Lithium titanate battery and electrolyte thereof
By using electrolytes of components such as fluorinated nitrile compounds and ether compounds in lithium titanate batteries, the problem of difficulty in transmission and desolvation in low-temperature environments is solved, and the low-temperature energy storage and Battery performance.
Patent Information
- Application Number
- CN202411102062.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-05
AI Technical Summary
Under low temperature environment, the Li+ of the lithium titanate battery has difficulty in transporting and desolvating in the electrolyte, which affects the performance of the battery.
Fluorinated nitrile compounds are used as the main solvent, and combined with ether compounds and mixed additives to form an electrolyte solution of lithium titanate batteries. Fluorinated nitrile compounds have weak interactions with Li+, and fluorine atoms have strong absorption Electronic capability weakens the interaction between solvent molecules and Li+, thereby achieving faster desolvation of Li+ and optimizing the performance of electrolyte at low temperatures.
It improves the energy storage performance and battery performance of lithium titanate batteries at low temperatures, suppresses the negative impact of low temperatures on battery performance, and improves the performance and cycle life of the battery.
Smart Images

Figure BDA0004989635790000121 
Figure BDA0004989635790000131 
Figure BDA0004989635790000132
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery electrolyte materials, and in particular to an electrolyte for a lithium titanate battery and a lithium titanate battery. Background Art
[0002] With the continuous growth of energy demand, energy storage technology plays an increasingly important role in achieving stable energy supply, improving energy utilization efficiency and reducing environmental pollution. Among them, lithium-ion batteries have the advantages of high energy density and long cycle life, and have received widespread attention. However, the harsh climate in cold regions such as Tibet, northern China and northern Europe makes it difficult for the current traditional nickel-cobalt-manganese ternary batteries and lithium iron phosphate batteries to meet the requirements of backup power and energy supply. Therefore, batteries with lithium titanate negative electrodes that perform better at low temperatures of -20°C or even -40°C have broader application prospects. However, due to the low temperature environment, the performance of lithium titanate batteries will also be restricted by multiple factors, such as Li + In the bulk electrolyte, it is difficult to transport Li + Difficulty in desolvation, etc. In order to further optimize the performance of lithium titanate batteries in low-temperature energy storage and suppress the negative impact of low temperature on its performance, it is urgent to develop an electrolyte for lithium titanate batteries suitable for low-temperature environments. Summary of the invention
[0003] In order to solve the above technical problems, the present application provides an electrolyte for a lithium titanate battery and a lithium titanate battery.
[0004] In order to achieve the above-mentioned purpose, according to the first aspect of the present technical solution, the present technical solution provides an electrolyte for a lithium titanate battery.
[0005] The electrolyte of the lithium titanate battery provided in the embodiment of the present application includes a lithium salt and an organic solvent, wherein the organic solvent includes a fluorinated nitrile compound.
[0006] Furthermore, in the electrolyte of the lithium titanate battery, the fluorinated nitrile compound is at least one of fluoroacetonitrile, 4,4,4-trifluorobutyronitrile, 3-amino-4,4,4-trifluorobutyronitrile, and 3,3,3-trifluoropropionitrile.
[0007] Furthermore, in the electrolyte of the lithium titanate battery, the organic solvent also includes an ether compound, and the ether compound is a crown ether compound and / or a cryptand compound.
[0008] Furthermore, in the electrolyte of the lithium titanate battery, the ether compound is at least one of 18-crown ether-6, benzo-18-crown ether-6, benzo-15-crown ether-5, dicyclohexane-18-crown ether-6, and [2,2,2]-cryptand.
[0009] Furthermore, in the electrolyte of the lithium titanate battery, the organic solvent also includes a mixed additive, and the mixed additive is at least two of 3-methoxypropionitrile, acetic anhydride, amyl acetate, isobutyl acetate and isopropyl alcohol.
[0010] Furthermore, in the electrolyte of the lithium titanate battery, the lithium salt is at least one of LITFSI, LIFSI, LiDFOB, and LiBF4.
[0011] Furthermore, in the electrolyte of the lithium titanate battery, the lithium salt is LITFSI and LiDFOB in a molar ratio of 1:1.
[0012] Furthermore, in the electrolyte of the lithium titanate battery, the concentration of the lithium salt is 1M-10M.
[0013] Furthermore, in the electrolyte of the lithium titanate battery, the organic solvent includes 70 to 100 wt % of a fluorinated nitrile compound, 0 to 30 wt % of an ether compound and 0 to 10 wt % of a mixed additive.
[0014] In order to achieve the above-mentioned purpose, according to the second aspect of the present technical solution, the present technical solution provides a lithium titanate battery, which includes the electrolyte provided by the first aspect of the present technical solution.
[0015] The present invention provides an electrolyte for a lithium titanate battery. The fluorinated nitrile compound in the electrolyte is a solvent with a low melting point and low viscosity. After the fluorinated nitrile compound is used as the main solvent of the electrolyte, the fluorinated nitrile compound reacts with Li + Has a weaker interaction, which is beneficial to reduce Li + The coordination strength with the fluorinated nitrile compound molecules, and the fluorine atoms in the fluorinated nitrile compounds have strong electron-withdrawing ability, which can further weaken the coordination strength with the solvent molecules and Li + interaction, thereby achieving Li + Faster desolvation. This can solve the problem of Li + Difficult transport in the electrolyte and Li + The technical problem of difficult desolvation is that when the electrolyte is applied to lithium titanate batteries, the performance of lithium titanate batteries in low-temperature energy storage is optimized, the negative impact of low temperature on the performance of lithium titanate batteries is suppressed, and the battery performance is improved. DETAILED DESCRIPTION
[0016] The present invention discloses an electrolyte for a lithium titanate battery. Those skilled in the art can refer to the content of this article and appropriately improve the components and ratios to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in the present invention. The products, processes and applications described in the present invention have been described through preferred embodiments. Relevant personnel can obviously modify or appropriately change and combine the products, processes and applications described herein without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0017] It should be noted that, in this document, relational terms such as "first" and "second", "step 1" and "step 2", and "(1)" and "(2)" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a..." does not exclude the presence of other identical elements in the process, method, article or device comprising the element.
[0018] Hereinafter, preferred embodiments of the present invention will be described in detail.
[0019] In order to enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present application.
[0020] The electrolyte of the lithium titanate battery provided in the embodiment of the present application mainly includes a lithium salt and an organic solvent, and the organic solvent includes a fluorinated nitrile compound.
[0021] Fluorinated nitrile compounds are low melting point, low viscosity solvents. When used as the main solvent of the electrolyte, the fluorinated nitrile compounds react with Li + Has a weaker interaction, which is beneficial to reduce Li +The coordination strength with the fluorinated nitrile compound molecules, and the fluorine atoms in the fluorinated nitrile compounds have strong electron-withdrawing ability, which can further weaken the coordination strength with the solvent molecules and Li + interaction, thereby achieving Li + Faster desolvation. This can solve the problem of Li + Difficult transport in the electrolyte and Li + The technical problem of difficult desolvation is that when the electrolyte is applied to lithium titanate batteries, the performance of lithium titanate batteries in low-temperature energy storage is optimized, the negative impact of low temperature on the performance of lithium titanate batteries is suppressed, and the battery performance is improved.
[0022] In some embodiments, the fluorinated nitrile compound in the electrolyte of the lithium titanate battery includes but is not limited to at least one of fluoroacetonitrile, 4,4,4-trifluorobutyronitrile, 3-amino-4,4,4-trifluorobutyronitrile, and 3,3,3-trifluoropropionitrile.
[0023] In some embodiments, the organic solvent in the electrolyte of the lithium titanate battery further includes an ether compound, wherein the ether compound is a crown ether compound and / or a cryptand compound. The crown ether compound or the cryptand compound can react with Li + The formation of a coated integration can enhance the solubility of lithium salts and make up for the shortcomings of fluorinated nitrile compounds in their insufficient dissociation ability for lithium salts.
[0024] Preferably, the ether compound is a crown ether compound and / or a cryptand compound with a relatively low freezing point and viscosity to meet the low temperature requirements of the electrolyte. It includes but is not limited to at least one of 18-crown-6, benzo-18-crown-6, benzo-15-crown-5, dicyclohexane-18-crown-6, and [2,2,2]-cryptand. Crown ether and cryptand solvents with relatively low freezing point and viscosity are introduced.
[0025] In some embodiments, the organic solvent of the electrolyte of the lithium titanate battery further includes a mixed additive, and the mixed additive is at least two of 3-methoxypropionitrile, acetic anhydride, amyl acetate, isobutyl acetate and isopropanol. The mixed additive is mixed with the above-mentioned multiple low melting point solvents to effectively increase the mixing entropy of the electrolyte, reduce the Gibbs free energy of the electrolyte system, enrich the solvation structure, and further broaden the working temperature of the electrolyte.
[0026] In some embodiments, the lithium salt of the electrolyte of the lithium titanate battery includes but is not limited to at least one of LITFSI, LIFSI, LiDFOB, and LiBF4. Among them, the sulfonate (LITFSI, LIFSI) has a strong perfluoroalkyl electron-withdrawing group and a stable conjugated structure, resulting in a high degree of electron delocalization, and a high solubility in solvents with low dielectric constants. Lithium difluorooxalatoborate (LiDFOB) has an extremely low salt / solvent mass ratio, so its cost is extremely low, and its viscosity is low, and its working characteristics at extreme temperatures can perfectly match the goal of low-temperature electrolytes. Compared with lithium hexafluorophosphate (LiPF6), which is the most commonly used room temperature electrolyte, lithium tetrafluoroborate (LiBF4) has a smaller charge transfer impedance at low temperatures, a smaller degree of battery polarization, and better thermal stability and hydrolysis stability. Preferably, in the electrolyte of the lithium titanate battery, the lithium salt is LITFSI and LiDFOB in a molar ratio of 1:1. The use of this new mixed lithium salt leads to a high degree of electron delocalization and a high solubility in solvents with low dielectric constants. The concentration of the lithium salt is preferably 1M-10M.
[0027] In some embodiments, the organic solvent of the electrolyte of the lithium titanate battery includes 70 to 100 wt % of a fluorinated nitrile compound, 0 to 30 wt % of an ether compound, and 0 to 10 wt % of a mixed additive.
[0028] The embodiment of the present invention also protects a lithium titanate battery, which is composed of a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte provided by the above embodiment. The negative electrode active material of the negative electrode sheet is preferably a nano lithium titanate material, and the positive electrode active material of the positive electrode sheet is preferably a lithium iron phosphate, lithium manganate, and a nickel cobalt manganese ternary material, and the separator is spaced between adjacent positive and negative electrode sheets.
[0029] Example 1
[0030] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 70wt% of fluoroacetonitrile, 20wt% of 18-crown ether-6, and 10wt% of a mixed additive, wherein the mixed additive is composed of 3-methoxypropionitrile, acetic anhydride, and amyl acetate in a mass ratio of 4:3:2. The lithium salt is a mixture of LITFSI and LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0031] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0032] Preparation of positive electrode sheets for lithium titanate batteries: spinel lithium manganate, polyvinylidene fluoride, and conductive agent Super-P are added to N-methylpyrrolidone in a mass ratio of 94:3:3 and mixed, and a slurry is obtained by stirring. The slurry is coated on a current collector aluminum foil on a coater and then dried. The positive electrode sheets are obtained by cold pressing, cutting, sheet making, powder sweeping, and sheet selection.
[0033] Preparation of negative electrode sheets for lithium titanate batteries: Nano lithium titanate is used as the negative electrode active material, and is mixed with polyvinylidene fluoride and conductive agent Super-P in a mass ratio of 94:4:2 in N-methylpyrrolidone. A slurry is obtained by stirring, which is coated on the current collector aluminum foil on a coater and then dried. The negative electrode sheets are obtained by cold pressing, cutting, sheet making, powder sweeping and sheet selection.
[0034] The positive electrode is coated with the negative electrode, and the positive electrode and the negative electrode are stacked into a single cell by a Z-type stacking process, and then packaged with an aluminum-plastic film, injected with the electrolyte of this embodiment, and formed to prepare a soft-pack lithium battery.
[0035] Example 2
[0036] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 35wt% of fluoroacetonitrile, 35wt% of 4,4,4-trifluorobutyronitrile, 20wt% of 18-crown ether-6, and 10wt% of a mixed additive, wherein the mixed additive is composed of 3-methoxypropionitrile, acetic anhydride, amyl acetate, isobutyl acetate, and isopropanol in a mass ratio of 1:1:1:1:1. The lithium salt is a mixture of LITFSI:LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0037] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0038] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this example as the injection object.
[0039] Example 3
[0040] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 35wt% of fluoroacetonitrile, 35wt% of 4,4,4-trifluorobutyronitrile, 20wt% of [2,2,2]-cryptand, and 10wt% of a mixed additive, wherein the mixed additive is composed of acetic anhydride, isobutyl acetate, and isopropanol in a mass ratio of 1:1:1. The lithium salt is a mixture of LITFSI:LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0041] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0042] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this example as the injection object.
[0043] Example 4
[0044] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 80wt% of fluoroacetonitrile and 20wt% of 18-crown ether-6. The lithium salt is a mixture of LITFSI and LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0045] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0046] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this example as the injection object.
[0047] Example 5
[0048] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 40wt% of fluoroacetonitrile, 40wt% of 4,4,4-trifluorobutyronitrile, 10wt% of 18-crown-6, and 10wt% of [2,2,2]-cryptand. The lithium salt is a mixture of LITFSI and LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0049] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0050] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this example as the injection object.
[0051] Example 6
[0052] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of the following raw materials uniformly mixed: 90wt% fluoroacetonitrile and 10wt% mixed additives. The mixed additives are 3-methoxypropionitrile, acetic anhydride, amyl acetate, isobutyl acetate, and isopropanol in a mass ratio of 1:1:1:1:1. The lithium salt is a mixture of LITFSI and LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0053] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0054] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this example as the injection object.
[0055] Example 7
[0056] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 45wt% of fluoroacetonitrile, 45wt% of 4,4,4-trifluorobutyronitrile, and 10wt% of a mixed additive. The mixed additive is composed of 3-methoxypropionitrile and acetic anhydride in a mass ratio of 1:1. The lithium salt is a mixture of LITFSI and LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0057] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0058] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this example as the injection object.
[0059] Example 8
[0060] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 45wt% of fluoroacetonitrile, 45wt% of 4,4,4-trifluorobutyronitrile, and 10wt% of a mixed additive. The mixed additive is composed of 3-methoxypropionitrile, acetic anhydride, and isopropanol in a mass ratio of 2:1:1. The lithium salt is a mixture of LITFSI:LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0061] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0062] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this example as the injection object.
[0063] Example 9
[0064] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 50wt% of fluoroacetonitrile and 50wt% of 4,4,4-trifluorobutyronitrile. The lithium salt is a mixture of LITFSI and LiDFOB in a molar ratio of 1:1, and the concentration of the lithium salt in the electrolyte is 2M.
[0065] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0066] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this example as the injection object.
[0067] Comparative Example 1
[0068] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of the following raw materials mixed evenly: 50wt% ethylene carbonate and 50% dimethyl carbonate. The lithium salt is LiPF6, and the concentration of the lithium salt in the electrolyte is 1M.
[0069] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0070] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this comparative example as the injection object.
[0071] Comparative Example 2
[0072] An electrolyte for a lithium titanate battery, whose composition and preparation method are the same as those of Comparative Example 1.
[0073] A soft-pack lithium battery was prepared in the same manner as in Example 1, using the electrolyte of this comparative example as the injection object, except that the negative electrode active material was graphite.
[0074] Comparative Example 3
[0075] An electrolyte for a lithium titanate battery, the electrolyte is composed of a lithium salt and an organic solvent, wherein the organic solvent is composed of a uniform mixture of the following raw materials: 70wt% of fluoroacetonitrile, 20wt% of 18-crown ether-6, and 10wt% of a mixed additive, wherein the mixed additive is composed of 3-methoxypropionitrile, acetic anhydride, and amyl acetate in a mass ratio of 4:3:2. The lithium salt is LiPF6, and the concentration of the lithium salt in the electrolyte is 1M.
[0076] The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2 less than 0.1ppm). During the preparation, the components of the organic solvent constituted above are first mixed uniformly according to the mass ratio, and then the lithium salt is slowly added and fully stirred to form a mixed solution, thereby obtaining the electrolyte of the lithium titanate battery.
[0077] In the same manner as in Example 1, a soft-pack lithium battery was prepared using the electrolyte of this comparative example as the injection object.
[0078] -20℃ rate discharge capacity test: The test objects are the soft-pack lithium batteries prepared in Examples 1-9 and Comparative Examples 1-3. Each time the soft-pack lithium batteries are charged at room temperature at a 1C rate current, and then discharged from 1C to 10C rates in an environment of -20℃. The test results are shown in Table 1. The electrochemical performance tests were all completed using a Titan 5V60A battery test cabinet.
[0079] Table 1 -20℃ rate discharge capacity test results
[0080]
[0081] -40℃ rate discharge capacity test: The test objects are the soft-pack lithium batteries prepared in Examples 1-9 and Comparative Examples 1-3. Each time the soft-pack lithium batteries are charged at room temperature at a 1C rate current, and then discharged from 1C to 10C rates in an environment of -40℃. The test results are shown in Table 2. The electrochemical performance tests were all completed using a Titan 5V60A battery test cabinet.
[0082] Table 2 -40℃ rate discharge capacity test
[0083]
[0084] Cycle life test: The test objects are the soft-pack lithium batteries prepared in Examples 1-9 and Comparative Examples 1-3. The soft-pack lithium batteries are charged and discharged at 1C current at room temperature to measure the initial capacity. After being fully charged at room temperature with 1C current, the soft-pack lithium batteries are placed in an environment of -20°C and charged and discharged at 1C current to test the battery cycle life. The test results are shown in Table 3. The electrochemical performance tests were all completed using a Titan 5V60A battery test cabinet.
[0085] Table 3 Cycle life test results
[0086]
[0087] It can be seen from Table 1 that the 10C rate discharge capacity retention rate of comparative example 1 is 41.27%, and the battery of comparative example 2 cannot complete discharge normally at a rate current of more than 3C, while the discharge capacity retention rates of the embodiments of the present invention at a 2C rate are all above 78%, and the discharge capacity retention rates at a 10C rate are all above 44%.
[0088] As shown in Table 2, the 3C rate discharge capacity retention rate of Comparative Example 1 is 45.97%, and the charge and discharge cannot be completed normally at a rate current above 3C. The battery of Comparative Example 2 cannot be discharged normally at -40°C, while the discharge capacity retention rates of the embodiments of the present invention at 2C rate are all above 58%, and the discharge capacity retention rates at 5C rate are all above 38%.
[0089] As shown in Table 3, Comparative Example 1 completed the charge-discharge cycle at 1C charge-discharge current at -20°C, and the capacity retention rate after 1000 cycles was 45.86%, while Comparative Example 2 could only perform more than 100 cycles under the same conditions, and the capacity retention rate after 100 cycles was 37.84%. The capacity retention rate of each embodiment after 1000 cycles was more than 56%.
[0090] The electrolyte of the lithium titanate battery of Example 9 of the present invention only introduces fluorinated nitrile compounds as solvents. Fluorinated nitrile compounds are beneficial to weaken the interaction between solvent molecules and Li + interaction, thereby achieving Li +Faster desolvation can improve the ionic conductivity of the electrolyte at low temperatures, so that the capacity retention rate and cycle life test at low temperatures of Example 9 are significantly better than those of the comparative example.
[0091] In Examples 1-5, crown ether or cryptand solvents with lower freezing point and viscosity are introduced, and the capacity retention rate and cycle life test at low temperature are significantly better than those in Example 9. This is because although the fluorinated nitrile compounds realize Li + Faster desolvation improves the ionic conductivity of the electrolyte at low temperatures, but the fluorinated nitrile compounds have insufficient dissociation ability for lithium salts, which will improve their performance as electrolytes. The crown ether or cryptand compound of Example 1-5 can be reacted with Li + The formation of a coated integration to enhance the solubility of lithium salts, crown ethers or cryptands and fluorinated nitrile compounds synergistically cooperate to achieve Li + Faster desolvation improves the ionic conductivity of the electrolyte at low temperatures while enhancing the solubility of lithium salts.
[0092] In Examples 1-3 and 6-8, a mixed additive composed of multiple substances is introduced to increase the mixing entropy of the electrolyte, reduce the Gibbs free energy of the electrolyte system, reduce the freezing point of the electrolyte system, enrich the solvation structure, and broaden the electrolyte working temperature, further improving the rate performance and cycle life of lithium titanate batteries at low temperatures.
[0093] Some embodiments in this specification are described in a progressive manner. Each embodiment focuses on the differences from other embodiments, and the same or similar parts between the embodiments can be referenced to each other.
[0094] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. An electrolyte for a lithium titanate battery, characterized in that: The invention comprises a lithium salt and an organic solvent, wherein the organic solvent comprises a fluorinated nitrile compound.
2. The electrolyte of the lithium titanate battery according to claim 1, characterized in that: The fluorinated nitrile compound is at least one of fluoroacetonitrile, 4,4,4-trifluorobutyronitrile, 3-amino-4,4,4-trifluorobutyronitrile and 3,3,3-trifluoropropionitrile.
3. The electrolyte of the lithium titanate battery according to claim 1, characterized in that: The organic solvent further comprises an ether compound, and the ether compound is a crown ether compound and / or a cryptand compound.
4. The electrolyte of the lithium titanate battery according to claim 3, characterized in that: The ether compound is at least one of 18-crown-6, benzo-18-crown-6, benzo-15-crown-5, dicyclohexane-18-crown-6, and [2,2,2]-cryptand.
5. The electrolyte of the lithium titanate battery according to any one of claims 1 to 4, characterized in that: The organic solvent further comprises a mixed additive, and the mixed additive is at least two of 3-methoxypropionitrile, acetic anhydride, amyl acetate, isobutyl acetate and isopropanol.
6. The electrolyte of the lithium titanate battery according to claim 1, characterized in that: The lithium salt is at least one of LITFSI, LIFSI, LiDFOB, and LiBF4.
7. The electrolyte of the lithium titanate battery according to claim 6, characterized in that: The lithium salts are LITFSI and LiDFOB in a molar ratio of 1:
1.
8. The electrolyte of the lithium titanate battery according to claim 6, characterized in that: The concentration of lithium salt is 1M-10M.
9. The electrolyte of the lithium titanate battery according to claim 5, characterized in that: The organic solvent comprises 70-100 wt % of fluorinated nitrile compounds, 0-30 wt % of ether compounds and 0-10 wt % of mixed additives.
10. A lithium titanate battery, characterized in that: Comprising the electrolyte as described in any one of claims 1-8.