Micro LED chip and manufacturing method thereof
Patent Information
- Application Number
- CN202310500964.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
AI Technical Summary
During the preparation of Micro LED chips, there are material stress and lattice mismatch problems in the InGaN quantum well, resulting in the quantum-limited Stark effect (QCSE) affecting the radiation recombination rate of carriers and high energy in laser stripping technology The state may cause damage to the device's quantum well structure and blue shift, affecting the chip brightness.
A plurality of holes are made on the sapphire substrate and filled with the first aluminum nitride layer, GaN layer and second aluminum nitride layer arranged stacked to form an LED device, and the sapphire substrate is peeled off by laser peeling technology to protect the quantum wells by filling layer The luminescent layer reduces laser energy penetration and increases the absorption of the GaN film layer, improving the luminescent characteristics.
It effectively prevents the precipitation of In under high temperatures on the interface, reduces the problem of wavelength blue shift, and improves the luminous performance and brightness of Micro LED chips.
Smart Images

Figure CN118899370A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of chip technology, and more specifically, to a Micro LED chip and a method for manufacturing the same. Background Art
[0002] Micro LED technology can make LED structures thinner, smaller, and arrayed, and has many advantages such as high brightness, wide viewing angle, long service life, short response time, and low power consumption. In particular, Micro LED display technology does not require a backlight source and is superior to traditional TFT-LCD display technology in terms of response time, color rendering, and energy consumption.
[0003] The bandgap width of nitride semiconductors is continuously adjustable over a wide range, and their physical and chemical properties are stable, making them the preferred materials for preparing optoelectronic devices. However, the realization of high-performance nitride full-color Micro LED chips: from the perspective of materials, especially in the red and green light bands, due to the high In component in InGaN, the large material stress and lattice mismatch make it very difficult to produce high-quality InGaN quantum wells. At the same time, there is a strong polarization electric field in the InGaN quantum well due to the piezoelectric effect. The quantum confined Stark effect (QCSE) caused by this electric field will reduce the radiative recombination rate of carriers, thereby affecting the performance of the Micro LED screen; from the perspective of chip preparation, in the preparation process of Micro LED vertical structure chips, laser lift-off technology, namely LLO (Laser lift off) process, is usually used to peel the LED epitaxial structure from the sapphire substrate. However, the instantaneous high energy (interface high temperature) can easily cause damage to the device quantum well structure, and the In in the well layer is easy to precipitate, resulting in blue shift, while the chip brightness is reduced. The above phenomenon is particularly prominent in the preparation process of high In component red and green light Micro LED chips. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a method for manufacturing a Micro LED chip, which can effectively improve the light-emitting characteristics of the Micro LED chip.
[0005] In one aspect of the present invention, the present invention provides a method for making a Micro LED chip. According to an embodiment of the present invention, the method for making a Micro LED chip includes: making a plurality of holes arranged at intervals on a surface of a sapphire substrate; forming a filling layer in the hole, the filling layer including a first aluminum nitride layer, a GaN layer, and a second aluminum nitride layer stacked; forming an LED device on the surface of the sapphire substrate, the step of forming the LED device including the step of forming a plurality of quantum well light-emitting layers, the quantum well light-emitting layer including a blue quantum well light-emitting layer, a green quantum well light-emitting layer, and a red quantum well light-emitting layer, wherein the orthographic projection of the effective light-emitting area of the quantum well light-emitting layer on the sapphire substrate is located in the hole, and the blue quantum well light-emitting layer, the green quantum well light-emitting layer, and the red quantum well light-emitting layer all include InGaN; forming a conductive film layer, a reflector, and a binding metal layer in sequence on a side of the LED device away from the sapphire substrate; binding a pixel driving circuit on the surface of the binding metal layer away from the sapphire substrate; and peeling off the sapphire substrate and the filling layer using laser lift-off technology. Therefore, by filling the holes of the sapphire substrate with a filling layer containing gallium nitride, the quantum well light-emitting layer can be better protected: on the one hand, during the laser stripping process, the distance between the laser beam and the film thickness of the quantum well light-emitting layer structure increases, so that the laser energy intensity that penetrates the film layer and reaches the quantum well light-emitting layer is attenuated, thereby preventing the wavelength blue shift problem caused by the precipitation of In (indium) in the quantum well light-emitting layer under high temperature conditions at the interface; on the other hand, the overall thickness of the GaN film layer increases, which has a better absorption effect on the laser, and improves the luminescence characteristics of the Micro LED chip to a certain extent.
[0006] According to an embodiment of the present invention, the method for making the hole includes: forming a protective layer on one surface of the sapphire substrate; drilling a hole on the surface of the sapphire substrate on one side of the protective layer using laser drilling to form the hole, or the method for making the hole includes: forming a photoresist layer on one surface of the sapphire substrate, and patterning the photoresist layer to expose the surface of a predetermined area of the sapphire substrate; etching the sapphire substrate at the predetermined area to form the hole; removing the photoresist layer; forming the protective layer on the surface of the sapphire substrate where the hole is formed, and removing the portion of the protective layer corresponding to the hole.
[0007] According to an embodiment of the present invention, the method for making the holes satisfies at least one of the following conditions: the depth of the holes is 2.2 to 4.3 microns; the distance between the center points of two adjacent holes is 2.5 to 10.5 microns; the shape of the holes is at least one of circular, square and rectangular.
[0008] According to an embodiment of the present invention, the diameter of the circle is 2 to 10 micrometers; the side length of the square is 2 to 10 micrometers; the long side of the rectangle is 2.2 to 10.2 micrometers, and the short side of the rectangle is 2 to 10 micrometers.
[0009] According to an embodiment of the present invention, the thickness of the protective layer is 200-300 nm.
[0010] According to an embodiment of the present invention, the method for forming the filling layer in the hole includes: depositing the first aluminum nitride layer on the surface of the protective layer and in the hole; epitaxially growing the GaN layer on the surface of the first aluminum nitride away from the sapphire substrate; depositing the second aluminum nitride layer on the surface of the GaN layer away from the sapphire substrate; removing the protective layer, and at the same time removing the first aluminum nitride layer, the GaN layer and the second aluminum nitride layer located on the surface of the protective layer, optionally, the filling layer satisfies at least one of the following conditions: the thickness of the first aluminum nitride layer is 0.5 to 1 micron, the thickness of the GaN layer is 1 to 2 microns, and the thickness of the second aluminum nitride layer is 0.5 to 1 micron; the growth temperature of the epitaxial growth of the GaN layer is 1040°C to 1060°C.
[0011] According to an embodiment of the present invention, a method for forming the LED device on the surface of the sapphire substrate comprises: depositing a buffer layer on the surface of the sapphire substrate, the buffer layer covering the filling layer; epitaxially growing an undoped GaN film on the surface of the buffer layer away from the sapphire substrate; epitaxially growing an n-type heavily doped GaN layer on the surface of the undoped GaN film away from the sapphire substrate; epitaxially growing an n-type lightly doped GaN layer on the surface of the n-type heavily doped GaN layer away from the sapphire substrate; epitaxially growing a first barrier layer (First barrier) on the surface of the n-type lightly doped GaN layer away from the sapphire substrate; sequentially growing a first superlattice structure layer and a second superlattice structure layer on the surface of the first barrier layer away from the sapphire substrate, the first superlattice structure layer comprising a stacked arrangement of In x Ga 1-x N layer and non-doped GaN layer, x is 0.01-0.05, and the second superlattice structure layer includes a stacked In y Ga 1-y N layer and an n-type doped GaN layer, y is 0.01-0.08; the blue light quantum well light-emitting layer, the green light quantum well light-emitting layer and the red light quantum well light-emitting layer are grown on the surface of the second superlattice structure layer away from the sapphire substrate; an undoped GaN protective layer, an electron blocking layer, a hole supply layer and an ohmic contact layer are grown in sequence on the surface of the quantum well light-emitting layer away from the sapphire substrate.
[0012] According to an embodiment of the present invention, the method for forming the blue light quantum well light-emitting layer comprises: sequentially growing a first non-doped GaN film layer, an In film layer, and a second non-doped GaN film layer on a surface of the second superlattice structure layer away from the sapphire substrate; a Ga 1-a N potential well layer, second non-doped GaN film layer and In b Ga 1-b N barrier layer, wherein a is 0.18-0.21, and b is 0.01-0.03; the method for forming the green light quantum well light-emitting layer comprises: sequentially growing a third non-doped GaN film layer, an In film layer, and a second non-doped GaN film layer on the surface of the second superlattice structure layer away from the sapphire substrate; c Ga 1-c N potential well layer, a fourth non-doped GaN film layer and a first n-type doped GaN barrier layer, a fifth non-doped GaN film layer, In d Ga 1-d N potential well layer, a sixth undoped GaN film layer and a second n-type doped GaN barrier layer, wherein c is 0.24-0.25 and d is 0.25-0.28; the method for forming the red light quantum well light-emitting layer comprises: sequentially growing a seventh undoped GaN film layer, an In film layer and a second n-type doped GaN barrier layer on the surface of the second superlattice structure layer away from the sapphire substrate; e Ga 1-e N potential well layer, the eighth non-doped GaN film layer and In f Ga 1-f N barrier layer, ninth undoped GaN film layer, In g Ga 1-g N potential well layer, tenth non-doped GaN film layer, p-type doped GaN barrier layer and Al h Ga 1-h N layer, where e is 0.18 to 0.21, f is 0.01 to 0.03, g is 0.35 to 0.38, and h is 0.10 to 0.30;
[0013] According to an embodiment of the present invention, the preparation method for forming the LED device further satisfies at least one of the following conditions: the thickness of the buffer layer is 15 to 35 nm; the thickness of the non-doped GaN film is 3 to 4 μm, and the growth temperature of the epitaxial growth of the non-doped GaN film is 1040° C. to 1060° C.; the thickness of the n-type heavily doped GaN layer is 2 to 3 μm, the growth temperature is 1040° C. to 1060° C., and the doping concentration is 2×10 18 ~1×10 19 cm -3 The thickness of the n-type lightly doped GaN layer is 0.2 to 0.5 μm, the growth temperature is 1040°C to 1060°C, and the doping concentration is 1×10 17 ~5×10 17 cm-3 The thickness of the first barrier layer is 10-20 nm, and the material is non-doped GaN or In z Ga 1-z N, z is 0.01 to 0.03; x Ga 1-x The thickness of the N layer is 2 to 3 nm, the thickness of the non-doped GaN layer is 10 to 15 nm; y Ga 1-y The thickness of the N layer is 2-3 nm, the thickness of the n-type doped GaN layer is 10-15 nm, and the doping concentration is 1×10 17 ~5×10 17 cm -3 .
[0014] According to an embodiment of the present invention, the method for forming the LED device further satisfies at least one of the following conditions: the thicknesses of the second non-doped GaN film layer to the tenth non-doped GaN film layer are 1 to 3 nm respectively; a Ga 1-a The thickness of the N potential well layer is 2.5 to 3.5 nm. b Ga 1-b The thickness of the N barrier layer is 10 to 15 nm; c Ga 1-c The thickness of the N potential well layer is 2.5-2.5 nm, the thickness of the first n-type doped GaN barrier layer is 10-15 nm, and the doping concentration of the first n-type doped GaN barrier layer is 1×10 17 ~5×10 17 cm -3 , the In d Ga 1-d The thickness of the N potential well layer is 2.5-2.5 nm, the thickness of the second n-type doped GaN barrier layer is 10-15 nm, and the doping concentration of the second n-type doped GaN barrier layer is 1×10 17 ~5×10 17 cm -3 ; The In e Ga 1-e The thickness of the N potential well layer is 2.5 to 2.5 nm. f Ga 1-f The thickness of the N barrier layer is 10 to 15 nm. g Ga 1-g The thickness of the N potential well layer is 2.5 to 2.5 nm, the thickness of the p-type doped GaN barrier layer is 10 to 15 nm, and the thickness of the Al h Ga 1-h The thickness of the N layer is 1 to 2 nm.
[0015] According to an embodiment of the present invention, the method for forming the LED device further satisfies at least one of the following conditions: the thickness of the non-doped GaN protective layer is 15 to 30 nm; the material of the electron blocking layer is p-type doped AlGaN, the thickness of the electron blocking layer is 50 to 60 nm, and in the direction away from the sapphire substrate, the Al component in the electron blocking layer linearly changes from 20% to 30% to 0; the hole supply layer is a first p-type doped GaN layer, and the hole concentration is 2×10 17 ~5×10 17 cm -3 , with a thickness of 80 to 160 nm, or the hole-providing layer is a stacked p-type doped Al i Ga 1-i N layer and the second p-type doped GaN layer, the hole concentration is 1×10 18 ~3×10 18 cm -3 , the p-type doped Al i Ga 1-i The thickness of the N layer is 1.5 to 2.5 nm, i is 0.15 to 0.25, the thickness of the second p-type doped GaN layer is 5 to 8 nm; the ohmic contact layer is a p-type heavily doped GaN layer with a thickness of 10 to 20 nm, or the ohmic contact layer is a p-type heavily doped In j Ga 1-j N layer, j is 0.10 to 0.30, or the ohmic contact layer is a stacked p-type doped In k Ga 1-k N layer and a third p-type doped GaN layer, k is 0.10 to 0.30, the p-type doped In k Ga 1-k The thickness of the N layer is 105-205 nm, and the thickness of the third p-type doped GaN layer is 5-8 nm.
[0016] According to an embodiment of the present invention, when the sapphire substrate is peeled off by using the laser lift-off technology, the laser wavelength is 355 nm, 266 nm and 248 nm.
[0017] In another aspect of the present invention, the present invention provides a Micro LED chip. According to an embodiment of the present invention, the Micro LED chip is manufactured using the method described above. As a result, the Micro LED chip has good luminous performance. It can be understood by those skilled in the art that the Micro LED chip has all the features and advantages described above, and no further elaboration is given here. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0019] Figure 1 is a schematic structural diagram of a sapphire substrate in one embodiment of the present invention;
[0020] Figure 2 is a schematic structural diagram of preparing a sapphire substrate in another embodiment of the present invention;
[0021] Figure 3 is a schematic structural diagram of preparing a sapphire substrate in another embodiment of the present invention;
[0022] Figure 4 is a schematic structural diagram of a sapphire substrate and a filling layer in another embodiment of the present invention;
[0023] Figure 5 yes Figure 4 Schematic diagram of the planar structure;
[0024] Figure 6 It is a partial structural schematic diagram of manufacturing a Micro LED chip in another embodiment of the present invention;
[0025] Figure 7 is a schematic structural diagram of a blue light quantum well light-emitting layer in another embodiment of the present invention;
[0026] Figure 8 is a schematic structural diagram of a green light quantum well light-emitting layer in another embodiment of the present invention;
[0027] Fig. 9 is a schematic structural diagram of a red light quantum well light-emitting layer in another embodiment of the present invention;
[0028] Fig.10 It is a partial structural schematic diagram of manufacturing a Micro LED chip in another embodiment of the present invention;
[0029] Fig.11 It is a partial structural schematic diagram of manufacturing a Micro LED chip in another embodiment of the present invention;
[0030] Fig.12 It is a partial structural schematic diagram of manufacturing a Micro LED chip in another embodiment of the present invention;
[0031] Fig.13 It is a partial structural schematic diagram of manufacturing a Micro LED chip in another embodiment of the present invention;
[0032] Fig.14 This is a partial structural schematic diagram of a Micro LED chip manufactured in another embodiment of the present invention. DETAILED DESCRIPTION
[0033] The scheme of the present invention will be explained below in conjunction with embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are followed.
[0034] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0035] In one aspect of the present invention, the present invention provides a method for manufacturing a Micro LED chip. According to an embodiment of the present invention, the method for manufacturing a Micro LED chip includes:
[0036] S100: A plurality of holes 11 arranged at intervals are formed on a surface of a sapphire substrate 10, such as Figure 1 shown.
[0037] Among them, there is no special requirement for the thickness of the sapphire substrate. Technical personnel in this field can flexibly choose according to the actual product needs. In some embodiments, the thickness of the sapphire substrate is 400-450 microns, such as 400 microns, 410 microns, 420 microns, 430 microns, 440 microns, 450 microns, etc.
[0038] Further, the depth of the hole is 2.2 to 4.3 microns, such as 2.2 microns, 2.3 microns, 2.4 microns, 2.5 microns, 2.6 microns, 2.7 microns, 2.8 microns, 2.9 microns, 3.0 microns, 3.2 microns, 3.4 microns, 3.5 microns, 3.7 microns, 3.9 microns, 4.0 microns, 4.2 microns, and 4.3 microns. The holes of the above depths can effectively meet the filling of the filling layer.
[0039] like Figure 1 and Figure 5 As shown, the distance D between the center points of two adjacent holes is 2.5 to 10.5 microns, such as 2.5 microns, 3 microns, 3.5 microns, 4 microns, 4.5 microns, 5 microns, 5.5 microns, 6 microns, 6.5 microns, 7 microns, 7.5 microns, 8 microns, 8.5 microns, 9 microns, 9.5 microns, 10 microns, and 10.5 microns.
[0040] According to the embodiments of the present invention, there are no special requirements for the shape of the holes, and those skilled in the art can flexibly choose according to the actual situation of the quantum well light-emitting layer, for example, the holes can be formed in at least one of a circle, a square and a rectangle. The above shapes are relatively regular and simple, and are easy to etch. In some embodiments, the shape of the hole is a circle, and the diameter of the circle is 2 to 10 microns; in some embodiments, the shape of the hole is a square, and the side length of the square is 2 to 10 microns; in some embodiments, the shape of the hole is a rectangle, and the long side of the rectangle is 2.2 to 10.2 microns, and the short side of the rectangle is 2 to 10 microns. Therefore, the holes of the above sizes
[0041] According to an embodiment of the present invention, the method for making the hole 11 can be prepared by the following two ways, specifically:
[0042] In some embodiments, reference Figure 2 The method for making the hole 11 includes: forming a protective layer on one surface of the sapphire substrate 10; and drilling a hole on the surface of the sapphire substrate 10 on one side of the protective layer 20 by laser drilling to form the hole 11. After the laser drilling, the surface can be further ultrasonically cleaned with toluene, acetone, ethanol or deionized water, and blown dry with nitrogen for later use.
[0043] In other embodiments, reference Figure 3 The method for making the hole 11 includes: forming a photoresist layer 21 on a surface of the sapphire substrate 10, and patterning the photoresist layer 21 to expose the surface of the predetermined area 12 of the sapphire substrate 10; etching the sapphire substrate 10 at the predetermined area to form the hole 11; removing the photoresist layer 21; forming a protective layer 20 on the surface of the sapphire substrate 10 where the hole 11 is formed, and removing the portion of the protective layer 20 corresponding to the hole 11. After removing the portion of the protective layer 20 corresponding to the hole 11, it can be further ultrasonically cleaned with toluene, acetone, ethanol or deionized water, and blown dry with nitrogen for standby use. The thickness of the photoresist layer is 1 to 2 microns, and the shape and size of the predetermined area 12 are consistent with those of the hole 11. Furthermore, the specific process of patterning the photoresist layer 21 may be exposure and development, and the etching of the sapphire substrate 10 at the predetermined area may be performed by using an inductively coupled plasma etching device (ICP-RIE), but the depth is the depth of the hole 2.2 to 4.3 microns. In addition, the method of removing the portion of the protective layer 20 corresponding to the hole 11 may be: forming a 1 to 2 micron thick photoresist layer on the surface of the protective layer away from the sapphire substrate, then exposing and developing the photoresist layer, exposing the portion of the protective layer 20 corresponding to the hole, and then using an inductively coupled plasma etching device (ICP-RIE) to etch to the surface of the sapphire substrate.
[0044] According to the embodiments of the present invention, both of the above two methods can accurately punch holes in the sapphire substrate to obtain holes of the required size; and the process is relatively mature and convenient for industrial mass production. In the above step of making holes, the provision of the protective layer can protect the laser from damaging the edge of the hole and the surface of the sapphire substrate during the laser drilling process, and from damaging the sapphire substrate by the corrosive liquid during the subsequent formation of the filling layer.
[0045] The thickness of the protective layer is 200-300 nm, such as 200 nm, 220 nm, 240 nm, 250 nm, 260 nm, 280 nm, and 300 nm, so that the protective effect is better. The material of the protective layer can be silicon nitride or silicon oxide.
[0046] S200: forming a filling layer 30 in the hole, the filling layer 30 comprising a first aluminum nitride layer 31, a GaN layer 32 and a second aluminum nitride layer 33 stacked in layers, such as Figure 4 and Figure 5 As shown. By filling the holes of the sapphire substrate with a filling layer containing gallium nitride, the quantum well light-emitting layer can be better protected: on the one hand, in the subsequent laser lift-off process, the distance between the laser beam and the film thickness of the quantum well light-emitting layer structure increases, so that the laser energy intensity penetrating the film layer to the quantum well light-emitting layer is attenuated, thereby preventing the wavelength blue shift problem caused by the precipitation of In (indium) in the quantum well light-emitting layer under the high temperature state of the interface; on the other hand, the overall thickness of the GaN film layer increases, which has a better absorption effect on the laser, and improves the light-emitting characteristics of the Micro LED chip to a certain extent. Among them, compared with gallium nitride materials, aluminum nitride and the sapphire substrate have a better lattice matching, so pre-depositing the first aluminum nitride layer before growing the GaN layer can better improve the bonding force between the filling layer and the sapphire substrate; in addition, aluminum nitride also has a certain absorption effect on lasers, and the setting of the first aluminum nitride layer 31 and the second aluminum nitride layer 33 can better protect the quantum well light-emitting layer.
[0047] According to an embodiment of the present invention, the method for forming the filling layer in the hole 11 includes: depositing a first aluminum nitride layer 31 on the surface of the protective layer 20 and in the hole 11; epitaxially growing a GaN layer 32 on the surface of the first aluminum nitride layer 31 away from the sapphire substrate 10; depositing a second aluminum nitride layer 33 on the surface of the GaN layer 32 away from the sapphire substrate 10; removing the protective layer 20, and at the same time removing the first aluminum nitride layer 31, the GaN layer 32 and the second aluminum nitride layer 33 located on the surface of the protective layer 20. The structural schematic diagram can be referred to Figure 4 and Figure 5 . The technology is mature and the precision is high.
[0048] Among them, the specific method of removing the protective layer 20 and the first aluminum nitride layer 31, the GaN layer 32 and the second aluminum nitride layer 33 located on the surface of the protective layer 20 can be to use HF solution or BOE solution (buffered oxide etching solution) to chemically treat the epitaxial wafer, and the silicon nitride or silicon oxide protective layer attached to the sapphire surface is more easily corroded by the HF solution or BOE solution, and the AlN / GaN / AlN on the corresponding protective layer is removed at the same time. Further, through confocal microscopy or SEM test analysis, it can be determined whether the silicon nitride protective layer or silicon oxide protective layer and the AlN / GaN / AlN on the protective layer are completely removed. If there is any residue, it can be corrected by ICP-RIE etching until it is completely removed to expose the sapphire substrate.
[0049] In some embodiments, the first aluminum nitride layer 31 and the second aluminum nitride layer 33 can be prepared by a physical vapor deposition (PVD) process, and the thickness of the first aluminum nitride layer is 0.5 to 1 micron, for example, 0.5 micron, 0.6 micron, 0.7 micron, 0.8 micron, 0.9 micron, and 1.0 micron, and the thickness of the second aluminum nitride layer is 0.5 to 1 micron, for example, 0.5 micron, 0.6 micron, 0.7 micron, 0.8 micron, 0.9 micron, and 1.0 micron.
[0050] In some embodiments, the GaN layer 32 can be grown by vapor phase epitaxial growth technology (MOCVD), and the thickness of the GaN layer is 1 to 2 microns, such as 1.2 microns, 1.4 microns, 1.5 microns, 1.6 microns, 1.8 microns, and 2.0 microns. In this way, the quantum well light-emitting layer can be well protected, and a thicker GaN layer is not required, so the cost will not be high. The growth temperature of the epitaxially grown GaN layer is 1040°C to 1060°C. Thus, a GaN layer with good performance can be well grown.
[0051] S300: forming an LED device on the surface of the sapphire substrate 10, wherein the step of forming the LED device includes the step of forming a plurality of quantum well light-emitting layers, wherein the quantum well light-emitting layers include a blue light quantum well light-emitting layer 481, a green light quantum well light-emitting layer 482, and a red light quantum well light-emitting layer 483, wherein the orthographic projection of the effective light-emitting area of the quantum well light-emitting layer on the sapphire substrate is located in the hole, and the blue light quantum well light-emitting layer, the green light quantum well light-emitting layer, and the red light quantum well light-emitting layer all include InGaN. The LED device may be located on the surface close to the filling layer (such as Figure 6 as shown), it may also be located on the surface away from the filling layer.
[0052] According to an embodiment of the present invention, referring to Figure 6 , a method for forming an LED device on a surface of a sapphire substrate comprises:
[0053] T1: a buffer layer 41 is deposited on the surface of the sapphire substrate 10, and the buffer layer 41 covers the filling layer 30. The buffer layer can be deposited by physical vapor deposition (PVD), and the thickness of the buffer layer is 15-35 nm.
[0054] T2: epitaxially grow a non-doped GaN film 42 on the surface of the buffer layer away from the sapphire substrate. The thickness of the non-doped GaN film 42 is 3-4 μm, and the non-doped GaN film 42 can be grown by vapor phase epitaxial growth technology (MOCVD) at a growth temperature of 1040°C to 1060°C.
[0055] T3: epitaxially grow an n-type heavily doped GaN layer 43 on the surface of the non-doped GaN film 42 away from the sapphire substrate. The thickness of the n-type heavily doped GaN layer is 2-3 μm. The n-type heavily doped GaN layer can be grown by vapor phase epitaxial growth technology (MOCVD) at a growth temperature of 1040°C to 1060°C and a doping concentration of 2×10 18 ~1×10 19 cm -3 , where SiH4 is used as an n-type dopant.
[0056] T4: epitaxially grow an n-type lightly doped GaN layer 44 on the surface of the n-type heavily doped GaN layer 43 away from the sapphire substrate. The thickness of the n-type lightly doped GaN layer 44 is 0.2-0.5 μm. The n-type lightly doped GaN layer 44 can be grown by vapor phase epitaxial growth technology (MOCVD) at a growth temperature of 1040°C-1060°C and a doping concentration of 1×10 17 ~5×10 17 cm -3 , where SiH4 is used as an n-type dopant.
[0057] T5: epitaxially grow a first barrier layer 45 (first barrier) on the surface of the n-type lightly doped GaN layer 44 away from the sapphire substrate. The thickness of the first barrier layer 45 is 10-20 nm, and the material of the first barrier layer (First barrier) 45 is non-doped GaN or In z Ga 1-z N, z is 0.01~0.03, that is, In z Ga 1-z The composition of In in N is 1% to 3%.
[0058] T6: A first superlattice structure layer 46 and a second superlattice structure layer 47 are sequentially grown on the surface of the first barrier layer 45 away from the sapphire substrate 10. The first superlattice structure layer 46 is grown for 3 to 5 cycles, including a stacked arrangement In x Ga 1-xN layer and non-doped GaN layer, x is 0.01 to 0.05, that is, In x Ga 1-x The composition of In in the N layer is 1% to 5%. x Ga 1-x The N layer is disposed close to the first barrier layer (First barrier) 45, and the non-doped GaN layer is disposed away from the first barrier layer (First barrier) 45. x Ga 1-x The thickness of the N layer is 2 to 3 nm, and the thickness of the non-doped GaN layer is 10 to 15 nm; the second superlattice structure layer 47 is grown for 3 to 5 cycles, including the stacked In y Ga 1-y N layer and n-type doped GaN layer, y is 0.01 to 0.08, that is, In y Ga 1-y The composition of In in N is 1% to 8%. y Ga 1-y The N layer is disposed close to the first barrier layer (First barrier) 45, and the n-type doped GaN layer is disposed away from the first barrier layer (First barrier) 45. y Ga 1-y The thickness of the N layer is 2-3 nm, the thickness of the n-type doped GaN layer is 10-15 nm, and the doping concentration is 1×10 17 ~5×10 17 cm -3 .
[0059] T7: A blue quantum well light emitting layer 481 , a green quantum well light emitting layer 482 and a red quantum well light emitting layer 483 are grown on the surface of the second superlattice structure layer 47 away from the sapphire substrate 10 .
[0060] In some embodiments, the method for forming the blue light quantum well light emitting layer 481 comprises: sequentially growing a first non-doped GaN film layer 4811, an In film layer 4821, and a second non-doped GaN film layer 4812 on a surface of the second superlattice structure layer 47 away from the sapphire substrate 10; a Ga 1-a N potential well layer 4812, second non-doped GaN film layer 4813 and In b Ga 1-b N barrier layer 4814, such as Figure 7 As shown, a is 0.18 to 0.21, b is 0.01 to 0.03, that is, In a Ga 1-a The composition of In in the N potential well layer 4812 is 18% to 21%. b Ga 1-bThe In component of the N barrier layer 4814 is 1% to 8%. Among them, the blue light quantum well light emitting layer 481 contains a relatively high amount of indium. Due to the protection of the filling layer in the present invention, the blue light quantum well light emitting layer 481 of the present invention can still have good light emitting characteristics; moreover, when growing In a Ga 1-a Growing a first non-doped GaN film layer 4811 before the N potential well layer 4812 can effectively improve the surface flatness of the film layer and increase the In a Ga 1-a The growth quality of the N potential well layer 4812 is beneficial to the improvement of the device's luminous brightness; b Ga 1-b A second non-doped GaN film layer 4813 is grown before the N barrier layer 4814 to prevent In a Ga 1-a The precipitation of In in the N potential well layer is beneficial to the improvement of the luminescence brightness of the device.
[0061] The thickness of the first non-doped GaN film layer and the second non-doped GaN film layer are 1-3 nm respectively, and the growth temperature of the first non-doped GaN film layer is a Ga 1-a The growth temperature of the N potential well layer 4812 is the same as that of the second non-doped GaN film layer. b Ga 1-b The growth temperature of the N barrier layer 4814 is the same, which can effectively alleviate the problem of wave shift under large current injection; a Ga 1-a The thickness of the N potential well layer is 2.5 to 3.5 nm, and In b Ga 1-b The thickness of the N barrier layer is 10-15 nm, thus ensuring good luminescence properties of the blue light quantum well light emitting layer 481.
[0062] In some embodiments, the method for forming the green light quantum well light emitting layer 482 comprises: sequentially growing a third non-doped GaN film layer 4821, an In c Ga 1-c N potential well layer 4822, fourth non-doped GaN film layer 4823 and first n-type doped GaN barrier layer 4824, fifth non-doped GaN film layer 4825, In d Ga 1-d N potential well layer 4826, sixth non-doped GaN film layer 4827 and second n-type doped GaN barrier layer 4828, such as Figure 8 As shown, where c is 0.24-0.25, d is 0.25-0.28, that is, In c Ga 1-cThe composition of In in the N4822 potential well layer is 24% to 25%. d Ga 1-d The In content of the N potential well layer 4826 is 25% to 28%. Among them, the green light quantum well light emitting layer 482 contains a relatively high amount of indium. Due to the protection of the filling layer in the present invention, the green light quantum well light emitting layer 482 of the present invention can still have good light emitting characteristics; moreover, when growing In c Ga 1-c Growing a third non-doped GaN film layer 4821 before the N potential well layer 4822 can effectively improve the surface flatness of the film layer and increase the In c Ga 1-c The growth quality of the N potential well layer 4822 is beneficial to the improvement of the luminous brightness of the device; before growing the first n-type doped GaN barrier layer 4824, a fourth non-doped GaN film layer 4823 is grown to prevent In c Ga 1-c The precipitation of In in the N potential well layer is beneficial to the improvement of the device's luminescence brightness; d Ga 1-d Growing a fifth non-doped GaN film layer 4825 before the N potential well layer 4826 can effectively improve the surface flatness of the film layer and increase the In d Ga 1-d The growth quality of the N potential well layer 4826 is beneficial to the improvement of the luminous brightness of the device; before growing the second n-type doped GaN barrier layer 4828, a sixth non-doped GaN film layer 4827 is grown to prevent In d Ga 1-d The precipitation of In in the N potential well layer 4826 is beneficial to improving the luminous brightness of the device.
[0063] The thicknesses of the third non-doped GaN film layer to the sixth non-doped GaN film layer are 1 to 3 nm respectively, and the growth temperature of the third non-doped GaN film layer 4821 is about 100 nm. c Ga 1-c The growth temperature of the fourth non-doped GaN film layer 4823 is the same as the growth temperature of the first n-type doped GaN barrier layer 4824, and the growth temperature of the fifth non-doped GaN film layer 4825 is the same as the growth temperature of the In d Ga 1-d The growth temperature of the N-type potential well layer 4826 is the same, and the growth temperature of the sixth non-doped GaN film layer 4827 is the same as the growth temperature of the second n-type doped GaN barrier layer 4828, thereby effectively alleviating the problem of wave shift under large current injection. c Ga 1-cThe thickness of the N potential well layer is 2.5-2.5 nm, the thickness of the first n-type doped GaN barrier layer is 10-15 nm, and the doping concentration of the first n-type doped GaN barrier layer is 1×10 17 ~5×10 17 cm -3 ,In d Ga 1-d The thickness of the N potential well layer is 2.5-2.5 nm, the thickness of the second n-type doped GaN barrier layer is 10-15 nm, and the doping concentration of the second n-type doped GaN barrier layer is 1×10 17 ~5×10 17 cm -3 In this way, the green light quantum well light emitting layer 482 is guaranteed to have good light emitting properties.
[0064] In some embodiments, the method for forming the red light quantum well light emitting layer 483 comprises: sequentially growing a seventh non-doped GaN film layer 4831, an In e Ga 1-e N potential well layer 4832, the eighth non-doped GaN film layer 4833 and In f Ga 1-f N barrier layer 4834, ninth undoped GaN film layer 4835, In g Ga 1-g N potential well layer 4836, tenth non-doped GaN film layer 4837, p-type doped GaN barrier layer 4838 and Al h Ga 1-h N layer 4839, such as Fig. 9 As shown, where e is 0.18-0.21, f is 0.01-0.03, g is 0.35-0.38, and h is 0.10-0.30, i.e., In e Ga 1-e The composition of In in the N potential well layer 4832 is 18% to 21%. f Ga 1-f The composition of In in the N barrier layer 4834 is 35% to 38%. g Ga 1-g The In content of the N potential well layer 4836 is 35% to 38%. Among them, the red light quantum well light emitting layer 483 contains a relatively high amount of indium. Due to the protection of the filling layer in the present invention, the red light quantum well light emitting layer 483 of the present invention can still have good light emitting characteristics; moreover, when growing In e Ga 1-e Growing a seventh non-doped GaN film layer 4831 before the N potential well layer 4832 can effectively improve the surface flatness of the film layer and increase the In e Ga 1-eThe growth quality of the N potential well layer 4832 is beneficial to the improvement of the device's luminous brightness; f Ga 1-f An eighth non-doped GaN film layer 4833 is grown before the N barrier layer 4834 to prevent In f Ga 1-f The precipitation of In in the N barrier layer 4834 is beneficial to the improvement of the device's luminous brightness; g Ga 1-g Growing a ninth non-doped GaN film layer 4835 before the N potential well layer 4836 can effectively improve the surface flatness of the film layer and increase the In g Ga 1-g The growth quality of the N potential well layer 4836 is beneficial to the improvement of the luminous brightness of the device; before growing the p-type doped GaN barrier layer 4838, a tenth undoped GaN film layer 4837 is grown.
[0065] The thicknesses of the seventh to tenth non-doped GaN film layers are 1 to 3 nm respectively, and the growth temperature of the seventh non-doped GaN film layer 4831 is about 100 nm. e Ga 1-e The growth temperature of the N potential well layer 4832 is the same as that of the In f Ga 1-f The growth temperature of the N barrier layer 4834 is the same as that of the In g Ga 1-g The growth temperature of the N-type potential well layer 4836 is the same as that of the tenth non-doped GaN film layer 4837, and the growth temperature of the p-type doped GaN barrier layer 4838 is the same, thereby effectively alleviating the problem of wave shift under large current injection. e Ga 1-e The thickness of the N potential well layer is 2.5 to 2.5 nm. f Ga 1-f The thickness of the N barrier layer is 10 to 15 nm. g Ga 1-g The thickness of the N potential well layer is 2.5 to 2.5 nm, the thickness of the p-type doped GaN barrier layer is 10 to 15 nm, and the thickness of the Al h Ga 1-h The thickness of the N layer is 1-2 nm, thus ensuring good luminescence properties of the red light quantum well light-emitting layer 483.
[0066] T8: On the surface of the quantum well light-emitting layer away from the sapphire substrate 10, a non-doped GaN protective layer 49, an electron blocking layer 50, a hole supply layer 51 and an ohmic contact layer 52 are sequentially grown. The structural schematic diagram is shown in FIG. Figure 6 .
[0067] In some embodiments, the thickness of the non-doped GaN protective layer 49 is 15-30 nm. The non-doped GaN protective layer 49 can prevent the precipitation of In on the one hand, and on the other hand, since etching occurs when the nitrogen film-forming atmosphere is switched to the hydrogen atmosphere, the non-doped GaN protective layer 49 can protect the quantum well light-emitting layer.
[0068] In some embodiments, the material of the electron blocking layer 50 is polarization-induced p-type doped AlGaN, the thickness of the electron blocking layer 50 is 50-60 nm, and in the direction away from the sapphire substrate 10, the Al component in the electron blocking layer is linearly gradually changed from 20% to 30% to 0, for example, the Al component in the electron blocking layer is linearly gradually changed from 25% to 0. In this way, due to the high doping activation energy in p-type doped AlGaN, it is difficult to achieve a high hole concentration and low resistivity of the film layer. The present invention selects the polarization-induced p-type doped AlGaN of the above thickness and the linear change of the aluminum component, which can well reduce the differential resistance of the device.
[0069] In some embodiments, the hole supply layer 51 is a single-layer structure of a first p-type doped GaN layer, and the hole concentration is 2×10 17 ~5×10 17 cm -3 , with a thickness of 80 to 160 nm; or, the hole supply layer 51 is a stacked p-type doped Al i Ga 1-i N layer and a second p-type doped GaN layer, wherein the p-type doped Al i Ga 1-i The N layer is arranged close to the electron blocking layer 50, and the hole concentration is 1×10 18 ~3×10 18 cm -3 , p-type doped Al i Ga 1-i The thickness of the N layer is 1.5 to 2.5 nm, and i is 0.15 to 0.25, that is, p-type doped Al i Ga 1-i The Al content in the N layer is 15% to 25%, and the thickness of the second p-type doped GaN layer is 5 to 8 nm. In this way, the hole supply layer 51 is guaranteed to have the best performance, and the light-emitting characteristics of the device are improved.
[0070] In some embodiments, the ohmic contact layer 52 is a single layer structure of a p-type heavily doped GaN layer with a thickness of 10 to 20 nm; or, the ohmic contact layer 52 is a p-type heavily doped In j Ga 1-j N-layer single-layer structure, j is 0.10-0.30, that is, p-type doped In j Ga 1-jThe composition of In in the N layer is 10% to 30%; or the ohmic contact layer is a p-type doped In layer 52 stacked k Ga 1-k N layer and a third p-type doped GaN layer, wherein the p-type doped In k Ga 1-k The N layer is arranged close to the hole supply layer 51, and k is 0.10-0.30, that is, the p-type doped In k Ga 1-k The In content in the N layer is 10% to 30%, and the p-type doped In k Ga 1-k The thickness of the N layer is 105-205 nm, and the thickness of the third p-type doped GaN layer is 5-8 nm. In this way, the ohmic contact layer 52 is guaranteed to have the best performance, and the light-emitting characteristics of the device are improved.
[0071] S400: On the side of the LED device away from the sapphire substrate 10 (i.e., the side of the ohmic contact layer 52 away from the sapphire substrate 10), a conductive film layer 61, a reflector 62, and a binding metal layer 63 are sequentially formed. The structural schematic diagram can be referred to Fig.10 .
[0072] Among them, the material of the conductive film layer 61 can be ITO, and a 20 to 500 nm thick ITO film layer can be deposited as the conductive film layer 61 by electron beam evaporation (EBM) or magnetron sputtering (PVD), and the ITO film layer can be processed by combining the RTA (rapid thermal annealing) process to thereby improve the transmittance of the ITO film layer and reduce the material resistance.
[0073] Furthermore, the reflector 62 may be an Ag reflector. Specifically, the Ag reflector with a thickness of 100 to 300 nm may be deposited by electron beam evaporation (EBM) to improve the light extraction efficiency of the Micro LED chip.
[0074] In addition, the bonding metal layer 63 may be deposited by electron beam evaporation (EBM). In some embodiments, the bonding metal layer 63 includes at least one of Cr, Pt, Ni, Ti, Ni and Ag.
[0075] S500: Binding the pixel driving circuit 64 on the surface of the binding metal layer 63 away from the sapphire substrate 10. The structural diagram can be referred to Fig.10 The pixel driving circuit 64 may be a Si substrate or a Si-based CMOS pixel driving backplane.
[0076] S600: Use laser lift-off technology (LLO) to peel off the sapphire substrate 10 and the filling layer 20. The structural diagram can be referred to Fig.11. Among them, the principle of LLO is: use a high-energy pulsed laser beam to uniformly scan the interface between the sapphire substrate and the GaN epitaxial layer (i.e., the non-doped GaN film 42), and its photon energy is between the sapphire and GaN band gaps. After the GaN film absorbs the photon energy, it decomposes to form liquid Ga and nitrogen, thereby realizing the separation of the sapphire substrate and the non-doped GaN film. In the present invention, by filling the holes of the sapphire substrate with a filling layer containing gallium nitride, the filling layer can play a good protective role on the quantum well light-emitting layer during the laser scanning process: on the one hand, during the laser stripping process, the film thickness of the laser beam from the quantum well light-emitting layer structure increases, so that the laser energy intensity penetrating the film layer to the quantum well light-emitting layer is attenuated, thereby preventing the wavelength blue shift problem caused by the precipitation of In (indium) in the quantum light-emitting layer under the high temperature state of the interface; on the other hand, the overall thickness of the GaN film layer increases, which has a good absorption effect on the laser, and improves the luminescence characteristics of the Micro LED chip to a certain extent.
[0077] According to an embodiment of the present invention, when the sapphire substrate is peeled off by using the laser lift-off technology, the laser wavelength is 355 nm, 266 nm and 248 nm, thereby achieving a better lift-off effect.
[0078] According to an embodiment of the present invention, after the LLO process, the non-doped GaN film 42 and the buffer layer 41 are etched by ICP-RIE until the n-type heavily doped GaN layer 43 is etched, and then the surface of the n-type heavily doped GaN layer 43 is CMP polished. The structural schematic diagram can be referred to Fig.12 .
[0079] According to an embodiment of the present invention, the steps of making a Micro LED chip further include: patterning a sapphire alignment mark, using ICP-RIE to etch InGaN-based RGB three-primary color Micro LED chips with different pixel sizes and different pixel pitches, ensuring that the etched pixel pattern is located in the pattern sapphire substrate area (i.e., in the hole), referring to Fig.13 , and then further wet etching (25% TMAH solution) can be used to repair the etched interface and reduce the point defect density (dangling bonds, etc.); refer to Fig.14, and then use ALD (atomic layer deposition) equipment to deposit a 20-40nm thick sidewall passivation layer 71 or PECVD (plasma enhanced chemical vapor deposition) equipment to deposit an 80-260nm thick sidewall passivation layer 71, and then use PVD or ALD to deposit a DBR (distributed Bragg reflector) reflective film layer 72 to enhance light extraction efficiency; then use photolithography and PECVD equipment to deposit a first passivation film layer 73; then use photolithography and ICP-RIE etching to remove the sidewall passivation layer 71 and DBR reflective film layer 72 on the pixel R, G, B mesa, expose the surface of the pixel R, G, B (the pixel R, G, B in the figure is an n-GaN film layer), and deposit 2 An ITO film layer 74 with a thickness of 0 to 100 nm is formed, and the ITO film layer 74 covers part of the side wall of the DBR reflective film layer 72, and is combined with an RTA process (rapid thermal annealing process) to improve the transmittance of the ITO film layer 74 and reduce the material resistance; then a second passivation film layer 75 is deposited using a photolithography process and a PECVD method, and finally electrical insulation between pixel countertops is achieved; finally, an ICP-RIE etching process, a degumming process, and an EBM (electron beam melting) device are used to deposit an n-type ohmic contact electrode 76 (Ti / Al / Ti / Au and other materials), and then a metal high-reflection electrode (such as Ag or Al and other materials) is deposited, which reduces the light crosstalk and light divergence angle between pixels on the one hand, and improves the light extraction efficiency on the other hand.
[0080] The sidewall passivation layer 71 , the first passivation film layer 73 and the second passivation film layer 75 are made of insulating materials such as silicon nitride or silicon oxide.
[0081] In another aspect of the present invention, the present invention provides a Micro LED chip. According to an embodiment of the present invention, the Micro LED chip is manufactured using the method described above. As a result, the Micro LED chip has good luminous performance. It can be understood by those skilled in the art that the Micro LED chip has all the features and advantages described above, and no further elaboration is given here.
[0082] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0083] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0084] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for manufacturing a Micro LED chip, characterized in that: include: Making a plurality of holes spaced apart from each other on a surface of a sapphire substrate; forming a filling layer in the hole, the filling layer comprising a first aluminum nitride layer, a GaN layer, and a second aluminum nitride layer stacked; An LED device is formed on the surface of the sapphire substrate, wherein the step of forming the LED device includes the step of forming a plurality of quantum well light-emitting layers, wherein the quantum well light-emitting layers include a blue light quantum well light-emitting layer, a green light quantum well light-emitting layer, and a red light quantum well light-emitting layer, wherein the orthographic projection of the effective light-emitting area of the quantum well light-emitting layer on the sapphire substrate is located in the hole, and the blue light quantum well light-emitting layer, the green light quantum well light-emitting layer, and the red light quantum well light-emitting layer all include InGaN; Forming a conductive film layer, a reflector, and a binding metal layer in sequence on a side of the LED device away from the sapphire substrate; Binding a pixel driving circuit on a surface of the binding metal layer away from the sapphire substrate; The sapphire substrate and the filling layer are peeled off using a laser lift-off technique.
2. The method according to claim 1, characterized in that The method for making the hole comprises: forming a protective layer on a surface of the sapphire substrate; The surface of the sapphire substrate is punched on one side of the protective layer by laser drilling to form the hole. Alternatively, the method for making the hole comprises: forming a photoresist layer on one surface of the sapphire substrate, and patterning the photoresist layer to expose a surface of a predetermined area of the sapphire substrate; Etching the sapphire substrate at the predetermined area to form the hole; removing the photoresist layer; The protective layer is formed on the surface of the sapphire substrate where the hole is formed, and a portion of the protective layer corresponding to the hole is removed.
3. The method according to claim 2, characterized in that At least one of the following conditions is also met: The depth of the holes is 2.2 to 4.3 microns; The distance between the center points of two adjacent holes is 2.5 to 10.5 microns; The shape of the hole is at least one of circular, square and rectangular.
4. The method according to claim 3, characterized in that The diameter of the circle is 2 to 10 micrometers; the side length of the square is 2 to 10 micrometers; the long side of the rectangle is 2.2 to 10.2 micrometers, and the short side of the rectangle is 2 to 10 micrometers.
5. The method according to claim 2, characterized in that: The thickness of the protective layer is 200-300 nm.
6. The method according to claim 2, characterized in that The method of forming the filling layer in the hole comprises: Depositing the first aluminum nitride layer on the surface of the protective layer and in the holes; epitaxially growing the GaN layer on a surface of the first aluminum nitride layer away from the sapphire substrate; Depositing the second aluminum nitride layer on a surface of the GaN layer away from the sapphire substrate; The protective layer is removed, and at the same time, the first aluminum nitride layer, the GaN layer and the second aluminum nitride layer located on the surface of the protective layer are removed, Optionally, the filling layer satisfies at least one of the following conditions: The thickness of the first aluminum nitride layer is 0.5 to 1 micron, the thickness of the GaN layer is 1 to 2 microns, and the thickness of the second aluminum nitride layer is 0.5 to 1 micron; The growth temperature of the epitaxial growth of the GaN layer is 1040°C to 1060°C.
7. The method according to claim 1, characterized in that The method for forming the LED device on the surface of the sapphire substrate comprises: Depositing a buffer layer on the surface of the sapphire substrate, wherein the buffer layer covers the filling layer; epitaxially growing a non-doped GaN thin film on a surface of the buffer layer away from the sapphire substrate; epitaxially growing an n-type heavily doped GaN layer on a surface of the non-doped GaN film away from the sapphire substrate; epitaxially growing an n-type lightly doped GaN layer on a surface of the n-type heavily doped GaN layer away from the sapphire substrate; Epitaxially growing a first barrier layer on a surface of the n-type lightly doped GaN layer away from the sapphire substrate; A first superlattice structure layer and a second superlattice structure layer are sequentially grown on a surface of the first barrier layer away from the sapphire substrate, wherein the first superlattice structure layer includes a stacked arrangement of x Ga 1-x N layer and non-doped GaN layer, x is 0.01-0.05, and the second superlattice structure layer includes a stacked In y Ga 1-y N layer and n-type doped GaN layer, y is 0.01 to 0.08; Growing the blue light quantum well light emitting layer, the green light quantum well light emitting layer and the red light quantum well light emitting layer on the surface of the second superlattice structure layer away from the sapphire substrate; A non-doped GaN protection layer, an electron blocking layer, a hole supply layer and an ohmic contact layer are sequentially grown on the surface of the quantum well light emitting layer away from the sapphire substrate.
8. The method according to claim 7, characterized in that The method for forming the blue light quantum well light emitting layer comprises: sequentially growing a first non-doped GaN film layer, an In film layer, and a second non-doped GaN film layer on a surface of the second superlattice structure layer away from the sapphire substrate; a Ga 1-a N potential well layer, second non-doped GaN film layer and In b Ga 1-b N barrier layer, wherein a is 0.18 to 0.21, and b is 0.01 to 0.03; The method for forming the green light quantum well light-emitting layer comprises: sequentially growing a third non-doped GaN film layer, an In film layer, and a second non-doped GaN film layer on a surface of the second superlattice structure layer away from the sapphire substrate; c Ga 1-c N potential well layer, a fourth non-doped GaN film layer and a first n-type doped GaN barrier layer, a fifth non-doped GaN film layer, In d Ga 1-d N potential well layer, a sixth non-doped GaN film layer and a second n-type doped GaN barrier layer, wherein c is 0.24 to 0.25, and d is 0.25 to 0.28; The method for forming the red light quantum well light emitting layer comprises: sequentially growing a seventh non-doped GaN film layer, an In film layer, and a second non-doped GaN film layer on a surface of the second superlattice structure layer away from the sapphire substrate; e Ga 1-e N potential well layer, the eighth non-doped GaN film layer and In f Ga 1-f N barrier layer, ninth undoped GaN film layer, In g Ga 1-g N potential well layer, tenth non-doped GaN film layer, p-type doped GaN barrier layer and Al h Ga 1-h N layer, wherein e is 0.18-0.21, f is 0.01-0.03, g is 0.35-0.38, and h is 0.10-0.
30.
9. The method according to claim 7, characterized in that: The method for forming the LED device further satisfies at least one of the following conditions: The thickness of the buffer layer is 15 to 35 nm; The thickness of the non-doped GaN film is 3-4 μm, and the growth temperature of the epitaxial growth of the non-doped GaN film is 1040° C.-1060° C.; The thickness of the n-type heavily doped GaN layer is 2 to 3 μm, the growth temperature is 1040° C. to 1060° C., and the doping concentration is 2×10 18 ~1×10 19 cm -3 ; The thickness of the n-type lightly doped GaN layer is 0.2-0.5 μm, the growth temperature is 1040° C.-1060° C., and the doping concentration is 1×10 17 ~5×10 17 cm -3 ; The thickness of the first barrier layer is 10-20 nm, and the material is non-doped GaN or In z Ga 1-z N, z is 0.01 to 0.03; In x Ga 1-x The thickness of the N layer is 2-3 nm, and the thickness of the non-doped GaN layer is 10-15 nm; In y Ga 1-y The thickness of the N layer is 2-3 nm, the thickness of the n-type doped GaN layer is 10-15 nm, and the doping concentration is 1×10 17 ~5×10 17 cm -3 .
10. The method according to claim 8, characterized in that The method for forming the LED device further satisfies at least one of the following conditions: The thicknesses of the first to the tenth undoped GaN film layers are 1 to 3 nm respectively; In a Ga 1-a The thickness of the N potential well layer is 2.5 to 3.5 nm. b Ga 1-b The thickness of the N barrier layer is 10 to 15 nm; In c Ga 1-c The thickness of the N potential well layer is 2.5-2.5 nm, the thickness of the first n-type doped GaN barrier layer is 10-15 nm, and the doping concentration of the first n-type doped GaN barrier layer is 1×10 17 ~5×10 17 cm -3 , the In d Ga 1-d The thickness of the N potential well layer is 2.5-2.5 nm, the thickness of the second n-type doped GaN barrier layer is 10-15 nm, and the doping concentration of the second n-type doped GaN barrier layer is 1×10 17 ~5×10 17 cm -3 ; In e Ga 1-e The thickness of the N potential well layer is 2.5 to 2.5 nm. f Ga 1-f The thickness of the N barrier layer is 10 to 15 nm. g Ga 1-g The thickness of the N potential well layer is 2.5-2.5 nm, the thickness of the p-type doped GaN barrier layer is 10-15 nm, and the thickness of the Al h Ga 1-h The thickness of the N layer is 1 to 2 nm.
11. The method according to claim 7, characterized in that The method for forming the LED device further satisfies at least one of the following conditions: The thickness of the non-doped GaN protective layer is 15 to 30 nm; The material of the electron blocking layer is p-type doped AlGaN, the thickness of the electron blocking layer is 50-60 nm, and in the direction away from the sapphire substrate, the Al component in the electron blocking layer linearly changes from 20% to 30% to 0; The hole supply layer is a first p-type doped GaN layer with a hole concentration of 2×10 17 ~5×10 17 cm -3 , with a thickness of 80 to 160 nm, or the hole-providing layer is a stacked p-type doped Al i Ga 1-i N layer and the second p-type doped GaN layer, the hole concentration is 1×10 18 ~3×10 18 cm -3 , the p-type doped Al i Ga 1-i The thickness of the N layer is 1.5 to 2.5 nm, i is 0.15 to 0.25, and the thickness of the second p-type doped GaN layer is 5 to 8 nm; The ohmic contact layer is a p-type heavily doped GaN layer with a thickness of 10 to 20 nm, or the ohmic contact layer is a p-type heavily doped In j Ga 1-j N layer, j is 0.10 to 0.30, or the ohmic contact layer is a stacked p-type doped In k Ga 1-k N layer and a third p-type doped GaN layer, k is 0.10 to 0.30, the p-type doped In k Ga 1-k The thickness of the N layer is 105-205 nm, and the thickness of the third p-type doped GaN layer is 5-8 nm.
12. The method according to any one of claims 1 to 11, characterized in that: When the sapphire substrate is peeled off by the laser lift-off technology, the laser wavelengths are 355nm, 266nm and 248nm.
13. A Micro LED chip, characterized in that: The method is prepared by any one of claims 1 to 12.