Layered oxide sodium-ion battery positive electrode material with high interface entropy as well as preparation method and application of layered oxide sodium-ion battery positive electrode material

By building a high-entropy layer on the interface, the problem of unstable structure of the positive electrode material of layered transition metal oxide sodium ion battery is solved, and the efficient circulation and electrochemical performance of the material is improved, simplified the synthesis process, suitable for large-scale Large-scale production.

CN118899433AActive Publication Date: 2024-11-05INST OF CHEM CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410926326.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The positive electrode material of the layered transition metal oxide sodium ion battery is unstable due to interface side reactions during the circulation process, resulting in electrolyte penetration and capacity attenuation, limiting its practical application.

Method used

By constructing an interface high-entropy layer, using multi-variable doping and process optimization of heavy elements, a high-entropy layer is formed, which improves the interface stability of the material, avoids the dissolution of transition metals and catalytic decomposition of electrolytes, and simplifies the synthesis process.

Benefits of technology

It significantly improves the long cycle performance and electrochemical performance of the material, avoids interface structure degradation and capacity attenuation, simplifies the synthesis process, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899433A_ABST
    Figure CN118899433A_ABST
Patent Text Reader

Abstract

The invention provides an interface high-entropy layered oxide sodium ion battery positive electrode material and a preparation method and application thereof, the chemical formula expression of the positive electrode material is NaNixFeyMnzAaBbCcDdO2, x + y + z + a + b + c + d = 1, a + b + c + d is less than or equal to 0.1, a is greater than 0, b is greater than 0, c is greater than 0, d is greater than or equal to 0, A is at least one of Y, Zr and Nb, B is at least one of lanthanide or Ta and W, and C and D are at least one of transition metal elements in the fourth period and the fifth period. The preparation method of the positive electrode material is simple in process and suitable for large-scale production. By adjusting the adding sequence of the doping source, the characteristic that transition metal elements in the fourth period and the fifth period tend to surface segregation is utilized, an interface high-entropy spinel structure is constructed through trace multi-element doping, all the doping elements are evenly distributed, the interface structure stability of the material is enhanced, and the cycle performance of the material is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical power sources, and in particular relates to the preparation and application of a type of interfacial high-entropy layered oxide sodium ion battery positive electrode material. Background Art

[0002] Lithium-ion batteries are currently the most widely used secondary batteries, and have been widely used in fields such as mobile phones, computers and electric vehicles. However, the shortage of lithium resources and the uneven distribution of lithium resources around the world have severely restricted the large-scale use of lithium-ion batteries. In contrast, sodium-ion batteries are considered to have good application prospects in the field of large-scale energy storage due to their rich sodium resources and wide sources, and thus their low cost.

[0003] Among the many cathode materials for sodium-ion batteries, layered transition metal oxides Na x TMO 2 (TM is a transition metal) has attracted extensive attention from researchers due to its advantages such as high specific capacity, high energy density and simple preparation method. However, during the cycle, layered transition metal oxides will undergo serious interfacial side reactions due to the dissolution of transition metals and the decomposition of transition metal-catalyzed electrolytes. This unfavorable interfacial side reaction will lead to the degradation of the layered structure of the interface, resulting in poor interfacial structural stability of such materials during long cycles, resulting in cracks. Then, the electrolyte will pass through the cracks and the inside of the positive electrode particles to produce more serious side reactions, thus restricting its performance in practical applications. In order to improve the interfacial structural stability of such materials, a coating layer is usually introduced into the layered transition metal oxide layer to stabilize the interfacial structure, thereby improving the cycle performance and inhibiting capacity decay. However, the construction method of the coating layer is generally more complicated, and due to the poor air stability of the layered transition metal oxide, it is easy to cause the material to fail during the coating post-treatment process. However, the construction of a surface high entropy structure can achieve modification in one step, without a post-treatment process, simplifying the process, and avoiding the failure of the synthesized positive electrode material exposed to the air, so this method is simpler, more convenient and more efficient. Summary of the invention

[0004] In view of this, the present invention solves the above-mentioned problem by modifying the layered positive electrode material by constructing an interface high entropy layer. In the synthesis process, heavy elements are directly doped with multivariate traces. The preparation method is simple and the effect is significant. The heavy elements are more inclined to surface segregation through process optimization, so that a high entropy layer is formed in the interface layer. The high entropy layer is conducive to improving the stability of the structure, avoiding the structural degradation of the layered phase on the surface during the cycle, thereby avoiding the dissolution of transition metals and the catalytic decomposition of transition metals on the electrolyte, improving the interface stability of the material, avoiding the generation of surface cracks, solving the capacity decay caused by interface problems, and effectively improving the long cycle performance of the material. In addition, the high entropy interface layer is conducive to improving the solid solubility of heavy elements, reducing the presence of impurities, and improving electrochemical performance. Traditional high entropy materials require similar content of each element in the component, and the high entropy effect cannot be achieved if the content of the doping element is too little, and the content is too much. It will not provide enough active pairs, which greatly limits the capacity of the high entropy material. The present invention optimizes the heavy element screening and doping process. Unlike traditional high entropy materials, the construction of the interface high entropy layer ensures sufficient active element content, thereby improving the stability of the structure without losing capacity. In addition, the construction of the interface high entropy layer reduces the content of active elements on the interface, avoiding the catalytic decomposition of the electrolyte by high-valent active elements and the dissolution of active elements.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] A layered oxide sodium ion battery positive electrode material with high interfacial entropy, characterized in that the chemical formula is NaNi x Fe y Mn z A a B b C c D d O 2 , wherein x+y+z+a+b+c+d=1, a+b+c+d≤0.1, and a>0, b>0, c>0, d≥0, wherein A is at least one of Y, Zr, and Nb, B is a lanthanide element or at least one of Ta and W, and C and D are at least one of the fourth and fifth period transition metal elements.

[0007] Preferably, 0.01≤a+b+c+d≤0.05.

[0008] The ratio of A, B, C must satisfy a: b: c = 1-2: 1-2: 1-2, preferably 1-1.3: 1-1.3: 1-1.3; if D element exists, A, B, C, D satisfy a: b: c: d = 1-2: 1-2: 1-2: 1-2, preferably 1-1.3: 1-1.3: 1-1.3: 1-1.3. The ratio of A, B, C, (D) elements satisfies the above ratio, that is, the content of A, B, C, (D) is close, which makes it easier to form a spinel phase structure at the interface, so that while high entropy increases the structural stability, it can also avoid the degradation of the layered phase during the cycle process.

[0009] The present invention also provides a method for preparing the above-mentioned interfacial high entropy layered oxide sodium ion battery positive electrode material, comprising the following steps:

[0010] (S1) adding a sodium source, a nickel source, an iron source, a manganese source, and an element A source, and mixing them uniformly to obtain a mixture I;

[0011] (S2) the mixture I is first calcined at 400-600° C., and after cooling, the source of elements B and C are added and mixed uniformly to obtain a mixture II; optionally, after cooling, in addition to the source of elements B and C, a source of element D is also added;

[0012] (S3) The mixture II is calcined for the second time at 800-1200°C, and after cooling, a layered oxide sodium ion battery positive electrode material with high interfacial entropy is obtained.

[0013] Since the temperature of the first calcination is low and the particle size of the precursor is large, it is difficult for the A source to diffuse into the bulk phase during the first calcination, and a spinel phase intermediate product with A uniformly enriched on the surface will be obtained. The A uniformly enriched on the surface provides a more favorable doping site for the B, C, and (D) elements. Due to the similar radius, after adding the B, C, and (D) sources, during the second calcination process, the B, C, and D elements will tend to combine with A first, thus avoiding the situation where the concentration of a certain doping source is too high in a local area, making the element distribution more uniform.

[0014] If A, B, C, (D) sources are added together in the first step of mixing, a layered oxide positive electrode modified by trace doping of A, B, C, and D will be obtained. Since the doping of inactive elements can stabilize the structure and improve the cycle performance, it cannot avoid the degradation of the interface structure during the cycle, nor does it reduce the content of active elements on the interface. Therefore, the catalytic decomposition of the electrolyte and the dissolution of transition metals are still relatively serious, and the most critical problem of failure of the layered oxide positive electrode is not solved. Therefore, its modification effect is worse than that of the layered oxide positive electrode with high entropy on the interface. If A, B, C, and D sources are added together in the second step of mixing, due to the small amount added, uneven mixing and excessive concentration of a certain doping source in the local area are prone to occur, resulting in uneven distribution of the surface high entropy layer, making the modification effect unsatisfactory.

[0015] Further, the sodium source is selected from at least one of sodium carbonate, sodium bicarbonate, sodium acetate, sodium oxalate, sodium hydroxide, sodium oxide, sodium peroxide, and sodium nitrite; the nickel, iron, and manganese source materials are selected from at least one of nickel, iron, and manganese oxides, hydroxides, sulfates, nitrates, carbonates, acetates, oxalates, and hydrates thereof;

[0016] According to the present invention, the doping element A source, B source, C source and D source required for the positive electrode are selected from at least one of the oxides, hydroxides, sulfates, nitrates, carbonates, acetates, oxalates and hydrated compounds of the doping elements.

[0017] The above sodium source materials are added according to the stoichiometric ratio determined by the general structural formula, and the sodium source materials are added at a ratio of 100%-120% of the stoichiometric ratio, and mixed evenly to form a mixture.

[0018] In the above method, the purity of the raw materials is greater than 99%, preferably ≥99.9%.

[0019] In the above method, the mixing method is not particularly limited, including manual mixing or mechanical mixing, specifically selected from at least one of mechanical ball milling, manual grinding, and mechanical grinding, wherein the ball milling mixing time is 1-50 hours, the ball mill speed is 200-1000rpm, the manual grinding time is 10-60 minutes, and the mechanical grinding time is 10-60 minutes.

[0020] The calcining atmosphere is at least one of oxygen, air, nitrogen and argon. The primary calcining temperature is 300-600°C, the holding time is 1-10h, the heating rate is 1-10°C / min, the cooling rate during cooling is 1-10°C / min, or it is cooled with the furnace. The secondary calcining temperature is 800-1200°C, the holding time is 5-40h, the heating rate is 1-10°C / min, the cooling rate during cooling is 1-10°C / min, or it is cooled with the furnace.

[0021] The present invention also provides a sodium ion battery, wherein the positive electrode comprises the above-mentioned interfacial high entropy layered oxide sodium ion battery positive electrode material.

[0022] The interfacial high entropy layered oxide sodium ion battery positive electrode material provided by the present invention can effectively realize the surface modification of doping elements A, B, and C. Since the radius of the fifth and sixth period transition metal elements is relatively large, when they are doped into the bulk phase, they will cause a large lattice distortion, which is not conducive to the stability of the structure, and thus the fifth and sixth period transition metal elements are more suitable for surface modification. After the first step of calcination, a spinel phase intermediate of nickel-iron-manganese will be formed. At this time, doping elements A, B, and C are added. Due to the slow diffusion rate, it is difficult to diffuse into the bulk phase. During the second calcination process, it is difficult to form a uniform layered oxide structure, and finally a high entropy spinel phase structure is formed on the surface. On the other hand, the fifth and sixth period transition metal elements are generally difficult to dope due to their large radius, and their solid solubility is limited, and they are easy to form a heterogeneous phase. However, the design of interfacial high entropy will reduce the Gibbs free energy in the synthesis process due to the increase in entropy, thereby making it easier to achieve the solid solution reaction process and avoid the formation of heterogeneous phases.

[0023] The second step of calcination is to add A, B, and C sources, taking advantage of the slow diffusion rate of the fifth and sixth period elements, making it difficult for them to diffuse evenly into the large particles generated after the first calcination, thereby achieving surface enrichment of the elements.

[0024] The beneficial effects of the present invention are:

[0025] 1. The interface high entropy layer in the method of the present invention can be directly formed during the calcination of the material, without the need for an additional modification process, and the synthesis process is simple and the production efficiency is high. In addition, all raw materials of the present invention are easily available, non-toxic, and low-cost, and the production process does not require special protection, has good compatibility with existing production equipment, and is suitable for large-scale production.

[0026] 2. The interfacial high entropy layered positive electrode material prepared by the present invention can significantly improve the cycle performance with less capacity loss because the inert elements are all segregated on the surface and are trace doped.

[0027] 3. The layered positive electrode material with high interfacial entropy prepared by the present invention has a stable high entropy interface structure, which improves the interface stability of the material during the cycle process, avoids the degradation of the layered phase at the interface, and effectively improves the long-cycle performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the XRD spectrum of the positive electrode prepared in Example 1.

[0029] Figure 2 This is the SEM spectrum of the positive electrode prepared in Example 1.

[0030] Figure 3 This is a cycle performance diagram of button batteries assembled with positive electrode materials of Example 1 and Comparative Example 1.

[0031] Figure 4 This is the HAADF-STEM image of the positive electrode prepared in Example 1. DETAILED DESCRIPTION

[0032] The interfacial high entropy layered oxide sodium ion battery positive electrode material of the present invention is further described below in conjunction with specific embodiments and drawings of the specification, but it should be understood that the protection scope of the present invention is not limited to the following embodiments.

[0033] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0034] Example 1

[0035] (S1) Weigh 0.105 mmol sodium carbonate and 0.02475 mmol nickel iron manganese hydroxide precursor (NiFeMn(OH) 2 ), 0.012375mmol of ferric oxide and 0.000165mmol of yttrium oxide were mixed to obtain a mixture I;

[0036] (S2) Place the mixture I in a magnetic boat, and then place it in a muffle furnace for the first calcination, with a heating rate of 5°C / min, heating to 450°C, keeping the temperature for 5 hours, and cooling to room temperature. Grind and mix the product after the first calcination with 0.00033 mmol of cerium dioxide and 0.000165 mmol of lanthanum oxide;

[0037] (S3) the mixture is placed in a muffle furnace for a second calcination at a heating rate of 5°C / min, heated to 1000°C and then kept warm for 15 hours, and then cooled to room temperature to obtain an iron-based layered oxide sodium ion battery positive electrode material;

[0038] (S4) The obtained positive electrode material, conductive additive SP, and binder PVDF are mixed in weight proportions of 80 parts, 10 parts, and 10 parts, dissolved in solvent NMP, and stirred to obtain a uniform slurry. The slurry is then evenly coated on a carbon-coated aluminum foil using a 200 μm scraper, dried, and sliced ​​to obtain a positive electrode sheet.

[0039] Figure 1 This is the XRD spectrum of the positive electrode material prepared in Example 1. It can be seen that the interface high entropy material still maintains the structure of the O3 phase and can be classified as an R3m type space group.

[0040] Figure 2 This is the SEM image of the positive electrode material prepared in Example 1. It can be seen that the interfacial high entropy positive electrode material is in the form of stacked sheets with relatively uniform particle size.

[0041] Figure 3This is a button cell cycle performance diagram of the positive electrode materials of Example 1 and Comparative Example 1.

[0042] Figure 4 This is the HAADF-STEM image of the positive electrode prepared in Example 1. It can be seen that the interface is a spinel phase structure.

[0043] Example 2

[0044] The operation steps are the same as those in Example 1, except that the mixture of 0.00033 mmol cerium dioxide, 0.000165 mmol yttrium trioxide, and 0.000165 mmol lanthanum oxide is replaced by 0.00033 mmol molybdenum dioxide, 0.000165 mmol niobium pentoxide, and 0.000165 mmol tantalum pentoxide, wherein niobium pentoxide is added as the source of element A in step (S1), and other doping element sources are added after the first calcination in step (S2).

[0045] Example 3

[0046] The operation steps are the same as those in Example 1, except that the total doping ratio of Ce, Y, and La is increased from 0.01 (a+b+c=0.01) to 0.05 (a+b+c=0.05).

[0047] Example 4

[0048] The operation steps are the same as those in Example 2, except that the doping amounts of Mo, Ta, and Nb are increased from 0.01 (a+b+c=0.01) to 0.15 (a+b+c=0.1).

[0049] Example 5

[0050] The operation steps are the same as those in Example 1, except that the mixture of 0.00033 mmol cerium dioxide, 0.000165 mmol yttrium trioxide, and 0.000165 mmol lanthanum oxide is changed to 0.00025 mmol molybdenum dioxide, 0.000125 mmol tantalum pentoxide, 0.000125 mmol niobium pentoxide, and 0.000125 mmol zirconium dioxide, wherein niobium pentoxide and zirconium dioxide are added as A sources in step (S1), and other doping element sources are added in step (S2).

[0051] Example 6

[0052] The operation steps are the same as those in Example 1, except that the mixture of 0.00033 mmol cerium dioxide, 0.000165 mmol yttrium trioxide, and 0.000165 mmol lanthanum oxide is replaced by 0.00025 mmol zirconium dioxide, 0.000125 mmol tantalum pentoxide, and 0.00025 mmol tungsten oxide.

[0053] Example 7

[0054] The operation steps are the same as those in Example 1, except that the mixture of 0.00033 mmol cerium dioxide, 0.000165 mmol yttrium trioxide, and 0.000165 mmol lanthanum oxide is replaced by 0.00025 mmol zirconium dioxide, 0.000125 mmol tantalum pentoxide, and 0.00025 mmol ruthenium dioxide.

[0055] Example 8

[0056] The operation steps are the same as those in Example 1, except that the holding time of the secondary calcination is extended from 15 hours to 20 hours.

[0057] Example 9

[0058] The operation steps are the same as those in Example 1, except that in step (S2), in addition to the cerium dioxide and lanthanum oxide doping sources, 0.000165 mmol of tantalum pentoxide is added as a D source.

[0059] Comparative Example 1

[0060] Preparation of NaNi 0.25 Fe 0.5 Mn 0.25 O 2 For the layered cathode material, 0.105 mmol sodium carbonate, 0.025 mmol nickel iron manganese hydroxide precursor, and 0.0125 mmol ferric oxide were weighed and mixed, and then manually ground for 1 hour.

[0061] The ground powder was placed in a magnetic boat, and then placed in a muffle furnace for calcination at a heating rate of 3°C / min. After heating to 450 degrees, it was kept warm for 5 hours, cooled to room temperature, and then placed in a muffle furnace for calcination at a heating rate of 5°C / min. After heating to 1000 degrees, it was kept warm for 15 hours. After cooling to room temperature, it was transferred to a hand box for standby use. The obtained positive electrode material, conductive additive SP, and binder PVDF were mixed in 80 parts, 10 parts, and 10 parts by weight, dissolved in the solvent NMP, and stirred to obtain a uniform slurry. Then, the slurry was evenly coated on the carbon-coated aluminum foil using a 200μm scraper, dried, and sliced ​​to obtain a positive electrode sheet.

[0062] Comparative Example 2

[0063] (S1) Weigh 0.105 mmol sodium carbonate and 0.02475 mmol nickel iron manganese hydroxide precursor (NiFeMn(OH) 2 ), 0.012375mmol ferric oxide, to obtain mixture I;

[0064] (S2) Place the mixture I in a magnetic boat, and then place it in a muffle furnace for the first calcination, with a heating rate of 5°C / min, heating to 450°C and then keeping the temperature for 5 hours, and cooling to room temperature to obtain a primary calcination product. The primary calcination product is ground and mixed with 0.00033mmol cerium dioxide, 0.000165mmol lanthanum oxide, and 0.000165mmol yttrium trioxide;

[0065] (S3) the mixture is placed in a muffle furnace for a second calcination at a heating rate of 5°C / min, heated to 1000°C and then kept warm for 15 hours, and then cooled to room temperature to obtain an iron-based layered oxide sodium ion battery positive electrode material;

[0066] (S4) The obtained positive electrode material, conductive additive SP, and binder PVDF are mixed in weight proportions of 80 parts, 10 parts, and 10 parts, dissolved in solvent NMP, and stirred to obtain a uniform slurry. The slurry is then evenly coated on a carbon-coated aluminum foil using a 200 μm scraper, dried, and sliced ​​to obtain a positive electrode sheet.

[0067] That is, compared with Example 1, the element A source yttrium trioxide is added together with the element B and C sources after the first calcination.

[0068] Application Examples Electrochemical performance test

[0069] Electrochemical performance test: The electrode sheets obtained in Examples 1-8 and Comparative Example 1 were used as positive electrodes, the metal sodium sheet was used as negative electrodes, the glass fiber was used as a separator, and 1 mol / L NaClO 4 (PC+5% FEC) was used as the electrolyte to assemble button cells. The positive electrode was activated at a current density of 13mA / g for one cycle in the voltage range of 2.0-4.0V, then activated at a current density of 26mA / g for two cycles, and then charged and discharged at a current density of 130mA / g. The electrochemical performance of the sodium battery of the embodiment of the present invention and the comparative example was tested, and the results are shown in Table 1:

[0070] Table 1 Electrochemical performance data

[0071]

[0072] The capacity retention rate after 200 cycles is compared with the 4th cycle, and the first three cycles belong to the formation process.

[0073] from Figure 1 It can be seen that the material after interface high entropy modification still maintains the structure of the O3 phase and can be classified as the R3m type space group. Figure 2 From the SEM image, it can be seen that the particles of the positive electrode material after interface high entropy modification are smaller, the surface is smoother, and the particles are more rounded. This may be because during the calcination process, heavy elements are adsorbed on the surface of the particles, thereby affecting the growth process of the particles.

[0074] From the test results of the half-cells of each embodiment in Table 1, it can be seen that after the interfacial high entropy layer is constructed on the surface of the layered positive electrode material, the capacity retention rate of the sodium ion battery after 200 cycles is significantly improved. For example, in Example 1, the capacity retention rate is still 91.3% after 200 cycles, while Comparative Example 1 has only 61% reversible specific capacity. Due to the formation of a spinel phase on the surface due to surface high entropy doping, surface degradation during the cycle is suppressed. On the other hand, the presence of a surface high entropy structure makes the Gibbs free energy of the surface structure lower, so the structure is more stable, thereby improving the cycle stability. It is worth noting that the content of element doping needs to be appropriate. When the element content is too much, due to the influence of solid solubility, inactive impurities may be generated, which will lead to performance deterioration. In addition, when the calcination time is longer, due to the more uniform diffusion of the elements, it may cause the doped heavy element bulk phase to be uniformly distributed rather than forming an interfacial high entropy layer.

[0075] The present invention provides a type of interface high entropy layered oxide sodium ion battery positive electrode modification design ideas and preparation methods, by constructing an interface high entropy layer, enhancing the structural stability of the interface, avoiding the structural degradation of the layered phase at the interface during the cycle, can greatly improve the cycle stability of the sodium ion battery, and the synthesis process is simple and efficient, suitable for large-scale industrial production. It can be understood that in each embodiment of the present invention, although the present invention is described in detail in combination with specific electrolytes, diaphragms, current collectors, active materials, binders, conductive additives, etc., the above is only to meet legal requirements and illustrate the composition of sodium ion batteries, and the present invention is not limited to the given embodiments. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention using the present invention specification, or directly or indirectly applied in other related technical fields, are similarly included in the patent protection scope of the present invention.

Claims

1. A layered oxide sodium ion battery positive electrode material with high interfacial entropy, characterized in that: The chemical formula is NaNi x Fe y Mn z A a B b C c D d O2, wherein x+y+z+a+b+c+d=1, a+b+c+d≤0.1, and a>0, b>0, c>0, d≥0, wherein A is at least one of Y, Zr, Nb, B is a lanthanide element or at least one of Ta, W, and C, D is at least one of the fourth and fifth period transition metal elements.

2. The interfacial high entropy layered oxide sodium ion battery positive electrode material according to claim 1, characterized in that: 0.01≤a+b+c+d≤0.

05.

3. The interfacial high entropy layered oxide sodium ion battery positive electrode material according to claim 1, characterized in that: The ratio of A, B, and C must satisfy a:b:c=1-2:1-2:1-2, preferably 1-1.3:1-1.3:1-1.3; if element D exists, A, B, C, and D must satisfy a:b:c:d=1-2:1-2:1-2:1-2, preferably 1-1.3:1-1.3:1-1.3:1-1.

3.

4. The method for preparing the interfacial high entropy layered oxide sodium ion battery positive electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (S1) adding a sodium source, a nickel source, an iron source, a manganese source, and an element A source, and mixing them uniformly to obtain a mixture I; (S2) the mixture I is first calcined at 400-600° C., and after cooling, the source of elements B and C are added and mixed uniformly to obtain a mixture II; optionally, after cooling, in addition to the source of elements B and C, a source of element D is also added; (S3) The mixture II is calcined for the second time at 800-1200°C, and after cooling, a layered oxide sodium ion battery positive electrode material with high interfacial entropy is obtained.

5. The preparation method according to claim 4, characterized in that: The sodium source is selected from at least one of sodium carbonate, sodium bicarbonate, sodium acetate, sodium oxalate, sodium hydroxide, sodium oxide, sodium peroxide, and sodium nitrite; the nickel, iron, and manganese source materials are selected from at least one of nickel, iron, and manganese oxides, hydroxides, sulfates, nitrates, carbonates, acetates, oxalates, and hydrated compounds thereof.

6. The preparation method according to claim 4, characterized in that: The doping element A source, B source, C source and D source are selected from at least one of the oxides, hydroxides, sulfates, nitrates, carbonates, acetates, oxalates and hydrated compounds of the doping elements.

7. The preparation method according to claim 4, characterized in that: The sodium source material is added according to the stoichiometric ratio determined by the general structural formula, and the sodium source material is added at a ratio of 100% to 120% of the stoichiometric ratio, and mixed evenly to form a mixture; Preferably, the purity of the raw materials is greater than 99%, preferably ≥99.9%.

8. The preparation method according to claim 4, characterized in that: The mixing method includes manual mixing or mechanical mixing, specifically selected from at least one of mechanical ball milling, manual grinding, and mechanical grinding; wherein the ball milling mixing time is 1-50 hours, the ball mill speed is 200-1000rpm, the manual grinding time is 10-60 minutes, and the mechanical grinding time is 10-60 minutes.

9. The preparation method according to claim 4, characterized in that: The calcining atmosphere is at least one of oxygen, air, nitrogen and argon. The primary calcining temperature is 300-600°C, the holding time is 1-10h, the heating rate is 1-10°C / min, the cooling rate during cooling is 1-10°C / min, or it is cooled with the furnace. The secondary calcining temperature is 800-1200°C, the holding time is 5-40h, the heating rate is 1-10°C / min, the cooling rate during cooling is 1-10°C / min, or it is cooled with the furnace.

10. A sodium ion battery, characterized in that: The positive electrode comprises the interfacial high entropy layered oxide sodium ion battery positive electrode material as described in any one of claims 1 to 3.

Citation Information

Patent Citations

  • Layered sodium ion medium-high entropy composite oxide positive electrode material

    CN115863625A

  • High-entropy doped manganese-based layered oxide, preparation method thereof, sodium ion battery positive electrode material and battery

    CN116062807A

  • Dual-doped lithium-rich solid solution positive electrode composite and preparation method thereof, lithium-ion battery positive electrode plate, and lithium-ion battery