the concentrated ammonia solution to the ionized water is 1:80.
[0050] The concentration of the glucose solution in step S32 is 80-160 g / L. Preferably, the concentration of the glucose solution is 100 g / L.
[0051] It should be noted that glucose as a reducing agent requires a moderate reaction speed. Other reducing agents such as triethanolamine have very slow reduction speeds, and the silver layer cannot grow normally. Sodium borohydride and hydrazine hydrate have strong reducing properties, so they react immediately after being added to the centrifuge tube, resulting in the inability to silver-plate the PET surface. Reducing agents such as formaldehyde may have potential effects due to the control of materials, but they have not been explored.
[0052] Glucose solution concentration requirements: If the glucose solution concentration is too low, the reaction will be incomplete due to diffusion and other factors, resulting in a thinner silver coating, poor coating continuity, and greater roughness, which seriously affects the preparation of the silver grid. If the glucose solution concentration is too high, the reaction will be rapid and the coating growth will be poor.
[0053] S33, heating; after the silver plating solution is evenly mixed, pour it into a plastic container containing PET, and transfer the plastic container to the center of the heating table, shake the plastic container until the surface of the PET turns black and then stop, and heat it on the heating table for reaction.
[0054] Furthermore, the temperature of the heating platform in step S33 is set to 50° C., and the heating time of the heating platform is 15-30 minutes. Preferably, the heating time of the heating platform is 20 minutes.
[0055] This application uses a release PET film as the initial substrate, which effectively protects the back of the silver-plated PET during the roughening and sensitization process. The bonding effect of the adhesive layer effectively prevents the back of the silver-plated PET from being contaminated. The release PET, as a key substrate material, can realize the solution-based chemical silver plating process.
[0056] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0057] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a silver grid transparent conductive film, characterized in that: The method comprises the following steps: S1. Roughening treatment: soak the release PET in the roughening liquid, and after the roughening treatment, rinse with deionized water; S2. Sensitization treatment: transfer the roughened release PET to the sensitization solution for immersion. After the sensitization is completed, rinse the silver-plated surface with deionized water and dry it with an air compressor. S3, chemical silver plating: after the sensitized PET completed in step S2 is peeled off, a silver plating solution is prepared, and after being mixed evenly, it is poured into a plastic container containing PET, and after the surface of the PET turns black, it is left to stand, and then heating is started; S4, drying treatment: after the silver plating is completed, pour out the reaction solution, wash with deionized water 2-3 times, and blow dry with an air compressor until the surface appears silvery white, and then peel off the silver-plated PET; S5. Laser direct writing: Draw the grid pattern shape and the number of arrays in advance, and then perform laser direct writing and etching on the silver-coated PET to successfully obtain a silver grid flexible transparent conductive film.
2. The method for preparing a silver grid transparent conductive film according to claim 2, characterized in that: The specific steps of S3 are: S31, peeling; transferring the sensitized PET into a plastic container, peeling off the back PET, so that the tape is directly bonded to the wall of the plastic container to prevent the PET from floating; S32, prepare a silver plating solution; first, add 1 ml of silver nitrate solution to a 10 ml centrifuge tube, then add the diluted ammonia solution, stop adding when the mixture becomes clear, then add deionized water until the volume rises to 8 ml, then add 2 ml of glucose solution. Quickly shake the 10 ml centrifuge tube to obtain a silver plating solution; S33, heating; after the silver plating solution is evenly mixed, pour it into a plastic container containing PET, and transfer the plastic container to the center of the heating table, shake the plastic container until the surface of the PET turns black and then stop, and heat it on the heating table for reaction.
3. The method for preparing a silver grid transparent conductive film according to claim 1 or 2, characterized in that: The temperature of the heating stage in the step S3 is set to 50° C., and the heating time of the heating stage is 15-30 min.
4. The method for preparing a silver grid transparent conductive film according to claim 2, characterized in that: In the step S1, the roughening solution includes concentrated sulfuric acid.
5. The method for preparing a silver grid transparent conductive film according to claim 4, characterized in that: The method for preparing the roughening solution is: diluting concentrated sulfuric acid in deionized water to obtain the roughening solution. The volume ratio of the concentrated sulfuric acid to the deionized water is 1:
1.
6. The method for preparing a silver grid transparent conductive film according to claim 5, characterized in that: The concentration of the silver nitrate solution in step S32 is 17 g / L-20 g / L.
7. The method for preparing a silver grid transparent conductive film according to claim 5 or 6, characterized in that: The method for preparing the diluted ammonia solution in step S32 is to dilute the concentrated ammonia solution in deionized water, and the volume ratio of the concentrated ammonia solution to deionized water is 1:
80.
8. The method for preparing a silver grid transparent conductive film according to claim 5, characterized in that: The concentration of the glucose solution in step S32 is 80-160 g / L.
9. The method for preparing a silver grid transparent conductive film according to claim 1, characterized in that: The soaking time in step S1 is 20-50 min. The soaking time in step S2 is 6-8 min.
10. The method for preparing a silver grid transparent conductive film according to claim 1, characterized in that: The sensitizing solution in step S2 includes a stannous chloride solution, and the concentration of the stannous chloride solution is 10-30 g / L.
Citation Information
Patent Citations
Method for preparing flexible polyester nickel-coating electrode
CN101892470A
Preparing method for vinyl plastic film silver cladding
CN105369225A
Composite flexible transparent electrode material and preparation method and application thereof
CN109801741A
Preparation method of flexible transparent conductive electrode with low surface roughness
CN112768116A