Negative pole piece, solid-state battery and electric equipment

By designing the current collector, storage layer and buffer layer in the negative electrode sheet of all solid state batteries, using carbon particles and metal particles of specific proportions and particle sizes, the problems of lithium dendrites and side reactions in lithium-ion batteries are solved, and the problem of lithium ion batteries is improved. Cycling performance and safety of the battery.

CN118899398AActive Publication Date: 2024-11-05XIAMEN HITHIUM ENERGY STORAGE TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310496634.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05
Estimated Expiration
2043-05-05

AI Technical Summary

Technical Problem

In all-solid-state batteries, lithium-ion metal negative electrodes are prone to form lithium dendrites, resulting in poor interface contact, uneven space charge distribution and side reactions, increasing interface impedance, affecting the safety and cycling performance of the battery.

Method used

A negative electrode sheet is designed, including a current collector, a storage layer and a buffer layer, which contains the first carbon particles and the first metal particles, and the buffer layer contains the second carbon particles and the second metal particles, through which the Specific proportions and particle size settings to avoid growth and side reactions of lithium dendrites and optimize the distribution and deposition of lithium ions.

Benefits of technology

This design effectively reduces the generation of lithium dendrites, improves the circulation performance and energy density of the negative electrode sheet, enhances the safety and stability of the battery, and avoids the risk of short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899398A_ABST
    Figure CN118899398A_ABST
Patent Text Reader

Abstract

The invention provides a negative pole piece, a solid-state battery and electric equipment. The negative pole piece comprises a current collector, a storage layer and a buffer layer, the current collector, the storage layer and the buffer layer are sequentially stacked, the storage layer comprises first carbon particles and first metal particles, and the first metal particles are used for storing active ions; the buffer layer comprises second carbon particles and second metal particles, the second metal particles are used for transmitting active ions, the active ions are formed after the active ions and the electrons are combined, the median particle size of the first carbon particles is larger than that of the second carbon particles, and the mass fraction of the first metal particles is larger than that of the second metal particles. The negative pole piece is not easy to generate lithium dendrites to pierce the solid electrolyte, is not easy to generate side reaction with the solid electrolyte, can relieve the volume change of the negative pole piece in the charging and discharging process, and can have excellent cycle performance and relatively high energy density when being applied to the energy storage device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a negative electrode plate, a solid-state battery, and an electrical device. Background Art

[0002] The frequent lithium-ion battery fire and explosion accidents in recent years have made it urgent to solve the safety problems of lithium-ion batteries. Using solid electrolytes to replace flammable organic electrolytes can greatly improve the safety of batteries. Therefore, all-solid-state batteries are considered to be the first choice for the next generation of power batteries. In all-solid-state batteries, lithium-ion metal is used as the negative electrode, and all-solid-state batteries can take into account both high energy density and high safety. However, when lithium metal is used as the negative electrode, during the charging process, the lithium released from the positive electrode is easy to form lithium dendrites at the negative electrode; during the discharge process, the stripping of lithium atoms will cause the existence of interfacial gaps, resulting in poor solid-solid interface contact between the negative electrode and the solid electrolyte, resulting in uneven spatial charge distribution. At the same time, direct contact between the solid electrolyte and lithium metal will also cause side reactions, generate an interfacial side reaction layer, and increase the interface impedance. Lithium dendrites are easily generated during the battery cycle. Lithium dendrites will cause accelerated failure of the battery or even short circuit, causing safety problems. Summary of the invention

[0003] In response to the above problems, an embodiment of the present application provides a negative electrode plate, which is not prone to produce dendrites, is not prone to side reactions with solid electrolytes, can alleviate the volume change of the negative electrode plate during the charging and discharging process, and when applied to an energy storage device, can have both excellent cycle performance and high energy density.

[0004] The first aspect of the present application provides a negative electrode plate, which includes: a current collector, a storage layer and a buffer layer, wherein the current collector, the storage layer and the buffer layer are stacked in sequence, the storage layer includes a plurality of first carbon particles and a plurality of first metal particles, the first metal particles are used to store active ions; the buffer layer includes a plurality of second carbon particles and a plurality of second metal particles, the second metal particles are used to transport active ions, and the active ions are formed after combining with electrons, wherein the median particle size of the first carbon particles is greater than the median particle size of the second carbon particles, and the mass fraction of the first metal particles is greater than the mass fraction of the second metal particles.

[0005] Wherein, the ratio of the mass fraction M1 of the first metal particles in the storage layer to the mass fraction M2 of the second metal particles in the buffer layer is in the range of 1.25≤M1 / M2≤5.

[0006] The mass fraction M1 of the first metal particles in the storage layer is in the range of 20%≤M1≤70%, and the mass fraction M2 of the second metal particles in the buffer layer is in the range of 9%≤M2≤50%.

[0007] Among them, the ratio range of the mass fraction C1 of the first carbon particles in the storage layer to the mass fraction M1 of the first metal particles is: 0.5≤C1 / M1≤3.5; the ratio range of the mass fraction C2 of the second carbon particles in the buffer layer to the mass fraction M2 of the second metal particles is: 1≤C2 / M2≤5.

[0008] Wherein, the ratio of the gram capacity of the second carbon particles to the gram capacity of the first carbon particles is less than or equal to 0.6.

[0009] The median particle size of the first carbon particles is in the range of 2 μm to 50 μm; the median particle size of the second carbon particles is in the range of 10 nm to 500 nm.

[0010] The storage layer has a thickness ranging from 20 μm to 100 μm, and the buffer layer has a thickness ranging from 1 μm to 20 μm.

[0011] Among them, the first metal particles include at least one of Mg, Sn, Ag, In, Zn, Al, Fe, Ga, Sb, Bi, and Au; the second metal particles include at least one of Mg, Sn, Ag, In, Zn, Al, Fe, Ga, Sb, Bi, and Au.

[0012] The first carbon particles include at least one of natural graphite, artificial graphite, hard carbon, soft carbon, and microporous carbon; and the second carbon particles include at least one of acetylene black, Ketjen black, and super carbon black.

[0013] The second aspect of the present application provides a solid-state battery, comprising: a solid electrolyte, a positive electrode plate and the negative electrode plate described in the embodiment of the present application, wherein the positive electrode plate is stacked on the surface of the solid electrolyte, and the negative electrode plate is stacked on the surface of the solid electrolyte away from the positive electrode plate, wherein the buffer layer is arranged between the solid electrolyte and the storage layer.

[0014] A third aspect of the present application provides an electrical device, which includes: an electrical device body and the solid-state battery described in the embodiment of the present application, wherein the solid-state battery is used to supply power to the electrical device body.

[0015] The current collector, storage layer and buffer layer are stacked in sequence, and the buffer layer avoids direct contact between the solid electrolyte and the storage layer, which causes side reactions. The first carbon particles and the first metal particles are arranged in the storage layer. In addition to storing active ions, the first carbon particles also play a role in skeleton support, which alleviates the volume change of the negative electrode plate during the charge and discharge process. When the first carbon particles are graphite and the active ions are lithium ions, the graphite potential after lithium insertion is close to the lithium deposition potential, which is conducive to the deposition of lithium in the storage layer. At the same time, the first metal particles can react with lithium to form an alloy, which can be used as a lithium nucleation site, reducing the lithium deposition interface energy. The first carbon particles and the first metal particles are evenly dispersed, so that multiple evenly dispersed nucleation sites can be constructed in the storage layer, optimizing the distribution and deposition of lithium ions. When the active ion is lithium, the buffer layer has the second metal particles. After the second metal particles are alloyed with lithium, they act as a medium for lithium ion transmission (equivalent to the function of a solid electrolyte), which can assist lithium ions to cross the buffer layer and be transmitted to the storage layer. The median particle size of the first carbon particles is greater than that of the second carbon particles. The median particle size of the second carbon particles is smaller, so that the second carbon particles have a higher lithium deposition interface energy. The void tortuosity formed after the second carbon particles are accumulated is also larger, so that lithium dendrites are not easy to grow along the buffer layer, thereby preventing lithium dendrites from piercing the solid electrolyte and causing a short circuit. The mass fraction of the first metal particles is greater than the mass fraction of the second metal particles. When the active ion is lithium, the lithium deposition interface energy in the storage layer is lower than the lithium deposition interface energy in the buffer layer, and the lithium ions are preferentially deposited in the first storage layer. The negative electrode plate is not easy to produce lithium dendrites piercing the solid electrolyte, is not easy to have side reactions with the solid electrolyte, and can alleviate the volume change of the negative electrode plate during the charge and discharge process. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0017] Figure 1 It is a schematic diagram of the structure of the negative electrode plate of one embodiment of the present application.

[0018] Figure 2 The negative electrode of one embodiment of the present application is along the Figure 1 Schematic diagram of the cross-sectional structure in the AA direction.

[0019] Figure 3 It is a schematic structural diagram of a solid-state battery according to an embodiment of the present application.

[0020] Figure 4A solid-state battery according to an embodiment of the present application Figure 3 Schematic diagram of the cross-sectional structure in the BB direction.

[0021] Figure 5 It is a structural schematic diagram of an electrical equipment according to an embodiment of the present application.

[0022] Description of reference numerals:

[0023] 100 - negative electrode plate, 110 - current collector, 120 - storage layer, 121 - first carbon particles, 122 - first metal particles, 130 - buffer layer, 131 - second carbon particles, 132 - second metal particles, 200 - solid-state battery, 210 - solid-state electrolyte, 220 - positive electrode plate, 300 - electrical equipment, 310 - electrical equipment body. DETAILED DESCRIPTION

[0024] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0025] The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.

[0026] The technical solutions in the embodiments of the present application will be described below in conjunction with the accompanying drawings.

[0027] It should be noted that, for the convenience of explanation, in the embodiments of the present application, the same figure marks represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments.

[0028] The frequent lithium-ion battery fire and explosion accidents in recent years have made it urgent to solve the safety problems of lithium-ion batteries. Using solid electrolytes to replace flammable organic electrolytes can greatly improve the safety of batteries. Therefore, all-solid-state batteries are considered to be the first choice for the next generation of power batteries. In all-solid-state batteries, lithium-ion metal is used as the negative electrode, and all-solid-state batteries can take into account both high energy density and high safety. However, when lithium metal is used as the negative electrode, during the charging process, the lithium released from the positive electrode is easy to form lithium dendrites at the negative electrode; during the discharge process, the stripping of lithium atoms will cause the existence of interfacial gaps, resulting in poor solid-solid interface contact between the negative electrode and the solid electrolyte, resulting in uneven spatial charge distribution. At the same time, direct contact between the solid electrolyte and lithium metal will also cause side reactions, generate an interfacial side reaction layer, and increase the interface impedance. Lithium dendrites are easily generated during the battery cycle. Lithium dendrites will cause accelerated failure of the battery or even short circuit, causing safety problems.

[0029] See also Figure 1 and Figure 2 In a first aspect, an embodiment of the present application provides a negative electrode plate 100, comprising: a current collector 110, a storage layer 120 and a buffer layer 130, wherein the current collector 110, the storage layer 120 and the buffer layer 130 are stacked in sequence, wherein the storage layer 120 comprises a plurality of first carbon particles 121 and a plurality of first metal particles 122, wherein the first metal particles 122 are used to store active ions; wherein the buffer layer 130 comprises a plurality of second carbon particles 131 and a plurality of second metal particles 132, wherein the second metal particles 132 are used to transport active ions, wherein the active ions are formed after combining with electrons, wherein the median particle size of the first carbon particles 121 is greater than the median particle size of the second carbon particles 131, and the mass fraction of the first metal particles 122 is greater than the mass fraction of the second metal particles 132.

[0030] It can be understood that the current collector 110 , the storage layer 120 and the buffer layer 130 are stacked in sequence, that is, the storage layer 120 is arranged on the surface of the current collector 110 , and the buffer layer 130 is arranged on the surface of the storage layer 120 away from the current collector 110 .

[0031] It is understandable that the active ions may be, but are not limited to, lithium ions, sodium ions, etc. The lithium ions combine with electrons to form lithium atoms, and the sodium ions combine with electrons to form sodium atoms.

[0032] It is understandable that when active ions are stored in the first metal particles 122 , the active ions receive electrons to form atoms and are alloyed with the first metal particles 122 to form alloys, thereby achieving storage of active ions in the first metal particles 122 .

[0033] It can be understood that the plurality of first carbon particles 121 and the plurality of first metal particles 122 are uniformly dispersed in the storage layer 120 , and the plurality of second carbon particles 131 and the plurality of second metal particles 132 are uniformly dispersed in the buffer layer 130 .

[0034] The current collector 110, the storage layer 120 and the buffer layer 130 are stacked in sequence, and the buffer layer 130 prevents the solid electrolyte 210 from directly contacting the storage layer 120 and causing side reactions. The first carbon particles 121 and the first metal particles 122 are arranged in the storage layer 120. In addition to storing active ions, the first carbon particles 121 also play a role in skeleton support, which alleviates the volume change of the negative electrode plate 100 during the charge and discharge process; when the first carbon particles 121 are graphite and the active ions are lithium ions, the graphite potential after lithium insertion is close to the lithium deposition potential, which is conducive to the deposition of lithium in the storage layer 120. When the active ion is lithium, the first metal particles 122 can react with lithium to form an alloy, and can serve as a lithium nucleation site, reducing the lithium deposition interface energy; the first carbon particles 121 and the first metal particles 122 are uniformly dispersed, so that multiple uniformly dispersed nucleation sites can be constructed in the storage layer 120, optimizing the distribution and deposition of lithium ions. When the active ion is lithium, the buffer layer 130 has the second metal particles 132. After the second metal particles 132 are alloyed with lithium, they act as a medium for lithium ion transmission (equivalent to the function of the solid electrolyte 210), which can assist lithium ions to cross the buffer layer 130 and be transmitted to the storage layer 120. The median particle size of the first carbon particles 121 is larger than the median particle size of the second carbon particles 131. The median particle size of the second carbon particles 131 is smaller, so it has a higher lithium deposition interface energy, and the void tortuosity formed after the second carbon particles 131 are accumulated is also larger, so that lithium dendrites are not easy to grow along the buffer layer 130, preventing lithium dendrites from piercing the solid electrolyte 210 and causing a short circuit. The mass fraction of the first metal particles 122 is greater than the mass fraction of the second metal particles 132. When the active ion is lithium, the lithium deposition interface energy in the storage layer 120 is lower than the lithium deposition interface energy in the buffer layer 130, and the lithium ions are preferentially deposited in the first storage layer 120. The negative electrode plate 100 is not prone to lithium dendrites piercing the solid electrolyte 210, is not prone to side reactions with the solid electrolyte 210, and can alleviate the volume change of the negative electrode plate 100 during the charge and discharge process.

[0035] It should be noted that, for the convenience of description, the active ions are mostly described as lithium ions in the embodiments.

[0036] In some embodiments, the porosity of the storage layer 120 ranges from 30% to 50%.

[0037] In the embodiments of the present application, when a numerical value range from a to b is involved, unless otherwise specified, it means that the numerical value can be any numerical value between a and b, including the endpoint numerical value a and the endpoint numerical value b.

[0038] Specifically, the porosity of the storage layer 120 may be 30%, 35%, 40%, 45%, 50%, and any value in between.

[0039] When the porosity of the storage layer 120 is less than 30%, the deposition space of active ions is reduced, resulting in a decrease in the energy density of the solid-state battery 200. When the porosity of the storage layer 120 is greater than 50%, the electrochemical impedance of the storage layer 120 increases, affecting the cycle performance of the solid-state battery 200. When the porosity of the storage layer 120 is between 30% and 50%, the solid-state battery 200 can have both high energy density and excellent cycle performance.

[0040] In some embodiments, the ratio of the mass fraction M1 of the first metal particles 122 in the storage layer 120 to the mass fraction M2 of the second metal particles 132 in the buffer layer 130 is in the range of 1.25≤M1 / M2≤5.

[0041] It can be understood that the mass fraction M1 of the first metal particles 122 in the storage layer 120 refers to the percentage of the mass of the first metal particles 122 in the storage layer 120 to the total mass of the storage layer 120; the mass fraction M2 of the second metal particles 132 in the buffer layer 130 refers to the percentage of the mass of the first metal particles 122 in the buffer layer 130 to the total mass of the buffer layer 130.

[0042] Specifically, the ratio of the mass fraction M1 of the first metal particles 122 in the storage layer 120 to the mass fraction M2 of the second metal particles 132 in the buffer layer 130 may be 1.25, 2, 3, 4, 5, and any value in between.

[0043] When the ratio of the mass fraction M1 of the first metal particles 122 in the storage layer 120 to the mass fraction M2 of the second metal particles 132 in the buffer layer 130 is less than 1.25, when the active ions are lithium ions, the lithium ions will also be deposited in the buffer layer 130, and lithium dendrites will easily grow along the buffer layer 130. The lithium dendrites will easily pierce the solid electrolyte 210, causing a short circuit. When the ratio of the mass fraction M1 of the first metal particles 122 in the storage layer 120 to the mass fraction M2 of the second metal particles 132 in the buffer layer 130 is greater than 5, the second metal particles 132 cannot help the active ions cross the buffer layer 130, resulting in the active ions being deposited in the buffer layer 130. When the ratio of the mass fraction M1 of the first metal particles 122 in the storage layer 120 to the mass fraction M2 of the second metal particles 132 in the buffer layer 130 is between 1.25 and 5, the active ions are not easily deposited in the buffer layer 130, but can help the active ions cross the buffer layer 130, so that the lithium ions are deposited in the storage layer 120.

[0044] In some embodiments, the mass fraction M1 of the first metal particles 122 in the storage layer 120 is in the range of 20%≤M1≤70%. Specifically, the mass fraction of the first metal particles 122 in the storage layer 120 can be 20%, 30%, 40%, 50%, 60%, 70%, and any value therebetween.

[0045] When the mass fraction of the first metal particles 122 in the storage layer 120 is less than 20%, the first metal particles 122 cannot construct multiple uniformly dispersed nucleation sites in the storage layer 120, and cannot optimize the distribution and deposition of active ions. When the mass fraction of the first metal particles 122 in the storage layer 120 is greater than 70%, the storage layer 120 cannot alleviate the volume change of the negative electrode plate 100 during the charge and discharge process. When the mass fraction of the first metal particles 122 in the storage layer 120 is between 20% and 70%, the first metal particles 122 can construct multiple uniformly dispersed nucleation sites in the storage layer 120, optimize the distribution and deposition of active ions, and the storage layer 120 can alleviate the volume change of the negative electrode plate 100 during the charge and discharge process.

[0046] In some embodiments, the mass fraction M2 of the second metal particles 132 in the buffer layer 130 is in the range of 9%≤M2≤50%. Specifically, the mass fraction of the second metal particles 132 in the buffer layer 130 can be 9%, 10%, 20%, 30%, 40%, 50%, and any value therebetween.

[0047] When the mass fraction of the second metal particles 132 in the buffer layer 130 is less than 9%, the second metal particles 132 cannot help the active ions to cross the buffer layer 130, so that the active ions are deposited in the buffer layer 130. When the mass fraction of the second metal particles 132 in the buffer layer 130 is greater than 50%, when the active ions are lithium ions, the lithium ions will also be deposited in the buffer layer 130, and lithium dendrites are likely to grow along the buffer layer 130. Lithium dendrites are likely to pierce the solid electrolyte 210, causing a short circuit. When the mass fraction of the second metal particles 132 in the buffer layer 130 is between 9% and 50%, when the active ions are lithium ions, the second metal particles 132 can both help lithium ions to cross the buffer layer 130, so that lithium ions are deposited in the storage layer 120, and can prevent lithium ions from being deposited in the buffer layer 130.

[0048] In some embodiments, the ratio of the mass fraction C1 of the first carbon particles 121 to the mass fraction M1 of the first metal particles 122 in the storage layer 120 is in the range of 0.5≤C1 / M1≤3.5.

[0049] It can be understood that the mass fraction C1 of the first carbon particles 121 in the storage layer 120 refers to the percentage of the mass of the first carbon particles 121 in the storage layer 120 to the total mass of the storage layer 120 .

[0050] Specifically, the ratio of the mass fraction C1 of the first carbon particles 121 to the mass fraction M1 of the first metal particles 122 may be 0.5, 1, 2, 3, 3.5, and any value in between.

[0051] When the ratio of the mass fraction C1 of the first carbon particles 121 to the mass fraction M1 of the first metal particles 122 is less than 0.5, the first carbon particles 121 are less and cannot alleviate the volume change of the negative electrode plate 100 during the charge and discharge process. When the ratio of the mass fraction C1 of the first carbon particles 121 to the mass fraction M1 of the first metal particles 122 is greater than 3.5, the first metal particles 122 cannot construct a plurality of uniformly dispersed nucleation sites in the storage layer 120, and cannot optimize the distribution and deposition of active ions, resulting in a lower cycle capacity retention rate of the solid-state battery 200. When the ratio of the mass fraction C1 of the first carbon particles 121 to the mass fraction M1 of the first metal particles 122 is between 0.5 and 3.5, the first metal particles 122 can both construct a plurality of uniformly dispersed nucleation sites in the storage layer 120, optimize the distribution and deposition of active ions, and the storage layer 120 can alleviate the volume change of the negative electrode plate 100 during the charge and discharge process.

[0052] In some embodiments, the ratio of the mass fraction C2 of the second carbon particles 131 to the mass fraction M2 of the second metal particles 132 in the buffer layer is in the range of 1≤C2 / M2≤5.

[0053] It can be understood that the mass fraction C2 of the second carbon particles 131 in the buffer layer 130 refers to the percentage of the mass of the second carbon particles 131 in the buffer layer 130 to the total mass of the buffer layer 130 .

[0054] Specifically, the ratio of the mass fraction C2 of the second carbon particles 131 to the mass fraction M2 of the second metal particles 132 may be 1, 2, 3, 4, 5, and any value in between.

[0055] When the ratio of the mass fraction C2 of the second carbon particles 131 to the mass fraction M2 of the second metal particles 132 is less than 1, when the active ions are lithium ions, the lithium ions will also be deposited in the buffer layer 130, and lithium dendrites are easy to grow along the buffer layer 130, and lithium dendrites are easy to pierce the solid electrolyte 210, causing a short circuit. When the ratio of the mass fraction C2 of the second carbon particles 131 to the mass fraction M2 of the second metal particles 132 is greater than 5, the second metal particles 132 cannot help the active ions cross the buffer layer 130, resulting in the active ions being deposited on the surface of the buffer layer 130, resulting in the generation of lithium dendrites, deteriorating the cycle performance, and even causing the solid-state battery 200 to short-circuit. When the ratio of the mass fraction C2 of the second carbon particles 131 to the mass fraction M2 of the second metal particles 132 is between 1 and 5, when the active ions are lithium ions, the second metal particles 132 can both help the lithium ions cross the buffer layer 130, resulting in the lithium ions being deposited in the buffer layer 130, and can prevent the lithium ions from being deposited in the buffer layer 130.

[0056] In some embodiments, a ratio of the gram capacity of the second carbon particles 131 to the gram capacity of the first carbon particles 121 is less than or equal to 0.6.

[0057] When the ratio of the gram capacity of the second carbon particles 131 to the gram capacity of the first carbon particles 121 is less than or equal to 0.6, when the active ions are lithium ions, it is more difficult for lithium ions to embed in the second carbon particles 131, and lithium dendrites will not grow along the buffer layer 130, thereby improving the safety of the solid-state battery 200.

[0058] In some embodiments, the gram capacity of the first carbon particles 121 is greater than or equal to 180 mAh / g, and the gram capacity of the second carbon particles 131 is less than or equal to 100 Ah / g.

[0059] When the gram capacity of the first carbon particles 121 is greater than or equal to 180mAh / g, and the gram capacity of the second carbon particles 131 is less than or equal to 100Ah / g, when the active ions are lithium ions, the lithium ions are easier to be embedded in the first carbon particles 121, which can improve the energy density of the solid-state battery 200 using the negative electrode plate 100. It is difficult for the lithium ions to be embedded in the second carbon particles 131, and lithium dendrites will not grow along the buffer layer 130, thereby improving the safety of the solid-state battery 200.

[0060] In some embodiments, the gram capacity of the first carbon particles 121 is 180 mAh / g to 372 mAh / g. Specifically, the gram capacity of the first carbon particles 121 can be, but is not limited to, 180 mAh / g, 200 mAh / g, 220 mAh / g, 240 mAh / g, 260 mAh / g, 280 mAh / g, 300 mAh / g, 320 mAh / g, 340 mAh / g, 360 mAh / g, 372 mAh / g, and any values ​​therebetween.

[0061] When the gram capacity of the first carbon particles 121 is less than 180 mAh / g, the gram capacity of the first carbon particles 121 is too small, resulting in a decrease in the energy density of the solid-state battery 200. The gram capacity of the first carbon particles 121 is difficult to be greater than 372 mAh / g, and the gram capacity of the first carbon particles 121 is too large, which is difficult to achieve with existing materials. When the gram capacity of the first carbon particles 121 is 180 mAh / g to 372 mAh / g, the energy density of the solid-state battery 200 can be increased as much as possible under existing materials.

[0062] Optionally, the gram capacity of the second carbon particles 131 may also be 0 mAh / g. It can be understood that the gram capacity of the second carbon particles 131 ranges from 0 to 100 Ah / g. Specifically, the gram capacity of the second carbon particles 131 may be, but is not limited to, 0 mAh / g, 10 mAh / g, 20 mAh / g, 30 mAh / g, 40 mAh / g, 50 mAh / g, 60 mAh / g, 70 mAh / g, 80 mAh / g, 90 mAh / g, 100 mAh / g, and any value between the above values.

[0063] When the gram capacity of the second carbon particles 131 is 0 mAh / g and the active ions are lithium ions, the lithium ions will not be embedded in the second carbon particles 131 and lithium dendrites will not grow along the buffer layer 130 , thereby improving the safety of the solid-state battery 200 .

[0064] In some embodiments, the first carbon particles 121 are first intercalated with lithium to obtain C6Li x In the embodiment, x is 0.5 to 1; the first carbon particle 121 firstly inserts lithium to obtain C6Li y, the y value is less than 0.5.

[0065] When the first carbon particle 121 is firstly intercalated with lithium to obtain C6Li x In the embodiment, x is 0.5 to 1; the first carbon particle 121 firstly inserts lithium to obtain C6Li y When the y value is less than 0.5, the lithium ions are more likely to be embedded in the first carbon particles 121, which can improve the energy density of the solid-state battery 200 using the negative electrode plate 100. The lithium ions are less likely to be embedded in the second carbon particles 131, and the lithium dendrites will not grow along the buffer layer 130, thereby improving the safety of the solid-state battery 200.

[0066] In some embodiments, the ratio of the median particle size of the second carbon particles 131 to the median particle size of the first carbon particles 121 ranges from 0.0005 to 0.03. Specifically, the ratio of the median particle size of the second carbon particles 131 to the median particle size of the first carbon particles 121 can be 0.0005, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.02, 0.03, and any value in between.

[0067] When the ratio of the median particle size of the second carbon particles 131 to the median particle size of the first carbon particles 121 is less than 0.0005, the porosity of the buffer layer 130 is low, and when the active ions are lithium ions, it is difficult for lithium ions to pass through the buffer layer 130. When the ratio of the median particle size of the second carbon particles 131 to the median particle size of the first carbon particles 121 is greater than 0.03, it is not easy to control the thickness of the interface buffer layer 130, and it is also impossible to greatly improve the tortuosity of the buffer layer 130, and the effect of inhibiting the penetration growth of lithium dendrites is not obvious. The specific surface area of ​​the second carbon particles 131 is small, and the contact area between the solid electrolyte 210 and the storage layer 120 cannot be increased. When the ratio of the median particle size of the second carbon particles 131 to the median particle size of the first carbon particles 121 is between 0.0005 and 0.03, the lithium ions can easily pass through the buffer layer 130, and the thickness of the interface buffer layer 130 can be easily controlled. The tortuosity of the buffer layer 130 can also be significantly improved, and the penetration growth of lithium dendrites can be inhibited. The second carbon particles 131 have a large specific surface area, which can increase the contact area between the solid electrolyte 210 and the storage layer 120.

[0068] In some embodiments, the median particle size of the first carbon particles 121 is in a range of 2 μm to 20 μm.

[0069] Specifically, the median particle size of the first carbon particles 121 may be 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, and any value in between.

[0070] It can be understood that the median particle size refers to the particle size corresponding to when the cumulative particle size distribution percentage of the sample reaches 50%.

[0071] When the median particle size of the first carbon particles 121 is less than 2 μm, the porosity of the storage layer 120 is low, resulting in a reduction in the deposition space of active ions, affecting the energy density of the solid-state battery 200. When the median particle size of the first carbon particles 121 is greater than 20 μm, the kinetic properties of the active ions are affected, and it is not easy to control the thickness of the lithium storage layer, affecting the energy density and cycle performance of the solid-state battery 200. When the median particle size of the first carbon particles 121 is between 2 μm and 20 μm, the porosity of the storage layer 120 is high, which can take into account both the high energy density and good cycle performance of the solid-state battery 200.

[0072] Furthermore, the median particle size of the first carbon particles 121 is in a range of 3 μm to 10 μm.

[0073] When the median particle size of the first carbon particles 121 is between 3 μm and 10 μm, it is possible to further take into account both the high energy density and good cycle performance of the solid-state battery 200 .

[0074] In some embodiments, the median particle size of the second carbon particles 131 is in a range of 10 nm to 500 nm.

[0075] Specifically, the median particle size of the second carbon particles 131 may be 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, and any value in between.

[0076] When the median particle size of the second carbon particles 131 is less than 10 nm, the porosity of the buffer layer 130 is low, and when the active ions are lithium ions, it is difficult for the lithium ions to pass through the buffer layer 130. When the median particle size of the second carbon particles 131 is greater than 500 nm, it is not easy to control the thickness of the interface buffer layer 130, and it is also impossible to greatly improve the tortuosity of the buffer layer 130, and the effect of inhibiting the penetration growth of lithium dendrites is not obvious. The specific surface area of ​​the second carbon particles 131 is small, and the contact area between the solid electrolyte 210 and the storage layer 120 cannot be increased. When the median particle size of the second carbon particles 131 is between 10 nm and 500 nm, lithium ions can easily pass through the buffer layer 130, it is easy to control the thickness of the interface buffer layer 130, and the tortuosity of the buffer layer 130 can also be significantly improved, and the penetration growth of lithium dendrites can be inhibited. The specific surface area of ​​the second carbon particles 131 is large, and the contact area between the solid electrolyte 210 and the storage layer 120 can be increased.

[0077] Further, the median particle size of the second carbon particles 131 ranges from 10 nm to 100 nm. Specifically, the median particle size of the second carbon particles 131 can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, and any value in between.

[0078] When the median particle size of the second carbon particles 131 is in the range of 10 nm to 100 nm, it is easier to control the thickness of the interface buffer layer 130, and the tortuosity of the buffer layer 130 can be greatly improved. When the active ions are lithium ions, the penetration growth of lithium dendrites is inhibited. The second carbon particles 131 have a large specific surface area, which can significantly increase the contact area between the solid electrolyte 210 and the storage layer 120.

[0079] In some embodiments, the first carbon particles 121 include at least one of natural graphite, artificial graphite, hard carbon, soft carbon, and microporous carbon.

[0080] When the first carbon particles 121 include at least one of natural graphite, artificial graphite, hard carbon, soft carbon, and micron porous carbon, the first carbon particles 121 can not only store active ions but also play a skeleton support role to alleviate the volume change of the negative electrode plate 100 during the charge and discharge process.

[0081] In some embodiments, the second carbon particles 131 include at least one of acetylene black, Ketjen black, and super carbon black (ie, Super P carbon black).

[0082] It can be understood that the super carbon black is Super P carbon black.

[0083] When the second carbon particles 131 include at least one of acetylene black, Ketjen black, and super carbon black (i.e., Super P carbon black), lithium will not be embedded in the second carbon particles 131, and the tortuosity of the voids formed after stacking is also large. When the active ions are lithium ions, lithium dendrites are not easy to grow along this layer, thereby preventing lithium dendrites from piercing the solid electrolyte 210 and causing a short circuit.

[0084] In some embodiments, the thickness of the storage layer 120 is greater than the thickness of the buffer layer 130 .

[0085] When the thickness of the storage layer 120 is greater than the thickness of the buffer layer 130, when the active ions are lithium ions, the lithium ions can easily enter the storage layer 120 through the buffer layer 130, and the lithium insertion capacity of the negative electrode plate 100 can also be increased, and the solid-state battery 200 has a higher energy density.

[0086] In some embodiments, the storage layer 120 has a thickness ranging from 20 μm to 100 μm.

[0087] Specifically, the thickness of the storage layer 120 can be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, and any value in between.

[0088] When the thickness of the storage layer 120 is less than 20 μm, the energy density of the solid-state battery 200 is greatly reduced when the negative electrode plate 100 is applied to the solid-state battery 200. When the thickness of the storage layer 120 is greater than 100 μm, the electrochemical impedance of the solid-state battery 200 increases when the negative electrode plate 100 is applied to the solid-state battery 200, affecting the cycle performance of the solid-state battery 200. When the thickness of the storage layer 120 is between 20 μm and 100 μm, the solid-state battery 200 can take into account both high energy density and good cycle performance.

[0089] Further, the thickness of the storage layer 120 ranges from 30 μm to 50 μm. Specifically, the thickness of the storage layer 120 can be 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, and any value in between.

[0090] When the thickness of the storage layer 120 is in a range of 30 μm to 50 μm, the solid-state battery 200 can further achieve both high energy density and good cycle performance.

[0091] In some embodiments, the thickness of the buffer layer 130 ranges from 1 μm to 20 μm. Specifically, the thickness of the buffer layer 130 can be 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, and any value in between.

[0092] When the thickness of the buffer layer 130 is less than 1 μm, the buffer layer 130 is prone to cracking during the cycle of the solid-state battery 200, affecting the protection effect of the storage layer 120. When the thickness of the buffer layer 130 is greater than 20 μm, the transmission path of the active ions in the buffer layer 130 will be extended, increasing the internal resistance of the solid-state battery 200. When the thickness of the buffer layer 130 is between 1 μm and 20 μm, the buffer layer 130 is not easy to crack during the cycle of the solid-state battery 200, nor will it significantly extend the transmission path of the active ions in the buffer layer 130.

[0093] Furthermore, the thickness of the buffer layer 130 is in a range of 5 μm to 15 μm.

[0094] When the thickness of the buffer layer 130 is between 5 μm and 15 μm, the buffer layer 130 is less likely to crack during the cycle of the solid-state battery 200 , and the transmission path of active ions in the buffer layer 130 will not be significantly prolonged.

[0095] In some embodiments, the first metal particles 122 include at least one of Mg, Sn, Ag, In, Zn, Al, Fe, Ga, Sb, Bi, and Au.

[0096] When the first metal particles 122 include at least one of Mg, Sn, Ag, In, Zn, Al, Fe, Ga, Sb, Bi, and Au, and the active ions are lithium ions, the first metal particles 122 can become lithium nucleation sites, thereby reducing the lithium deposition interface energy.

[0097] In some embodiments, the second metal particles 132 include at least one of Mg, Sn, Ag, In, Zn, Al, Fe, Ga, Sb, Bi, and Au.

[0098] When the second metal particles 132 include at least one of Mg, Sn, Ag, In, Zn, Al, Fe, Ga, Sb, Bi, and Au, and the active ions are lithium ions, the second metal particles 132 can alloy with lithium to assist the lithium ions to cross the buffer layer 130, so that the lithium ions are deposited in the storage layer 120.

[0099] In some embodiments, the median particle size of the first metal particles 122 is 1 nm to 500 nm. Specifically, the median particle size of the first metal particles 122 can be 1 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, and any value in between.

[0100] When the median particle size of the first metal particles 122 is less than 1 nm, the manufacturing cost of the first metal particles 122 is too high. When the median particle size of the first metal particles 122 is greater than 500 nm, the kinetics of the reaction between the first metal particles 122 and the active ions is slow, and the first metal particles 122 are also difficult to be evenly distributed in the storage layer 120. When the median particle size of the first metal particles 122 is between 1 nm and 500 nm, the kinetics of the reaction between the first metal particles 122 and the active ions is fast, and the first metal particles 122 can also be more easily and evenly distributed in the storage layer 120.

[0101] Further, the median particle size of the first metal particles 122 is 10 nm to 100 nm. Specifically, the median particle size of the first metal particles 122 can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, and any value in between.

[0102] When the median particle size of the first metal particles 122 is between 10 nm and 500 nm, the kinetics of the reaction between the first metal particles 122 and the active ions is faster, and the first metal particles 122 can be more easily and evenly distributed in the storage layer 120 .

[0103] In some embodiments, the median particle size of the second metal particles 132 is 1 nm to 500 nm. Specifically, the median particle size of the second metal particles 132 can be 1 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, and any value in between.

[0104] When the median particle size of the second metal particles 132 is less than 1 nm, the manufacturing cost of the second metal particles 132 is too high. When the median particle size of the second metal particles 132 is greater than 500 nm, the second metal particles 132 cannot quickly conduct active ions to the storage layer 120, and the second metal particles 132 are also difficult to be evenly distributed in the buffer layer 130. When the active ions are lithium ions, lithium dendrites are generated. When the median particle size of the second metal particles 132 is between 1 nm and 500 nm, the second metal particles 132 can quickly conduct active ions to the storage layer 120, and the second metal particles 132 are also easy to be evenly distributed in the buffer layer 130.

[0105] Furthermore, the median particle size of the second metal particles 132 is 10 nm to 100 nm. Specifically, the median particle size of the second metal particles 132 can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, and any value in between.

[0106] When the median particle size of the second metal particles 132 is between 10 nm and 100 nm, the second metal particles 132 can quickly conduct active ions to the storage layer 120 , and the second metal particles 132 are also more easily and evenly distributed in the buffer layer 130 .

[0107] In some embodiments, the storage layer 120 also includes a first binder, which is at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF HFP), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN), polyacrylic acid (PAA), polyamide (PI), carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), sodium alginate (Alg), and polyethylene oxide (PEO).

[0108] When the storage layer 120 further includes a first binder, the first carbon particles 121 and the first metal particles 122 are not easy to fall off.

[0109] In some embodiments, the mass fraction of the first binder in the storage layer 120 ranges from 0.1% to 10%.

[0110] When the mass fraction of the first binder is less than 0.1%, the first carbon particles 121 and the first metal particles 122 are easier to fall off. When the mass fraction of the first binder is greater than 10%, when the storage layer 120 is applied to the solid-state battery 200, the energy density of the solid-state battery 200 is low. When the mass fraction of the first binder is between 0.1% and 10%, the first carbon particles 121 and the first metal particles 122 are not easy to fall off, and when the storage layer 120 is applied to the solid-state battery 200, the energy density of the solid-state battery 200 will not be significantly reduced.

[0111] In some embodiments, the buffer layer 130 also includes a second binder, which is at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF HFP), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN), polyacrylic acid (PAA), polyamide (PI), carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), sodium alginate (Alg), and polyethylene oxide (PEO).

[0112] When the buffer layer 130 further includes a second binder, the second carbon particles 131 and the second metal particles 132 are not easy to fall off.

[0113] In some embodiments, the mass fraction of the second binder in the buffer layer 130 is in a range of 0.1% to 10%.

[0114] When the mass fraction of the second binder is less than 0.1%, the second carbon particles 131 and the second metal particles 132 are easier to fall off. When the mass fraction of the second binder is greater than 10%, when the buffer layer 130 is applied to the solid-state battery 200, the energy density of the solid-state battery 200 is low. When the mass fraction of the second binder is between 0.1% and 10%, the second carbon particles 131 and the second metal particles 132 are not easy to fall off, and when the buffer layer 130 is applied to the solid-state battery 200, the energy density of the solid-state battery 200 will not be significantly reduced.

[0115] See also Figure 3 and Figure 4 The embodiment of the present application provides a solid-state battery 200, which includes: a solid electrolyte 210, a positive electrode plate 220 and the negative electrode plate 100 described in the embodiment of the present application, wherein the positive electrode plate 220 is stacked on the surface of the solid electrolyte 210, and the negative electrode plate 100 is stacked on the surface of the solid electrolyte 210 away from the positive electrode plate 220, wherein the buffer layer 130 is arranged between the solid electrolyte 210 and the storage layer 120.

[0116] In some embodiments, the solid electrolyte 210 may be at least one of a ceramic oxide having a garnet structure, a ceramic oxide having a perovskite structure, a NaSICON-type ceramic electrolyte, a LiPON solid electrolyte 210 , and a sulfide-type solid electrolyte 210 .

[0117] The present application is further described below in conjunction with the examples. It should be understood that the examples provided in the present application are only to help understand the present application and should not be regarded as specific limitations of the present application.

[0118] For ease of understanding, the present application lists the following examples. Those skilled in the art should understand that if no specific conditions are specified in the examples, the conventional conditions shall be followed.

[0119] Example 1 to Example 17

[0120] (1) Preparation of composite storage layer 120:

[0121] The first carbon particles 121 and the first metal particles 122 are ball-milled in a certain ratio, and mixed with 5wt% polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) at a speed of 1200r / min for 6 hours. The mixture is coated on a stainless steel substrate by a doctor blade method, vacuum dried at 80°C for 2 hours, and then rolled to obtain a composite layer of the storage layer 120 and the current collector 110. The particle sizes and ratios of the first carbon particles 121 and the first metal particles 122 in Examples 1 to 17 are shown in Tables 1 and 2.

[0122] (2) Preparation of interface buffer layer 130:

[0123] The second carbon particles 131 and the second metal particles 132 are mixed in a certain proportion, and then 5wt% polyvinylidene fluoride (PVDF) is added to the N-methylpyrrolidone (NMP) solution, and stirred at a speed of 1200r / min for 6 hours. The storage layer 120 is coated by a scraping method, and vacuum dried at 80°C for 2 hours to obtain the negative electrode sheet 100. The particle size and ratio of the second carbon particles 131 and the second metal particles 132 in Examples 1 to 17 are shown in Tables 1 and 2.

[0124] (3) Preparation of positive electrode powder:

[0125] NCM622 positive electrode particles, LiPSCl, and acetylene black were mixed in a mass ratio of 55:42:3, wherein the mass of NCM622 active material was about 10 mg, and ground evenly to obtain positive electrode powder.

[0126] (4) Assembly of 200 solid-state batteries:

[0127] The composite layer of the storage layer 120 and the current collector 110 is cut into discs with a diameter of 10 mm, placed in a solid-state battery 200 mold with a 10 mm aperture, 100 mg of LiPSCl electrolyte powder is added, and 1 ton of pressure is applied for pre-pressing; then, the positive electrode powder is added, and 2.5 tons of pressure is applied to finally obtain the solid-state batteries 200 of Examples 1 to 17.

[0128] Embodiment 18

[0129] (1) Preparation of composite storage layer 120:

[0130] The first carbon particles 121 and the first metal particles 122 are ball-milled in a certain ratio, and mixed with 5wt% sodium alginate in N-methylpyrrolidone (NMP) at a speed of 1200r / min for 6 hours. The mixture is coated on a stainless steel substrate by a doctor blade method, vacuum dried at 80°C for 2 hours, and then rolled to obtain a composite layer of a storage layer 120 and a current collector 110. The particle sizes and ratios of the first carbon particles 121 and the first metal particles 122 in Example 18 are shown in Tables 1 and 2.

[0131] (2) Preparation of interface buffer layer 130:

[0132] The second carbon particles 131 and the second metal particles 132 are mixed in a certain proportion, and then 5wt% sodium alginate is added to the N-methylpyrrolidone (NMP) solution, and stirred at a speed of 1200r / min for 6 hours. The storage layer 120 is coated by a scraping method, and vacuum dried at 80°C for 2 hours to obtain the negative electrode sheet 100. The particle size and ratio of the second carbon particles 131 and the second metal particles 132 in Example 18 are shown in Tables 1 and 2.

[0133] (3) Preparation of positive electrode powder: The preparation method of the positive electrode powder is the same as that of Example 1.

[0134] (4) Assembly of solid-state battery 200: The assembly method of solid-state battery 200 is the same as that of Example 1.

[0135] Comparative Example 1

[0136] (1) Preparation of composite storage layer 120:

[0137] The first carbon particles 121 and the first metal particles 122 were ball-milled in a certain ratio, and mixed with 5wt% polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) at a speed of 1200r / min for 6 hours. The mixture was coated on a stainless steel substrate by a doctor blade method, vacuum dried at 80°C for 2 hours, and then rolled to obtain a composite layer of a storage layer 120 and a current collector 110. The particle size and ratio of the first carbon particles 121 and the first metal particles 122 in Comparative Example 1 are shown in Table 1.

[0138] (2) Preparation of positive electrode powder:

[0139] NCM622 positive electrode particles, LiPSCl, and acetylene black were mixed in a mass ratio of 55:42:3, wherein the mass of NCM622 active material was about 10 mg, and ground evenly to obtain positive electrode powder.

[0140] (3) Assembly of 200 solid-state batteries:

[0141] The composite layer of the storage layer 120 and the current collector 110 is cut into discs with a diameter of 10 mm, placed in a solid-state battery 200 mold with a 10 mm aperture, 100 mg of LiPSCl electrolyte powder is added, and 1 ton of pressure is applied for pre-pressing; then, the positive electrode powder is added, and 2.5 tons of pressure is applied to finally obtain the solid-state battery 200.

[0142] Comparative Example 2

[0143] (1) Preparation of composite storage layer 120:

[0144] The first carbon particles 121 and the first metal particles 122 were ball-milled in a certain ratio, and mixed with 5wt% polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) at a speed of 1200r / min for 6 hours. The mixture was coated on a stainless steel substrate by a doctor blade method, vacuum dried at 80°C for 2 hours, and then rolled to obtain a composite layer of a storage layer 120 and a current collector 110. The particle size and ratio of the first carbon particles 121 and the first metal particles 122 in Comparative Example 2 are shown in Tables 1 and 2.

[0145] (2) Preparation of interface buffer layer 130:

[0146] The second carbon particles 131 and the second metal particles 132 are mixed in a certain proportion, and then 5wt% polyvinylidene fluoride (PVDF) is added to the N-methylpyrrolidone (NMP) solution, and stirred at a speed of 1200r / min for 6 hours. The storage layer 120 is coated by a scraping method, and vacuum dried at 80°C for 2 hours to obtain the negative electrode sheet 100. The particle size and ratio of the second carbon particles 131 and the second metal particles 132 in Comparative Example 2 are shown in Tables 1 and 2.

[0147] (3) Preparation of positive electrode powder:

[0148] NCM622 positive electrode particles, LiPSCl, and acetylene black were mixed in a mass ratio of 55:42:3, wherein the mass of NCM622 active material was about 10 mg, and ground evenly to obtain positive electrode powder.

[0149] (4) Assembly of 200 solid-state batteries:

[0150] The composite layer of the storage layer 120 and the current collector 110 is cut into discs with a diameter of 10 mm, placed in a solid-state battery 200 mold with a pore size of 10 mm, 100 mg of LiPSCl electrolyte powder is added, and 1 ton of pressure is applied for pre-pressing; then, the positive electrode powder is added, and 2.5 tons of pressure is applied to finally obtain the solid-state battery 200 of comparative example 2.

[0151] Solid-state battery 200 cycle performance test

[0152] The solid-state battery 200 obtained in the above embodiment is subjected to a charge and discharge cycle test on a charge and discharge instrument, the test temperature is 45°C, the cycle rate is 1 / 3C (i.e., the charge rate and the discharge rate are both 1 / 3C), the charging voltage is 2.8V to 4.3V, and the capacity retention rate after the cycle is calculated. The capacity retention rate calculation formula of the cycle is: capacity retention rate after the nth cycle = (discharge capacity after the nth cycle / maximum value of the cycle discharge capacity)*100%.

[0153] It is understood that the term "cycle" in this application refers to the number of times the solid-state battery 200 is charged at a preset rate and discharged at a preset rate. The solid-state battery 200 completing one charge and discharge process is called a cycle, and the capacity retention rate after 50 cycles refers to the capacity retention rate after the solid-state battery 200 has undergone 50 charge and discharge processes at a charging rate of 1 / 3C and a discharge rate of 1 / 3C.

[0154] The performance test data of the solid-state battery 200 is shown in Table 2:

[0155] Table 1:

[0156]

[0157]

[0158] Table 2:

[0159]

[0160]

[0161] As shown in Table 1 and Table 2, from the data of Example 1 and Comparative Example 1, it can be seen that the negative electrode plate 100 of Comparative Example 1 does not have a buffer layer 130. After 50 cycles, the capacity retention rate of the solid-state battery 200 has dropped to 80%. This is because the buffer layer 130 of Comparative Example 1 does not inhibit the interface side reaction and the growth of lithium dendrites, resulting in a significant decrease in the capacity retention rate of the solid-state battery 200.

[0162] From the data of Example 1 and Comparative Example 2, it can be seen that a short circuit has occurred in the solid-state battery 200 in Comparative Example 2 after 50 cycles. This is because the mass fraction of the first metal particles 122 is less than the mass fraction of the second metal particles 132, and the lithium ions are preferentially deposited in the buffer layer 130, which makes it easier to generate lithium dendrites, thereby piercing the solid electrolyte 210 and causing a short circuit.

[0163] It can be seen from the data of Example 1, Example 5 and Example 6 that as the median particle size of the first carbon particles 121 increases, the kinetic performance of the lithium ions deteriorates, affecting the cycle performance of the solid-state battery 200.

[0164] It can be seen from the data of Example 1, Example 7 and Example 8 that as the ratio of the mass fraction of the first carbon particles 121 to the mass fraction of the first metal particles 122 increases, the first metal particles 122 cannot construct a plurality of uniformly dispersed nucleation sites in the storage layer 120, and cannot optimize the distribution and deposition of lithium ions, resulting in a low cycle capacity retention rate of the solid-state battery 200.

[0165] It can be seen from the data of Example 1, Example 9 and Example 10 that as the ratio of the mass fraction of the second carbon particles 131 to the mass fraction of the second metal particles 132 increases, the second metal particles 132 cannot help lithium ions cross the buffer layer 130, causing lithium ions to easily deposit in the buffer layer 130, resulting in the generation of lithium dendrites, which reduces the cycle capacity retention rate.

[0166] From the data of Example 1, Example 11 to Example 13, it can be seen that as the thickness of the buffer layer 130 increases, the growth of lithium dendrites is suppressed, and the cycle capacity retention rate is increased. When the thickness of the buffer layer 130 increases to a certain value, the thickness of the buffer layer 130 continues to increase, and the lithium ions cannot cross the buffer layer 130, causing the lithium ions to easily deposit in the buffer layer 130, resulting in the generation of lithium dendrites, which reduces the cycle capacity retention rate.

[0167] It can be seen from the data of Example 1 and Example 16 that as the median particle size of the second carbon particles 131 increases, it is difficult to control the thickness of the interface buffer layer 130, and the tortuosity of the buffer layer 130 cannot be greatly improved, and the effect of inhibiting the penetration growth of lithium dendrites is not obvious.

[0168] It can be seen from the data of Example 1 and Example 17 that when the median particle size of the second metal particles 132 increases, the second metal particles 132 cannot quickly conduct lithium ions to the storage layer 120, and the second metal particles 132 are also difficult to be evenly distributed in the buffer layer 130, resulting in the generation of lithium dendrites in the negative electrode plate 100, thereby reducing the cycle capacity retention rate.

[0169] See also Figure 5 , the embodiment of the present application provides an electric device 300, which includes: an electric device body 310 and a solid-state battery 200 described in the embodiment of the present application, and the solid-state battery 200 is used to supply power to the electric device body 310. It can be understood that for the convenience of illustration, the solid-state battery 200 is placed outside the electric device body 310, and in a normal use state, the solid-state battery 200 is inside the electric device body 310.

[0170] The power-consuming device 300 of the embodiment of the present application may be, but is not limited to, electronic devices such as mobile phones, tablet computers, laptop computers, desktop computers, smart bracelets, smart watches, e-readers, game consoles, toys, etc.; in addition, the power-consuming device 300 may also be a car, household appliances, etc.

[0171] It can be understood that the electrical equipment 300 described in this embodiment is merely a form of the electrical equipment 300 used by the solid-state battery 200, and should not be understood as a limitation on the electrical equipment 300 provided in this application, nor should it be understood as a limitation on the solid-state battery 200 provided in each embodiment of this application.

[0172] Mentioning "embodiment" and "implementation method" in this application means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrases in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should also be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, provided that there is no contradiction between them.

[0173] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the above preferred implementation modes, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.

Claims

1. A negative electrode plate, characterized in that: The negative electrode plate includes a current collector, a storage layer and a buffer layer, which are stacked in sequence. The storage layer includes a plurality of first carbon particles and a plurality of first metal particles, and the first metal particles are used to store active ions; the buffer layer includes a plurality of second carbon particles and a plurality of second metal particles, and the second metal particles are used to transport active ions, and the active ions are formed after combining with electrons, wherein the median particle size of the first carbon particles is greater than the median particle size of the second carbon particles, and the mass fraction of the first metal particles is greater than the mass fraction of the second metal particles.

2. The negative electrode sheet according to claim 1, characterized in that: The ratio of the mass fraction M1 of the first metal particles in the storage layer to the mass fraction M2 of the second metal particles in the buffer layer is in the range of 1.25≤M1 / M2≤5.

3. The negative electrode sheet according to claim 2, characterized in that: The mass fraction M1 of the first metal particles in the storage layer is in the range of 20%≤M1≤70%, and the mass fraction M2 of the second metal particles in the buffer layer is in the range of 9%≤M2≤50%.

4. The negative electrode sheet according to claim 1, characterized in that: The ratio of the mass fraction C1 of the first carbon particles in the storage layer to the mass fraction M1 of the first metal particles is in the range of 0.5≤C1 / M1≤3.5; the ratio of the mass fraction C2 of the second carbon particles in the buffer layer to the mass fraction M2 of the second metal particles is in the range of 1≤C2 / M2≤5.

5. The negative electrode sheet according to claim 1, characterized in that: The ratio of the gram capacity of the second carbon particles to the gram capacity of the first carbon particles is less than or equal to 0.

6.

6. The negative electrode sheet according to claim 1, characterized in that: The median particle size of the first carbon particles is in a range of 2 μm to 50 μm; the median particle size of the second carbon particles is in a range of 10 nm to 500 nm.

7. The negative electrode sheet according to claim 1, characterized in that: The storage layer has a thickness ranging from 20 μm to 100 μm, and the buffer layer has a thickness ranging from 1 μm to 20 μm.

8. The negative electrode sheet according to claim 1, characterized in that: The first metal particles include at least one of Mg, Sn, Ag, In, Zn, Al, Fe, Ga, Sb, Bi, Au, and Pt; the second metal particles include at least one of Mg, Sn, Ag, In, Zn, Al, Fe, Ga, Sb, Bi, Au, and Pt.

9. The negative electrode sheet according to claim 6, characterized in that: The first carbon particles include at least one of natural graphite, artificial graphite, hard carbon, soft carbon, and microporous carbon; the second carbon particles include at least one of acetylene black, Ketjen black, and super carbon black.

10. A solid-state battery, characterized in that: include: Solid electrolytes, A positive electrode sheet, stacked on the surface of the solid electrolyte, and The negative electrode plate according to claims 1 to 9, wherein the negative electrode plate is stacked on a surface of the solid electrolyte facing away from the positive electrode plate, wherein the buffer layer is arranged between the solid electrolyte and the storage layer.

11. An electrical device, characterized in that: include: The electrical equipment itself; and The solid-state battery as described in claim 10 is used to power the electrical device body.

Citation Information

Patent Citations

  • All-solid secondary battery and method of manufacturing all-solid secondary battery

    CN111293352A

  • Negative electrode and preparation method and application thereof

    CN112952031A

  • Composite buffer layer with stable negative electrode interface and solid-state lithium metal battery thereof

    CN114242942A

  • Anode for all-solid-state battery containing no active material and all-solid-state battery including the same

    US20220320483A1

  • Negative electrode active material for lithium secondary cell, and lithium secondary cell

    WO2014122748A1