Microcrystalline graphite negative electrode material, preparation method thereof and battery
By using repeated constant voltage vacuum impregnation and pulse vacuum impregnation technology in a vacuum environment, a uniform amorphous carbon layer is formed, which solves the electrolyte loss problem caused by the microcrystalline graphite pore structure and improves the performance and stability of the battery.
Patent Information
- Application Number
- CN202410928719.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
The pore structure of microcrystalline graphite causes electrolyte loss, affecting the first Coulomb efficiency and cycling performance of the battery. It is difficult for the existing technology to achieve uniform coating, resulting in direct contact between the electrolyte and the graphite, reducing the battery performance.
In a vacuum environment, microcrystalline graphite is mixed with polymer material and diluent, and repeated constant pressure vacuum impregnation and pulse vacuum impregnation technology are used to spray dry to form a uniform amorphous carbon layer to block the contact of the electrolyte with the graphite.
It improves the service life and first-time efficiency of the battery, reduces electrolyte consumption, enhances the cycle stability and rate performance of the battery, and reduces the charge transfer resistance.
Smart Images

Figure CN118899412A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of negative electrode materials, and in particular to a microcrystalline graphite negative electrode material and a preparation method thereof and a battery. Background Art
[0002] There are a large number of primary pores in the microcrystalline graphite particles, which are the supporting structures formed by the interweaving growth of graphite grain boundaries. Although the grain size of microcrystalline graphite is small, the particles are large. After proper crushing and shaping, the surface is rough, but the internal pores have a stable self-supporting structure due to the interpenetration of crystal planes. After shaping, a large number of primary pores are still retained in the grains, which still have an adverse effect on the subsequent tap density and specific capacity.
[0003] Coating carbonization to form an amorphous carbonized film on the surface of microcrystalline graphite is the main means to reduce the inability of electrolyte to react with graphite in direct contact, resulting in electrolyte loss, and further affecting the initial coulombic efficiency of the battery. Due to the large number of pores in the middle of microcrystalline graphite, cracks are formed in some carbonized films during the processing. The electrolyte enters the interior of the microcrystalline graphite through the cracks and directly contacts and reacts with the graphite, thereby reducing the coulombic efficiency and affecting the cycle performance of the battery.
[0004] Therefore, how to improve the impregnation effect and achieve uniform encapsulation of microcrystalline graphite is a problem that needs to be solved at present. Summary of the invention
[0005] The purpose of this application is to provide a microcrystalline graphite negative electrode material and a preparation method and a battery to solve the above problems.
[0006] To achieve the above objectives, the present application provides a first aspect of a method for preparing a microcrystalline graphite negative electrode material, comprising:
[0007] In a vacuum environment, microcrystalline graphite and a coating agent are mixed, and constant pressure vacuum impregnation and pulse vacuum impregnation are repeatedly performed, and then spray-dried to obtain a microcrystalline graphite negative electrode material;
[0008] The coating agent includes a polymer material and a diluent;
[0009] The pulsed vacuum impregnation includes obtaining pressure pulses by periodically applying and releasing pressure.
[0010] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0011] A. The grain size of the microcrystalline graphite is less than 1 μm;
[0012] B. The graphitization degree of the microcrystalline graphite is ≥ 90%;
[0013] C. The particle size of the microcrystalline graphite is 8 μm-22 μm;
[0014] D. The microcrystalline graphite is obtained by crushing and grinding the microcrystalline graphite to be processed.
[0015] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0016] A. The pressure difference of the pressure pulse is 0.1pa-1pa in the negative pressure state, and 800kpa-1000kpa in the positive pressure state;
[0017] B. The time of a single pulse vacuum impregnation is 6 minutes to 18 minutes.
[0018] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0019] A. The impregnation temperature of the constant pressure vacuum impregnation and the pulse vacuum impregnation is 25°C-45°C;
[0020] B. The solid-liquid ratio of the microcrystalline graphite and the coating agent is 1g:(1.5mL-2mL);
[0021] C. The vacuum degree of the vacuum environment is 0.04MPa-0.09Mpa;
[0022] D. The time of a single constant pressure vacuum impregnation is 30 min-60 min.
[0023] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0024] A. The total time ratio of the constant pressure vacuum impregnation to the total time ratio of the pulse vacuum impregnation is 4:(1.5-2);
[0025] B. The number of repetitions is 4 to 14 times;
[0026] C. The spray drying temperature is 150°C-250°C.
[0027] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0028] A. The polymer material includes high-purity coal tar pitch;
[0029] B. The diluent includes diesel.
[0030] Optionally, the mass ratio of the polymer material to the diluent is 1:(0.5-0.8).
[0031] Optionally, the coating agent further comprises an auxiliary agent, and the auxiliary agent accounts for 1%-5% of the total mass of the coating agent.
[0032] A second aspect of the present application provides a microcrystalline graphite negative electrode material, which is prepared by the preparation method of the microcrystalline graphite negative electrode material.
[0033] The third aspect of the present application provides a battery, comprising the above-mentioned microcrystalline graphite negative electrode material.
[0034] Compared with the prior art, the beneficial effects of this application include:
[0035] The preparation method of the microcrystalline graphite negative electrode material provided in the present application, firstly, by adding a diluent to the coating agent, the diluent can enhance the fluidity and wettability of the coating agent, so that it can quickly penetrate into the pores of the microcrystalline graphite, which helps the coating agent to be more evenly distributed on the surface and pores of the microcrystalline graphite; secondly, in a vacuum environment, the wetting effect of the coating agent can be improved to ensure that it is not only evenly distributed on the surface of the microcrystalline graphite particles, but also can effectively fill the pores inside the particles; then, pulse vacuum impregnation is performed to further promote the infiltration of the electrolyte into the pores inside the microcrystalline graphite particles, forming a containment effect, preventing the electrolyte from directly entering the pores, thereby reducing the occurrence of adverse reactions, helping to reduce the gas in the pores, and thus improving the filling efficiency; finally, by repeated constant pressure vacuum impregnation and pulse vacuum impregnation, the desired wetting and filling effects are achieved.
[0036] The microcrystalline graphite negative electrode material provided in the present application has a coating agent uniformly distributed on the surface and pores of the microcrystalline graphite. The coating agent is formed after carbonization to form a uniform amorphous carbon layer on the surface and pores of the graphite, which can prevent the electrolyte from directly contacting the graphite.
[0037] The battery provided in the present application reduces direct contact between the electrolyte and the microcrystalline graphite negative electrode material, thereby extending the battery life, improving the initial efficiency, and reducing the performance degradation of the battery due to electrolyte consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0039] Figure 1 is a SEM image of the microcrystalline graphite of Example 1;
[0040] Figure 2 This is the SEM image of the microcrystalline graphite negative electrode material prepared in Example 1. DETAILED DESCRIPTION
[0041] As used herein:
[0042] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0043] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0044] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0045] In these examples, parts and percentages are by mass unless otherwise indicated.
[0046] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0047] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0048] The first aspect of the present application provides a method for preparing a microcrystalline graphite negative electrode material, comprising:
[0049] In a vacuum environment, microcrystalline graphite and a coating agent are mixed, and constant pressure vacuum impregnation and pulse vacuum impregnation are repeatedly performed, and then spray-dried to obtain a microcrystalline graphite negative electrode material;
[0050] The coating agent includes a polymer material and a diluent;
[0051] It should be noted that in order to enhance the fluidity and wettability of the coating agent, an appropriate amount of diluent is added to the substrate. The diluent can be an organic solvent, such as alcohols, ketones and esters. The main feature of the diluent is that it can reduce the viscosity of the asphalt, making it easier to flow. At the same time, the diluent also helps to improve the polarity of the solution molecules and promote wettability with the surface of the microcrystalline graphite. The selection of the diluent needs to consider factors such as its volatility, solubility and safety. Compared with a single polymer material, increasing the amount of diluent impregnation has significantly improved.
[0052] The pulsed vacuum impregnation includes obtaining pressure pulses by periodically applying and releasing pressure.
[0053] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0054] A. The grain size of the microcrystalline graphite is less than 1 μm;
[0055] Optionally, the grain size of the microcrystalline graphite may be 0.01 μm, 0.1 μm, 0.5 μm, 0.9 μm or any value less than 1 μm;
[0056] B. The graphitization degree of the microcrystalline graphite is ≥ 90%;
[0057] Optionally, the degree of graphitization of the microcrystalline graphite may be 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or any value ≥ 90%;
[0058] It should be noted that the grain size of microcrystalline graphite is less than 1 micron, the degree of graphitization is ≥90%, and its crystal structure is in a short-range ordered and long-range disordered stacking state. Pore channels are formed between grain boundaries due to the interweaving of sheets, and most of them are narrow channels. Some are closed pores under normal pressure, but the pore channels are easily broken under high temperature and high pressure during the cycle process;
[0059] C. The particle size of the microcrystalline graphite is 8 μm-22 μm;
[0060] Optionally, the particle size of the microcrystalline graphite may be 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 22 μm or any value between 8 μm and 22 μm;
[0061] It should be noted that microcrystalline graphite is a polycrystalline particle.
[0062] D. The microcrystalline graphite is obtained by crushing and grinding the microcrystalline graphite to be processed.
[0063] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0064] A. The pressure difference of the pressure pulse in the negative pressure state is 0.1pa-1pa, and the pressure difference in the positive pressure state is 800kpa-1000kpa;
[0065] Optionally, the pressure difference of the pressure pulse in the negative pressure state can be 0.1Pa, 0.2Pa, 0.4Pa, 0.6Pa, 0.8Pa, 1Pa or any value between 0.1Pa-1Pa, and the pressure difference in the positive pressure state can be 800kPa, 850kPa, 900kPa, 950kPa, 1000kPa or any value between 800kPa-1000kPa;
[0066] It should be noted that the periodic pressure difference generated by pulsed vacuum impregnation can promote the flow of the coating agent in the pores of microcrystalline graphite. The pressure pulse can push the liquid into the pores to achieve deeper penetration and filling. Through pulsed vacuum impregnation, a dynamic containment effect can be formed at the entrance of the pores to prevent further penetration of the electrolyte.
[0067] B. The time of a single pulse vacuum impregnation is 6 minutes to 18 minutes.
[0068] Optionally, the time of a single pulse vacuum impregnation may be 6 min, 8 min, 10 min, 12 min, 14 min, 16 min, 18 min or any value between 6 min and 18 min.
[0069] It should be noted that the penetration effect can be optimized by controlling the pressure difference of the pressure pulse and the duration of the pulsed vacuum impregnation.
[0070] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0071] A. The impregnation temperature of the constant pressure vacuum impregnation and the pulse vacuum impregnation is 25°C-45°C;
[0072] Optionally, the impregnation temperature of the constant pressure vacuum impregnation and the pulse vacuum impregnation may be 25°C, 30°C, 35°C, 40°C, 45°C or any value between 25°C and 45°C;
[0073] It should be noted that the increase in temperature has a promoting effect on the fluidity of polymer materials. With the increase in temperature, the viscosity of polymer materials also decreases. The increase in temperature reduces the surface tension of the liquid, and the wettability between the polymer material and the microcrystalline graphite is enhanced. The amount of polymer impregnation in the microcrystalline graphite also increases. With the increase in temperature, when the impregnation temperature is 25℃-45℃, the liquid asphalt under negative pressure conditions is applicable to the following rules: Under negative pressure, the vapor pressure of the liquid becomes supersaturated relative to the external pressure, and its boiling point decreases. Although the impregnation temperature is room temperature, it can still reduce the softening temperature of the asphalt, which promotes its fluidity. At the same time, room temperature is easy to reach in the industrial field, which is conducive to reducing energy consumption.
[0074] It should also be noted that it also has an important influence on the impregnation amount. The polymer material often has poor fluidity at the softening point, but when the treatment temperature rises to the softening point, the viscosity of the polymer material decreases significantly. At the same time, the increase in temperature reduces the surface tension of the liquid, and the wettability between the polymer material and the microcrystalline graphite is enhanced. The impregnation amount of the polymer material also gradually increases, in order to increase the impregnation amount of the polymer material in the microcrystalline graphite;
[0075] B. The solid-liquid ratio of the microcrystalline graphite and the coating agent is 1g:(1.5mL-2mL);
[0076] Optionally, the solid-liquid ratio of microcrystalline graphite to the coating agent may be any value between 1g:1.5mL, 1g:1.6mL, 1g:1.7mL, 1g:1.8mL, 1g:1.9mL, 1g:2mL or 1g:(1.5mL-2mL);
[0077] C. The vacuum degree of the vacuum environment is 0.04MPa-0.09Mpa;
[0078] Optionally, the vacuum degree of the vacuum environment may be 0.04 MPa, 0.05 MPa, 0.06 MPa, 0.07 MPa, 0.08 MPa, 0.09 MPa or any value between 0.04 MPa and 0.09 MPa;
[0079] D. The time of a single constant pressure vacuum impregnation is 30 minutes to 60 minutes.
[0080] Optionally, the time of a single constant-pressure vacuum impregnation can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min or any value between 30 min and 60 min.
[0081] It should be noted that when the single constant pressure vacuum impregnation time is 30min-60min, it has the following beneficial effects:
[0082] Sufficient impregnation: A longer impregnation time can ensure that the impregnation liquid has enough time to penetrate into the deep structure of the porous material, achieving a more uniform and in-depth impregnation effect;
[0083] Improve efficiency: Under constant pressure conditions, the penetration rate of the impregnation liquid is relatively stable, which helps to improve production efficiency because the impregnation process can be predicted and controlled;
[0084] Reduce defects: Longer impregnation times help reduce defects caused by rapid impregnation, such as entrapment of bubbles or uneven filling;
[0085] Reduce stress: Under the combined effect of vacuum and constant pressure, the stress and porosity inside the material can be reduced, thereby improving the mechanical and electrical properties of the material;
[0086] Improve product quality: By extending the impregnation time, the consistency and reliability of the product can be improved and the defective product rate in the production process can be reduced;
[0087] Adaptability: The longer time window (30 minutes to 60 minutes) provides flexibility in process adjustment, which can be optimized according to material characteristics and production requirements;
[0088] Reduced number of cycles: In some cases, appropriate single immersion time can reduce the number of immersion cycles required, saving time and cost;
[0089] Promote chemical reaction: If there is a chemical reaction between the impregnation liquid and the material, a longer time can promote the reaction and thus improve the performance of the material;
[0090] Environmentally friendly: Under constant pressure conditions, it can reduce energy consumption and environmental impact caused by pressure fluctuations;
[0091] Safe operation: Constant pressure operation is generally safer than operation with fluctuating pressure because equipment and materials are not easily affected by sudden changes in pressure.
[0092] It should also be noted that there is an upper limit to the amount of coating agent impregnated in microcrystalline graphite. When the pores of the microcrystalline graphite are completely filled with the coating agent, the coating agent reaches the theoretical maximum impregnation amount in the microcrystalline graphite. The impregnation process of the coating agent in the microcrystalline graphite needs to overcome the viscous resistance and the gas compression resistance in the pores. Although the influence of gas resistance is reduced under vacuum, the flow rate is low, so a certain impregnation time is required. This application chooses to add a diluent to enhance the flow rate.
[0093] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0094] A. The total time ratio of the constant pressure vacuum impregnation to the total time ratio of the pulse vacuum impregnation is 4:(1.5-2);
[0095] Optionally, the total time ratio of constant pressure vacuum impregnation to the total time ratio of pulse vacuum impregnation may be 4:1.5, 4:1.6, 4:1.7, 4:1.8, 4:1.9, 4:2 or any value between 4:(1.5-2);
[0096] B. The number of repetitions is 4 to 14 times;
[0097] Optionally, the number of repetitions may be 4 times, 6 times, 8 times, 10 times, 12 times, 14 times, or any value between 4 and 14 times;
[0098] It should be noted that when the number of repetitions is 4 to 14 times, the following beneficial effects can be achieved within this range:
[0099] Improve permeability: Pulse vacuum impregnation can help break the adsorption state of air in the pores of the material by periodically changing the pressure, thereby improving the permeability of the impregnation liquid;
[0100] Reduce bubbles: Bubbles may form inside the material during constant pressure impregnation, and pulse operation can help release and remove these bubbles through pressure changes;
[0101] Optimize the impregnation depth: Alternating between constant pressure and pulse impregnation can more effectively deliver the impregnation liquid into the deep structure of the material, achieving a more uniform impregnation effect;
[0102] Improved material properties: By alternating constant pressure and pulse impregnation, the distribution of the impregnation liquid in the material can be better controlled, thereby improving the performance of the final product, such as mechanical strength and electrical properties;
[0103] Improve production efficiency: Pulse operation can shorten the impregnation cycle and improve production efficiency. At the same time, constant pressure impregnation ensures full penetration of the impregnation liquid.
[0104] Reduce material damage: Constant pressure impregnation can avoid material damage caused by excessive pressure, while pulse operation can reduce material deformation caused by long-term constant pressure.
[0105] Adapt to different material properties: Different materials may respond differently to pressure changes. Alternating constant pressure and pulse impregnation can adapt to the pore structure and permeability characteristics of different materials;
[0106] Promote solvent evaporation: In some impregnation processes, pulse operation can help the solvent evaporate faster, thereby accelerating the curing process of the impregnation liquid;
[0107] Achieve better coating agent flow: Alternating pressure changes can promote the flow and filling of coating agents in the material, reducing dead corners and unimpregnated areas;
[0108] Improve product quality: By continuously alternating and repeating constant pressure and pulse impregnation, the consistency and reliability of products can be improved and the defective rate in the production process can be reduced.
[0109] C. The spray drying temperature is 150°C-250°C.
[0110] Optionally, the spray drying temperature may be 150°C, 200°C, 250°C or any value between 150°C and 250°C.
[0111] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:
[0112] A. The polymer material includes high-purity coal tar pitch;
[0113] It should be noted that high-purity coal tar pitch helps to increase the weight gain rate and reduce the open porosity, which helps to enhance the wetting ability of polymer materials on microcrystalline graphite to further improve the wettability and dispersibility of the coating agent.
[0114] B. The diluent includes diesel.
[0115] It should be noted that diesel, as a diluent, has a chemical structure mainly composed of hydrocarbons with a wide molecular weight range, usually ranging from C10 to C20, and is not easy to volatilize. It is highly safe to use. At the same time, after addition, it can effectively reduce the viscosity of polymer materials, improve the fluidity of polymer materials and the wettability of microcrystalline graphite.
[0116] In some embodiments, the mass ratio of the polymer material to the diluent is 1:(0.5-0.8).
[0117] Optionally, the mass ratio of the polymer material to the diluent may be 1:0.5, 1:0.6, 1:0.7, 1:0.8 or any value between 1:(0.5-0.8).
[0118] It should be noted that by adjusting the ratio of the diluent, the polymer material and the diluent are mixed in the range of 1: (0.5-0.8). The relevant ratio is limited by the molecular weight of the polymer material. If the molecular weight is large, the amount of the diluent should be appropriately increased to control the viscosity of the coating agent and make it easier to penetrate into the pores of the microcrystalline graphite.
[0119] It should also be noted that, by adjusting the coating agent formula in the present application, the surface tension is reduced, the contact angle between the coating agent and the microcrystalline graphite is increased, and the wettability is improved.
[0120] In some embodiments, the coating agent further includes an auxiliary agent, and the auxiliary agent accounts for 1%-5% of the total mass of the coating agent.
[0121] Optionally, the auxiliary agent may account for 1%, 2%, 3%, 4%, 5% or any value between 1% and 5% of the total mass of the coating agent.
[0122] It should be noted that in order to further optimize the formula, additives can also be added. The additives can be surfactants. Adding surfactants is helpful to improve the stability of the slurry and enhance the wetting ability of uncured graphite, which helps to evenly disperse the coating agent on the surface of microcrystalline graphite and prevent aggregation and precipitation.
[0123] It should also be noted that the performance of microcrystalline graphite negative electrode materials can be significantly improved by improving the coating agent and combining repeated constant pressure vacuum impregnation and pulse vacuum impregnation. The coating agent specified in this application can form a uniform and stable protective layer, while repeated constant pressure vacuum impregnation and pulse vacuum impregnation can further improve the filling effect of the pores, thereby improving the overall performance of the material.
[0124] Specifically, the coating provided in this application can have the following beneficial effects:
[0125] ① Improve battery performance: The amorphous carbon layer can significantly improve the performance of the battery, reduce the irreversible capacity of the first charge and discharge cycle, and help form a uniform and dense SEI film, reducing the lithium ion consumption during the formation of the SEI film;
[0126] ② Improve cycle stability: The amorphous carbon layer covers the graphite surface, which can reduce the direct contact between graphite and electrolyte, thereby reducing graphite exfoliation, pulverization and volume expansion caused by the solvation effect, and improving the cycle stability of the battery;
[0127] ③ Improve rate performance: Due to its isotropy, the amorphous carbon layer is conducive to the rapid insertion and extraction of lithium ions, thereby improving the high-current charge and discharge performance of the battery;
[0128] ④ Reduce charge transfer resistance: Amorphous carbon coating can effectively reduce the charge transfer resistance at the interface between graphite and electrolyte, and improve the charge and discharge efficiency of the battery;
[0129] ⑤ Improve the first coulombic efficiency: Amorphous carbon coating helps improve the first coulombic efficiency of the battery by reducing irreversible side reactions during the first charge and discharge process;
[0130] ⑥ Expand the selection range of electrolyte systems: The amorphous carbon layer can prevent the co-embedding of solvent molecules, thereby expanding the selection range of electrolyte systems and improving the cycle stability of electrode materials.
[0131] ⑦ Enhance the electrochemical properties of electrode materials: Amorphous carbon coating helps to improve the electrochemical properties of materials, including improving reversible capacity and Coulomb efficiency.
[0132] A second aspect of the present application provides a microcrystalline graphite negative electrode material, which is prepared by the preparation method of the microcrystalline graphite negative electrode material.
[0133] The third aspect of the present application provides a battery, comprising the above-mentioned microcrystalline graphite negative electrode material.
[0134] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0135] Example 1
[0136] This embodiment provides a method for preparing a microcrystalline graphite negative electrode material, comprising:
[0137] S1: crushing and grinding the microcrystalline graphite to be processed to obtain microcrystalline graphite with a particle size of 17 μm, a grain size of less than 1 μm, and a graphitization degree of ≥90%;
[0138] S2: The microcrystalline graphite is sealed in a pulse vacuum impregnation container, and the pulse vacuum impregnation container is evacuated. The vacuum degree in the container is 0.09MPa. This state is maintained for 0.5 hours and the container is not depressurized. Under the vacuum condition, the coating agent is injected into the vacuum impregnation container through a pipeline. The coating agent is high-purity coal tar and diesel in a mass ratio of 1:0.5, and the graphite powder is completely immersed in the coating agent. The solid-liquid ratio of microcrystalline graphite and coating agent is 1g:2mL. Then the vacuum impregnation state is maintained. The time for a single vacuum impregnation is 30min. During the process, ultrasonic vibration external field force is applied, and pressure is periodically applied and released to obtain pressure pulses. The pressure difference of the pressure pulse is 0.2Pa under negative pressure, and it is maintained at 800kpa under positive pressure. The time for a single pulse vacuum impregnation is 6min-18min, and a single vacuum impregnation and a single pulse vacuum impregnation are one cycle. After 4 cycles, the total time of vacuum impregnation and the total time of pulse vacuum impregnation are 4:2. The temperature of the entire impregnation process is 25°C. After the end, spray drying is carried out, and the nozzle temperature is 300 degrees Celsius to obtain a microcrystalline graphite negative electrode material.
[0139] This embodiment also provides a microcrystalline graphite negative electrode material, which is prepared by the above-mentioned method for preparing the microcrystalline graphite negative electrode material.
[0140] SEM of microcrystalline graphite Figure 1 shown.
[0141] SEM images of microcrystalline graphite negative electrode materials Figure 2 shown.
[0142] Example 2
[0143] This embodiment provides a method for preparing a microcrystalline graphite negative electrode material, comprising:
[0144] S1: crushing and grinding the microcrystalline graphite to be processed to obtain microcrystalline graphite with a particle size of 8 μm, a grain size of less than 1 μm, and a graphitization degree of ≥90%;
[0145] S2: The microcrystalline graphite is sealed in a pulse vacuum impregnation container, and the pulse vacuum impregnation container is evacuated. The vacuum degree in the container is 0.09MPa. This state is maintained for 0.5 hours and the container is not depressurized. Under the vacuum condition, the coating agent is injected into the vacuum impregnation container through a pipeline. The coating agent is high-purity coal tar and diesel in a mass ratio of 1:0.7, and the graphite powder is completely immersed in the coating agent. The solid-liquid ratio of microcrystalline graphite and coating agent is 1g:1.6. Then the vacuum impregnation state is maintained. The time of a single vacuum impregnation is 30min. During the process, ultrasonic vibration external field force is applied, and pressure is periodically applied and released to obtain pressure pulses. The pressure difference of the pressure pulse is 0.3Pa under negative pressure, and it is maintained at 900kpa under positive pressure. The time for a single pulse vacuum impregnation is 10min. A single vacuum impregnation and a single pulse vacuum impregnation are one cycle. After 6 cycles, the ratio of the total time of vacuum impregnation to the total time of pulse vacuum impregnation is 4:1.6. The temperature of the entire impregnation process is 26.5°C. After the end, spray drying is carried out with a nozzle temperature of 300 degrees Celsius to obtain a microcrystalline graphite negative electrode material.
[0146] This embodiment also provides a microcrystalline graphite negative electrode material, which is prepared by the above-mentioned method for preparing the microcrystalline graphite negative electrode material.
[0147] Example 3
[0148] This embodiment provides a method for preparing a microcrystalline graphite negative electrode material, comprising:
[0149] S1: crushing and grinding the microcrystalline graphite to be processed to obtain microcrystalline graphite with a particle size of 22 μm, a grain size of less than 1 μm, and a graphitization degree of ≥90%;
[0150] S2: The microcrystalline graphite is sealed in a pulse vacuum impregnation container, and the pulse vacuum impregnation container is evacuated. The vacuum degree in the container is 0.09MPa. This state is maintained for 0.5 hours and the container is not depressurized. Under the vacuum condition, the coating agent is injected into the vacuum impregnation container through a pipeline. The coating agent is high-purity coal tar and diesel in a mass ratio of 1:0.8, and the graphite powder is completely immersed in the coating agent. The solid-liquid ratio of microcrystalline graphite and coating agent is 1g:1.8. Then the vacuum impregnation state is maintained. The single vacuum impregnation time is 50min. During the impregnation process, ultrasonic vibration external field force is applied, and pressure is periodically applied and released to obtain pressure pulses. The pressure difference of the pressure pulse is 0.8Pa under negative pressure, and it is maintained at 1000kpa under positive pressure. The time for a single pulse vacuum impregnation is 16. A single vacuum impregnation and a single pulse vacuum impregnation are one cycle. After 10 cycles, the total time of vacuum impregnation and the total time of pulse vacuum impregnation are 4:1.8. The temperature of the entire impregnation process is 30°C. After the end, spray drying is carried out, and the nozzle temperature is 300 degrees Celsius to obtain a microcrystalline graphite negative electrode material.
[0151] This embodiment also provides a microcrystalline graphite negative electrode material, which is prepared by the above-mentioned method for preparing the microcrystalline graphite negative electrode material.
[0152] Comparative Example 1
[0153] This comparative example provides a method for preparing a microcrystalline graphite negative electrode material, which is different from Example 1 in that the microcrystalline graphite obtained in this comparative example is immersed in air.
[0154] This comparative example also provides a microcrystalline graphite negative electrode material, which is prepared by the above-mentioned method for preparing the microcrystalline graphite negative electrode material.
[0155] Comparative Example 2
[0156] This comparative example provides a method for preparing a microcrystalline graphite negative electrode material, which is different from Example 1 in that this comparative example only performs vacuum impregnation.
[0157] This comparative example also provides a microcrystalline graphite negative electrode material, which is prepared by the above-mentioned method for preparing the microcrystalline graphite negative electrode material.
[0158] Comparative Example 3
[0159] This comparative example provides a method for preparing a microcrystalline graphite negative electrode material, which is different from Example 1 in that this comparative example only performs pulse vacuum impregnation.
[0160] This comparative example also provides a microcrystalline graphite negative electrode material, which is prepared by the above-mentioned method for preparing the microcrystalline graphite negative electrode material.
[0161] Comparative Example 4
[0162] This comparative example provides a method for preparing a microcrystalline graphite negative electrode material, which is different from Example 1 in that this comparative example only performs one single vacuum impregnation and one pulse vacuum impregnation cycle, that is, one cycle.
[0163] This comparative example also provides a microcrystalline graphite negative electrode material, which is prepared by the above-mentioned method for preparing the microcrystalline graphite negative electrode material.
[0164] Comparative Example 5
[0165] This comparative example provides a method for preparing a microcrystalline graphite negative electrode material, which is different from Example 1 in that the ratio of the total time of vacuum impregnation to the total time of pulse vacuum impregnation in this comparative example is 4:7.
[0166] This comparative example also provides a microcrystalline graphite negative electrode material, which is prepared by the above-mentioned method for preparing the microcrystalline graphite negative electrode material.
[0167] The performance of the microcrystalline graphite negative electrode materials obtained in the above examples and comparative examples was tested, and the test results are shown in Table 1.
[0168] Table 1 Performance test
[0169]
[0170] Density test: The true density test is used to determine the true density of graphite negative electrode materials, that is, the ratio of material mass to true volume (excluding the volume of pores and voids outside particles). The instrument used is a fully automatic true density meter (such as TD-2200 / STD-3200). The specific test method includes: turning on and preheating the true density meter for 30 minutes, introducing helium as a replacement gas, placing the sample chamber into the true density meter, loading the sample and covering the chamber cover, and performing a true density test according to the instrument operating instructions, which usually includes steps such as gas replacement, volume measurement and mass measurement. The instrument automatically calculates and displays the true density result.
[0171] Porosity test: The porosity test is used to evaluate the volume ratio of pores in graphite negative electrode materials, including open pores and closed pores, in order to understand the pore structure characteristics of the material. The instrument used is a porosity tester.
[0172] Cycle performance test: By simulating the actual use conditions of the battery, the graphite negative electrode material is subjected to multiple charge and discharge cycle tests to evaluate its key performance indicators such as capacity retention, coulombic efficiency, and voltage stability, so as to determine its cycle stability and service life.
[0173] Capacity test: Through specific test conditions and methods, the actual capacity of the graphite negative electrode material is measured to evaluate its lithium storage capacity and its impact on battery performance.
[0174] It can be seen from the above embodiments that when the porosity drops to less than 20%, it means that the pores in the graphite aggregate are effectively filled and coated; at the same time, the negative electrode material made of the aggregate has significantly improved cycle performance, indicating that during the cycle, the graphite crystal structure is stable, and the electrolyte has good compatibility with the amorphous carbon formed by carbonization on the graphite surface and the inner wall of the pores, which effectively prevents the consumption of the electrolyte during the charge and discharge process, thereby ensuring that its cycle performance is fully utilized. At the same time, due to the opening of the pore channels, the lithium ion migration channels are further enriched, and the lithium storage space is increased, which promotes the capacity of the material to be improved; at the same time, since the interlayer spacing of the amorphous carbon material is larger than that of graphite, it is helpful to improve the diffusion performance of lithium ions therein, which is equivalent to forming a lithium ion buffer layer on the outer surface of the graphite, reducing the charge transfer resistance on the graphite and electrolyte surfaces, and greatly improving the rate performance without reducing the initial coulomb efficiency.
[0175] It can be seen from Comparative Example 5 that as the proportion of vacuum impregnation time increases, its beneficial effect is limited, and the pulse type is more conducive to breaking through the narrow channels in the pores, and the vacuum environment only plays an auxiliary role in preparing the vacuum conditions.
[0176] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0177] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for preparing a microcrystalline graphite negative electrode material, It is characterized in that include: In a vacuum environment, microcrystalline graphite and a coating agent are mixed, and constant pressure vacuum impregnation and pulse vacuum impregnation are repeatedly performed, and then spray-dried to obtain a microcrystalline graphite negative electrode material; The coating agent includes a polymer material and a diluent; The pulsed vacuum impregnation includes obtaining pressure pulses by periodically applying and releasing pressure.
2. The method for preparing the microcrystalline graphite negative electrode material according to claim 1, It is characterized in that At least one of the following conditions is met: A. The grain size of the microcrystalline graphite is less than 1 μm; B. The graphitization degree of the microcrystalline graphite is ≥ 90%; C. The particle size of the microcrystalline graphite is 8 μm-22 μm; D. The microcrystalline graphite is obtained by crushing and grinding the microcrystalline graphite to be processed.
3. The method for preparing the microcrystalline graphite negative electrode material according to claim 1, It is characterized in that At least one of the following conditions is met: A. The pressure difference of the pressure pulse in the negative pressure state is 0.1pa-1pa, and the pressure difference in the positive pressure state is 800kpa-1000kpa; B. The time of a single pulse vacuum impregnation is 6 minutes to 18 minutes.
4. The method for preparing the microcrystalline graphite negative electrode material according to claim 1, It is characterized in that At least one of the following conditions is met: A. The impregnation temperature of the constant pressure vacuum impregnation and the pulse vacuum impregnation is 25°C-45°C; B. The solid-liquid ratio of the microcrystalline graphite and the coating agent is 1g:(1.5mL-2mL); C. The vacuum degree of the vacuum environment is 0.04MPa-0.09Mpa; D. The time of a single constant pressure vacuum impregnation is 30 min-60 min.
5. The method for preparing the microcrystalline graphite negative electrode material according to claim 1, It is characterized in that At least one of the following conditions is met: A. The total time ratio of the constant pressure vacuum impregnation to the total time ratio of the pulse vacuum impregnation is 4:(1.5-2); B. The number of repetitions is 4 to 14 times; C. The spray drying temperature is 150°C-250°C.
6. The method for preparing the microcrystalline graphite negative electrode material according to claim 1, It is characterized in that At least one of the following conditions is met: A. The polymer material includes high-purity coal tar pitch; B. The diluent includes diesel.
7. The method for preparing the microcrystalline graphite negative electrode material according to claim 1, It is characterized in that The mass ratio of the polymer material to the diluent is 1:(0.5-0.8).
8. The method for preparing the microcrystalline graphite negative electrode material according to claim 1, It is characterized in that The coating agent further comprises an auxiliary agent, and the auxiliary agent accounts for 1%-5% of the total mass of the coating agent.
9. A microcrystalline graphite negative electrode material, It is characterized in that The microcrystalline graphite negative electrode material is prepared by the preparation method of the microcrystalline graphite negative electrode material according to any one of claims 1 to 8.
10. A battery, It is characterized in that Including the microcrystalline graphite negative electrode material as described in claim 9.
Citation Information
Cited By
High-rate natural graphite negative electrode material and preparation method thereof
CN121626984A