Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery

By adding aluminum into the P3 phase structure of the positive electrode material of sodium ion battery, the NaO6 octahedral structure is suppressed and the Mitsubishi column structure is optimized, and the capacity and rate performance problems of sodium ion battery under high-speed conditions are solved, and higher electricity is achieved Chemical properties.

CN118899423APending Publication Date: 2024-11-05JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411239596.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode materials show lower capacity and poor rate performance under high magnification conditions, which cannot meet the actual application needs.

Method used

Aluminum is doped into a specific P3 phase structure, and the formation of NaO6 octahedral structure is inhibited through the coordinated coordination of aluminum, and the synthesis of Mitsubishi column structure is optimized, thereby improving the diffusion activation energy and capacity of sodium ions.

Benefits of technology

It achieves better gram capacity and rate performance of sodium electropositive electrode materials, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899423A_ABST
    Figure CN118899423A_ABST
Patent Text Reader

Abstract

The invention provides a sodium-ion battery positive electrode material, a preparation method thereof and a sodium-ion battery. The sodium battery positive electrode material is of a P3 phase structure, and the sodium battery positive electrode material comprises nickel, manganese and aluminum. According to the sodium battery positive electrode material provided by the invention, aluminum is doped into a specific P3 phase structure, so that the sodium battery positive electrode material has more excellent gram volume and rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion batteries and relates to a sodium positive electrode material and a preparation method thereof and a sodium ion battery. Background Art

[0002] Sodium-ion batteries have the advantages of low cost and good safety performance, and are generally considered to be an ideal alternative to lithium-ion batteries. In recent years, with the growing demand for battery energy storage systems, sodium-ion batteries can provide a cheaper alternative to current lithium-based energy storage systems, especially for large-scale energy storage applications with high safety and cost requirements. At present, the main bottleneck for the commercialization of sodium-ion batteries is the relatively low energy density of their positive electrode materials. Sodium-ion battery positive electrode materials are mainly divided into three categories: layered metal oxides, polyanion compounds, and Prussian blue compounds. Although polyanion compounds and Prussian blue compounds have been extensively studied as positive electrode materials in the past decade, layered oxides are still considered to be the best choice for the commercialization of sodium-ion batteries due to their higher energy density.

[0003] The general formula of layered oxide cathode materials for sodium ion batteries is Na x MO2 (M is one or more transition metal elements). According to the coordination configuration of sodium ions in the MO6 polyhedron and the stacking mode of oxygen, layered oxides can be divided into different structures such as O3, O2, P3 and P2 (generally, when the sodium content is low (x≤0.8), it tends to form P phase, and when the sodium content is high (0.8<x≤1), it is easy to form O phase). For example, CN117276521A discloses an O3 type sodium ion positive electrode material, a preparation method and application thereof. The preparation method of the O3 type sodium ion positive electrode material of the present application comprises the following steps: first, a Ni source, a Mn source, a dopant M1 source and a Na source are mixed and calcined for the first time to obtain a primary sintered positive electrode material; then, the mixture is mixed with a dopant M2 source and calcined for the second time to obtain a secondary sintered positive electrode material; finally, the mixture is mixed with a coating agent and calcined for the third time to obtain an O3 type sodium ion positive electrode material. For another example, CN115799493A provides a sodium ion battery layered oxide positive electrode material, a preparation method and application thereof. The sodium ion battery layered oxide positive electrode material is a P-type structural material, and the metal elements other than sodium in the sodium ion positive electrode material include chromium and tantalum. The positive electrode material provided by the present invention has a P2 configuration, which broadens the interplanar spacing of the sodium chromite layered oxide, and effectively avoids the complex phase transition problem when sodium chromite is used as a sodium ion battery positive electrode material. At present, compared with polyanion compound sodium electric positive electrode materials, although layered oxide positive electrode materials have better rate performance, when used under high rate conditions of 5C and above, their actual capacity is only 50-60% of the rated capacity, which cannot meet their practical application under this working condition.

[0004] Among them, in the O phase structure, sodium ions occupy the central site of the NaO6 octahedron. This structure can accommodate more Na, so it exhibits a higher specific capacity, but the sodium ion transmission rate is low, resulting in poor rate performance. The P phase structure usually has a lower Na concentration, and the sodium ions occupy the central site of the NaO6 triangular column structure. The sodium layer spacing is larger, and the activation energy of sodium ion diffusion is lower, so it has better rate performance. That is, there are problems with both the O phase structure and the P phase structure.

[0005] Therefore, how to obtain a sodium ion layered oxide material with both high capacity and high rate is a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a sodium positive electrode material and a preparation method thereof and a sodium ion battery. The sodium positive electrode material provided by the present invention incorporates aluminum in a specific P3 phase structure, thereby having more excellent gram capacity and rate performance.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a sodium battery positive electrode material, wherein the sodium battery positive electrode material has a P3 phase structure and comprises nickel, manganese and aluminum.

[0009] The sodium positive electrode material provided by the present invention is doped with aluminum under a specific P3 phase structure. The P3 phase structure type and the aluminum doping cooperate with each other. The presence of aluminum can inhibit the formation of the NaO6 octahedral structure and facilitate the synthesis of the triangular prism structure, thereby obtaining a better and purer P3 phase layered oxide structure. In the P3 phase structure of the sodium positive electrode material, sodium ions occupy the central site of the NaO6 triangular prism structure, the sodium layer spacing is larger, and the activation energy of sodium ion diffusion is lower, thereby having more excellent gram capacity and rate performance.

[0010] In the present invention, the P-phase structure and the doping of aluminum must cooperate with each other and are indispensable; if aluminum is not doped, it is not conducive to the formation of the triangular prism structure, and the P-phase structure with higher purity cannot be obtained; and if aluminum is doped, but it is other phase structure types, such as P2 phase or O phase, the problem of slow sodium ion transmission rate cannot be solved, and a positive electrode material with excellent gram capacity and rate performance cannot be obtained.

[0011] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0012] Preferably, the chemical formula of the sodium positive electrode material is Na a Ni xMn y Al z O2, wherein 0.65≤a≤0.75, 0.15≤x≤0.25, 0.55≤y≤0.65, 0.15≤z≤0.25, x+y+z=1.

[0013] For example, a may be 0.65, 0.66, 0.67, 0.68, 0.69, 0.7, 0.71, 0.72, 0.73, 0.74 or 0.75, etc.; x may be 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24 or 0.25, etc.; y may be 0.55, 0.56, 0.57, 0.58, 0.59, 0.60, 0.61, 0.62, 0.63, 0.64 or 0.65, etc. 6, 0.57, 0.58, 0.59, 0.6, 0.61, 0.62, 0.63, 0.64 or 0.65, etc.; the z can be 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24 or 0.25, etc.; but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] In the present invention, by further regulating the molar ratio of sodium and the molar ratio of aluminum, a better and purer P3 phase layered oxide structure can be obtained; and if the molar ratio of sodium is too high or too low, it will lead to the formation of O phase structure and P2 phase structure; and if the molar ratio of aluminum is too high or too low, it will also affect the purity of the final P3 phase structure.

[0015] In a second aspect, the present invention provides a method for preparing the sodium positive electrode material as described in the first aspect, the preparation method comprising the following steps:

[0016] The sodium positive electrode material is obtained by mixing a nickel-manganese-aluminum-sodium electric precursor and a sodium source and sintering them.

[0017] The preparation method provided by the present invention incorporates aluminum in the precursor stage, and after subsequent sintering, a purer P3 phase structure can be obtained, thereby improving the capacity and rate performance of the obtained sodium battery positive electrode material; and the preparation method is simple to operate and is suitable for large-scale industrial production.

[0018] Preferably, the chemical formula of the nickel manganese aluminum sodium precursor is Ni x Mn y Al z (OH)2, wherein 0.15≤x≤0.25, 0.55≤y≤0.65, 0.15≤z≤0.25, x+y+z=1.

[0019] For example, the x can be 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24 or 0.25, etc.; the y can be 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, 0.61, 0.62, 0.63, 0.64 or 0.65, etc.; the z can be 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24 or 0.25, etc.; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] Preferably, the average particle size of the nickel manganese aluminum sodium electrical precursor is 4 to 10 μm, for example 4.0 μm, 5.0 μm, 6.0 μm, 7.0 μm, 8.0 μm, 9.0 μm or 10.0 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the method for preparing the nickel-manganese-aluminum-sodium electrical precursor comprises:

[0022] The nickel-manganese-aluminum mixed salt solution, the precipitant solution and the complexing agent solution are added in parallel to perform a co-precipitation reaction to obtain the nickel-manganese-aluminum-sodium electrical precursor material.

[0023] Preferably, the temperature of the coprecipitation reaction is 20-70°C, for example, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the pH value of the coprecipitation reaction is 8 to 12, for example 8, 8.3, 8.5, 8.8, 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8, 11, 11.3, 11.5, 11.8 or 12, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] In the present invention, a precursor material uniformly doped with aluminum in the bulk phase can be obtained by a coprecipitation method; and in addition to the regulation of the molar amount of aluminum during the coprecipitation process, the concentration of the raw materials, the feed flow rate and other specific preparation processes can be adaptively selected and adjusted by those skilled in the art according to actual needs;

[0026] The present invention does not limit the type of metal salt in the mixed salt solution, the type of precipitant in the precipitant solution, and the type of complexing agent in the complexing agent solution. The present invention is applicable to any conventional type that can be used in the coprecipitation reaction process.

[0027] Optionally, the type of the mixed salt includes but is not limited to at least one of sulfate, chloride, nitrate or acetate, etc.; the precipitant includes but is not limited to alkali (sodium hydroxide solution and / or potassium hydroxide solution, etc.) and / or carbonate precipitant (such as sodium carbonate solution and / or sodium bicarbonate solution, etc.); the complexing agent includes but is not limited to at least one of sodium citrate, tetrasodium ethylenediaminetetraacetate, ammonium bicarbonate, ammonium carbonate or ammonia water, etc.;

[0028] Optionally, the total concentration of metal ions in the nickel-manganese-aluminum mixed salt solution is 0.5 to 5 mol / L, such as 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L or 5 mol / L, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0029] Optionally, the concentration of the precipitant solution is 2 to 15 mol / L, for example, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0030] Optionally, the concentration of the complexing agent solution is 4 to 12 mol / L, such as 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L or 12 mol / L, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0031] Optionally, the feed rate of the nickel-cobalt-manganese mixed salt solution is 4 to 100 L / h, for example, 4 L / h, 5 L / h, 10 L / h, 20 L / h, 30 L / h, 40 L / h, 50 L / h, 60 L / h, 70 L / h, 80 L / h, 90 L / h or 100 L / h, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0032] Optionally, the feed rate of the precipitant solution is 1 to 20 L / h, such as 1 L / h, 3 L / h, 5 L / h, 8 L / h, 10 L / h, 13 L / h, 15 L / h, 18 L / h or 20 L / h, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0033] Optionally, the feeding rate of the complexing agent solution is 0.5 to 10 L / h, such as 0.5 L / h, 1 L / h, 2 L / h, 3 L / h, 4 L / h, 5 L / h, 6 L / h, 7 L / h, 8 L / h, 9 L / h or 10 L / h, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0034] Optionally, during the reaction, the reaction container may include a base liquid, that is, the reaction solution is added to the base liquid in parallel, the base liquid may include water, a precipitant and a complexing agent, the pH value of the base liquid is 8 to 13, for example, 8, 8.3, 8.5, 8.8, 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8, 11, 11.3, 11.5, 11.8, 12, 12.3, 12.5, 12.8 or 13, etc., the concentration of the complexing agent in the base liquid is 0 to 2 mol / L, for example, 0 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L or 2 mol / L, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0035] Optionally, after the coprecipitation reaction is completed, alkali washing and water washing are performed in sequence, and then drying is performed to obtain a nickel-manganese-aluminum-sodium electrical precursor;

[0036] Those skilled in the art may refer to the above specific preparation process and make adaptive selections and adjustments according to actual needs.

[0037] Preferably, the molar ratio of the sum of the total molar amounts of all metal elements in the nickel-manganese-aluminum-sodium electrical precursor to the sodium in the sodium source is 1:(0.65-0.75), for example 1:0.65, 1:0.66, 1:0.67, 1:0.68, 1:0.69, 1:0.7, 1:0.71, 1:0.72, 1:0.73, 1:0.74 or 1:0.75, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0038] In the present invention, by adjusting the molar ratio of the sum of the total molar amounts of all metal elements in the nickel-manganese-aluminum-sodium electrical precursor to the sodium in the sodium source to be 1:(0.65-0.75), the generation of the O phase structure in the subsequent sintering process is avoided, thereby obtaining a relatively pure P phase structure.

[0039] Preferably, the sintering atmosphere is an oxygen-containing atmosphere.

[0040] In the present invention, the oxygen-containing atmosphere refers to an atmosphere containing oxygen, including but not limited to an oxygen atmosphere or an air atmosphere.

[0041] Preferably, the sintering temperature is 650-750°C, for example 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C or 750°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] In the present invention, by adjusting the sintering temperature to 650-750° C., the formation of the P2 phase structure can be better suppressed, and finally a high-purity aluminum-doped P3 phase structure with better rate performance and capacity is prepared.

[0043] Preferably, the sintering time is 12 to 20 hours, for example 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] As a preferred technical solution, the preparation method comprises the following steps:

[0045] Adding a nickel-manganese-aluminum mixed salt solution, a precipitant solution and a complexing agent solution in parallel for a co-precipitation reaction to obtain the nickel-manganese-aluminum-sodium electrical precursor material;

[0046] A nickel-manganese-aluminum-sodium electric precursor and a sodium source are mixed, wherein the molar ratio of the sum of the total molar amounts of all metal elements in the nickel-manganese-aluminum-sodium electric precursor to the sodium in the sodium source is 1:(0.65-0.75), and the mixture is sintered at 650-750° C. for 12-20 hours in an oxygen-containing atmosphere to obtain the sodium electric positive electrode material.

[0047] In a third aspect, the present invention further provides a sodium ion battery, comprising the sodium positive electrode material as described in the first aspect or the sodium positive electrode material prepared by the preparation method as described in the second aspect.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] The sodium positive electrode material provided by the present invention is doped with aluminum under a specific P3 phase structure. The P3 phase structure type and the aluminum doping cooperate with each other. The presence of aluminum can inhibit the formation of the NaO6 octahedral structure and is beneficial to the synthesis of the triangular prism structure, thereby obtaining a better and purer P3 phase layered oxide structure. In the P3 phase structure of the sodium positive electrode material, sodium ions occupy the central site of the NaO6 triangular prism structure, the sodium layer spacing is larger, and the activation energy of sodium ion diffusion is lower, thereby having more excellent gram capacity and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 This is the SEM image of the nickel-manganese-aluminum-sodium electrical precursor provided in Example 1.

[0051] Figure 2 This is the XRD diagram of the sodium positive electrode material provided in Example 1. DETAILED DESCRIPTION

[0052] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0053] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.

[0054] Example 1

[0055] This embodiment provides a sodium positive electrode material, the sodium positive electrode material has a P3 phase structure, and the chemical formula of the sodium positive electrode material is Na 0.7 Ni 0.2 Mn 0.6 Al 0.2 O2.

[0056] The preparation method of the sodium positive electrode material is as follows:

[0057] (1) mixing nickel-manganese-aluminum salt solutions at a nickel-manganese-aluminum metal molar ratio of 0.2:0.6:0.2 to obtain a mixed metal salt solution with a total metal ion concentration of 2 mol / L;

[0058] Add the mixed metal salt solution, 10 mol / L sodium hydroxide solution of the precipitant solution and 8 mol / L ammonia solution of the complexing agent solution in parallel into the base solution having a pH value of 12.0 and an ammonia concentration of 0.7 mol / L;

[0059] During the parallel addition process, the feed rate of the mixed metal salt solution was 40 L / h. The pH value of the reaction system was controlled between 11.4 and 11.6, and the ammonia concentration was controlled between 0.6 and 0.8 mol / L by controlling the flow rates of the sodium hydroxide solution and the ammonia water. The coprecipitation reaction was carried out at a reaction temperature of 52° C. under nitrogen protection. The reaction was stopped after 50 hours of reaction when the average particle size reached 6.0 μm.

[0060] The product after the coprecipitation reaction is subjected to a centrifugal washing process of alkali washing and water washing in sequence, and dried at 150° C. to obtain a nickel-manganese-aluminum-sodium electrical precursor;

[0061] (2) Sodium carbonate and sodium nickel manganese aluminum electric precursor are mixed evenly according to a molar ratio of Na:Me (Me is the sum of the total molar amounts of nickel manganese and aluminum) of 0.70:1, sintered at a sintering temperature of 700°C for 16 hours in a tubular furnace under oxygen flow, and ground and sieved to obtain the sodium electric positive electrode material.

[0062] Figure 1 The SEM image of the nickel-manganese-aluminum-sodium electric precursor provided in Example 1 is shown. Figure 1 It can be seen that the nickel-manganese-aluminum-sodium electrical precursor provided in Example 1 has a uniform particle size distribution and good sphericity.

[0063] Figure 2 The XRD pattern of the sodium positive electrode material provided in Example 1 is shown. Figure 2 It can be seen that the sodium positive electrode material provided in Example 1 has a good P3 phase layered structure and high purity without obvious impurity phase generation.

[0064] Example 2

[0065] This embodiment provides a sodium positive electrode material, the sodium positive electrode material has a P3 phase structure, and the chemical formula of the sodium positive electrode material is Na 0.75 Ni 0.25 Mn 0.58 Al 0.17 O2.

[0066] The preparation method of the sodium positive electrode material is as follows:

[0067] (1) mixing nickel-manganese-aluminum salt solutions at a metal molar ratio of nickel-manganese-aluminum of 0.25:0.58:0.17 to obtain a mixed metal salt solution having a total metal ion concentration of 1.5 mol / L;

[0068] Add the mixed metal salt solution, 10 mol / L sodium hydroxide solution of the precipitant solution and 8 mol / L ammonia solution of the complexing agent solution in parallel into the base solution with a pH value of 11.5 and an ammonia concentration of 0.5 mol / L;

[0069] During the parallel addition process, the feed rate of the mixed metal salt solution was 10 L / h. The pH value of the reaction system was controlled between 11.0 and 11.2, and the ammonia concentration was controlled between 0.4 and 0.6 mol / L by controlling the flow rates of the sodium hydroxide solution and the ammonia water. The coprecipitation reaction was carried out at a reaction temperature of 45° C. under nitrogen protection. The reaction lasted for 70 hours, and the reaction was stopped when the average particle size reached 7 μm.

[0070] The product after the coprecipitation reaction is subjected to a centrifugal washing process of alkali washing and water washing in sequence, and dried at 150° C. to obtain a nickel-manganese-aluminum-sodium electrical precursor;

[0071] (2) Sodium carbonate and sodium nickel manganese aluminum electric precursor are mixed evenly according to a molar ratio of Na:Me (Me is the sum of the total molar amounts of nickel manganese and aluminum) of 0.75:1, sintered at a sintering temperature of 740°C for 12 hours in a tubular furnace under oxygen flow, and ground and sieved to obtain the sodium electric positive electrode material.

[0072] Example 3

[0073] This embodiment provides a sodium positive electrode material, the sodium positive electrode material has a P3 phase structure, and the chemical formula of the sodium positive electrode material is Na 0.65 Ni 0.2 Mn 0.65 Al 0.15 O2.

[0074] The preparation method of the sodium positive electrode material is as follows:

[0075] (1) mixing nickel-manganese-aluminum salt solutions at a metal molar ratio of nickel-manganese-aluminum of 0.2:0.65:0.15 to obtain a mixed metal salt solution with a total metal ion concentration of 2 mol / L;

[0076] Add the mixed metal salt solution, 10 mol / L sodium hydroxide solution of the precipitant solution and 8 mol / L ammonia solution of the complexing agent solution in parallel into the base solution having a pH value of 12.0 and an ammonia concentration of 0.7 mol / L;

[0077] During the parallel addition process, the feed rate of the mixed metal salt solution was 40 L / h. The pH value of the reaction system was controlled between 11.4 and 11.6, and the ammonia concentration was controlled between 0.6 and 0.8 mol / L by controlling the flow rates of the sodium hydroxide solution and the ammonia water. The coprecipitation reaction was carried out at a reaction temperature of 52° C. under nitrogen protection. The reaction was stopped after 50 hours of reaction when the average particle size reached 6.0 μm.

[0078] The product after the coprecipitation reaction is subjected to a centrifugal washing process of alkali washing and water washing in sequence, and dried at 150° C. to obtain a nickel-manganese-aluminum-sodium electrical precursor;

[0079] (2) Sodium carbonate and sodium nickel manganese aluminum electric precursor are mixed evenly according to a molar ratio of Na:Me (Me is the sum of the total molar amounts of nickel manganese and aluminum) of 0.65:1, sintered at a sintering temperature of 650°C for 20 hours in a tubular furnace under oxygen flow, and ground and sieved to obtain the sodium electric positive electrode material.

[0080] Example 4

[0081] The difference between this embodiment and embodiment 1 is that the chemical formula of the sodium positive electrode material in this embodiment is Na 0.78 Ni 0.2 Mn 0.6 Al 0.2 O2.

[0082] In the preparation method, the Na:Me (Me is the sum of the total molar amounts of nickel, manganese and aluminum) in step (2) is 0.78:1.

[0083] The rest of the preparation methods and parameters were the same as those in Example 1.

[0084] Example 5

[0085] The difference between this embodiment and embodiment 1 is that the chemical formula of the sodium positive electrode material in this embodiment is Na 0.6 Ni 0.2 Mn 0.6 Al 0.2 O2.

[0086] In the preparation method, the Na:Me (Me is the sum of the total molar amounts of nickel, manganese and aluminum) in step (2) is 0.6:1.

[0087] The rest of the preparation methods and parameters were the same as those in Example 1.

[0088] Example 6

[0089] The difference between this embodiment and embodiment 1 is that the chemical formula of the sodium positive electrode material in this embodiment is Na 0.7 Ni 0.25 Mn 0.65 Al 0.1 O2;

[0090] In the preparation method, the nickel-manganese-aluminum salt solution in step (1) has a metal molar ratio of nickel-manganese-aluminum of 0.25:0.65:0.1

[0091] The rest of the preparation methods and parameters were the same as those in Example 1.

[0092] Example 7

[0093] The difference between this embodiment and embodiment 1 is that the chemical formula of the sodium positive electrode material in this embodiment is Na 0.7 Ni 0.15 Mn 0.55 Al 0.3 O2;

[0094] In the preparation method, the nickel-manganese-aluminum salt solution in step (1) has a metal molar ratio of nickel-manganese-aluminum of 0.15:0.55:0.3.

[0095] The rest of the preparation methods and parameters were the same as those in Example 1.

[0096] Example 8

[0097] The difference between this embodiment and embodiment 1 is that the sintering temperature in step (2) of this embodiment is 600°C.

[0098] The rest of the preparation methods and parameters were the same as those in Example 1.

[0099] Example 9

[0100] The difference between this embodiment and embodiment 1 is that the sintering temperature in step (2) of this embodiment is 850°C.

[0101] The rest of the preparation methods and parameters were the same as those in Example 1.

[0102] Comparative Example 1

[0103] The difference between this comparative example and Example 1 is that the sodium positive electrode material provided in this comparative example is not doped with aluminum, and the chemical formula of the sodium positive electrode material is Na 0.7 Ni 0.25 Mn 0.75 O2.

[0104] In the preparation method, step (1) is a nickel-manganese mixed salt solution, and the nickel-manganese salt solution has a metal molar ratio of nickel and manganese of 0.25:0.75.

[0105] The rest of the preparation methods and parameters were the same as those in Example 1.

[0106] Comparative Example 2

[0107] The difference between this comparative example and Example 1 is that the sodium positive electrode material in this comparative example is an O3 phase structure, and the chemical formula of the sodium positive electrode material is Na1Ni 0.25 Mn 0.75 O2;

[0108] In the preparation method, the Na:Me (Me is the sum of the total molar amounts of nickel, manganese and aluminum) in step (2) is 1:1.

[0109] The rest of the preparation methods and parameters were the same as those in Example 1.

[0110] [Battery preparation and performance testing]

[0111] The sodium positive electrode materials provided in Examples 1-9 and Comparative Examples 1-2 are respectively used as positive electrode materials, and the positive electrode material, polyvinylidene fluoride (PVDF) and conductive carbon black are mixed in a mass ratio of 8:1:1 and dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, so that there are no particles inside the slurry, and the slurry is evenly coated on an aluminum foil on a coating machine to make a pole piece; the coated pole piece is placed in a vacuum drying oven at a temperature of 120° C. and vacuum dried for 12 hours, and the pole piece is taken out and rolled on a roller press for standby use; the pole piece is cut with a sheet cutting machine The circular electrode piece with a diameter of 12 mm was cut into pieces, placed in a vacuum drying oven and dried at 60°C for 12 h, then taken out and weighed with an electronic balance. Finally, the positive electrode piece, sodium piece, spring, gasket, positive electrode shell, negative electrode shell, diaphragm and electrolyte were assembled into a CR2025 button half-cell in a glove box filled with argon. The electrolyte was an electrolyte formed by dissolving 1 M NaPF6 in a mixture of EC (ethylene carbonate) and DMC (dimethyl carbonate) (EC:DMC=1:1 by volume), and the metal sodium sheet was the counter electrode.

[0112] The batteries provided in Examples 1-9 and Comparative Examples 1-2 were subjected to performance tests, and then electrochemical performance tests were performed at 25°C, in the voltage range of 1.5-4.0V, at discharge current densities of 50mA / g and 800mA / g, respectively. The rate performance test was the ratio of the capacity at a discharge current density of 800mA / g to the capacity at a discharge current density of 50mA / g. The test results are shown in Table 1.

[0113] Table 1

[0114]

[0115]

[0116] Depend on Figure 1-Figure 2 From Table 1, we can get:

[0117] It can be seen from the data results of Example 1 and Examples 4-7 that by further adjusting the stoichiometric ratio of sodium and aluminum, a better and purer P3 phase layered oxide structure can be obtained, which can better improve the discharge capacity and rate performance.

[0118] From the data results of Example 1 and Examples 8 and 9, it can be seen that if the sintering temperature in the present invention is too high, more P2 phase structures will be formed, which will further affect the discharge capacity of the positive electrode material. If the sintering temperature is too low, it is not conducive to obtaining a well-structured layered oxide positive electrode material and will also affect the electrochemical properties of the positive electrode material.

[0119] It can be seen from the data results of Example 1 and Comparative Examples 1-2 that in the present invention, the phase structure of the sodium cathode material and the doping of aluminum must cooperate with each other and are indispensable. Without any one of the conditions, it is impossible to obtain a sodium cathode material with excellent gram capacity and rate performance.

[0120] In summary, the sodium positive electrode material provided by the present invention is doped with aluminum under a specific P3 phase structure. The P3 phase structure type cooperates with the aluminum doping. The presence of aluminum can inhibit the formation of the NaO6 octahedral structure and is beneficial to the synthesis of the triangular prism structure, thereby obtaining a better and purer P3 phase layered oxide structure. The P3 phase structure of the sodium positive electrode material, the sodium ions occupy the central site of the NaO6 triangular prism structure, the sodium interlayer spacing is larger, and the activation energy of the sodium ion diffusion is lower, thereby having more excellent gram capacity and rate performance.

[0121] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A sodium positive electrode material, characterized in that: The sodium battery positive electrode material has a P3 phase structure and includes nickel, manganese and aluminum.

2. The sodium positive electrode material according to claim 1, characterized in that The chemical formula of the sodium positive electrode material is Na a Ni x Mn y Al z O2, wherein 0.65≤a≤0.75, 0.15≤x≤0.25, 0.55≤y≤0.65, 0.15≤z≤0.25, x+y+z=1.

3. A method for preparing a sodium positive electrode material as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: The sodium positive electrode material is obtained by mixing a nickel-manganese-aluminum-sodium electric precursor and a sodium source and sintering them.

4. The preparation method according to claim 3, characterized in that: The chemical formula of the nickel-manganese-aluminum-sodium electrical precursor is Ni x Mn y Al z (OH)2, wherein 0.15≤x≤0.25, 0.55≤y≤0.65, 0.15≤z≤0.25, x+y+z=1; Preferably, the average particle size of the nickel-manganese-aluminum-sodium electrical precursor is 4 to 10 μm.

5. The preparation method according to claim 3 or 4, characterized in that: The preparation method of the nickel-manganese-aluminum-sodium electrical precursor comprises: The nickel-manganese-aluminum mixed salt solution, the precipitant solution and the complexing agent solution are added in parallel to perform a co-precipitation reaction to obtain the nickel-manganese-aluminum-sodium electrical precursor material.

6. The preparation method according to claim 5, characterized in that: The temperature of the coprecipitation reaction is 20 to 70° C. Preferably, the pH value of the coprecipitation reaction is 8-12.

7. The preparation method according to any one of claims 3 to 6, characterized in that: The molar ratio of the sum of the total molar amounts of all metal elements in the nickel-manganese-aluminum-sodium electrical precursor to the sodium in the sodium source is 1:(0.65-0.75).

8. The preparation method according to any one of claims 3 to 7, characterized in that: The sintering atmosphere is an oxygen-containing atmosphere; Preferably, the sintering temperature is 650-750°C; Preferably, the sintering time is 12 to 20 hours.

9. The preparation method according to claim 3, characterized in that: The preparation method comprises the following steps: Adding a nickel-manganese-aluminum mixed salt solution, a precipitant solution and a complexing agent solution in parallel for a co-precipitation reaction to obtain the nickel-manganese-aluminum-sodium electrical precursor material; A nickel-manganese-aluminum-sodium electric precursor and a sodium source are mixed, wherein the molar ratio of the sum of the total molar amounts of all metal elements in the nickel-manganese-aluminum-sodium electric precursor to the sodium in the sodium source is 1:(0.65-0.75), and the mixture is sintered at 650-750° C. for 12-20 hours in an oxygen-containing atmosphere to obtain the sodium electric positive electrode material.