Flexible Ag2Se / fabric thermoelectric composite material and preparation method thereof
Flexible Ag2Se/fabric thermoelectric composite materials were prepared by depositing Ag2Se layers on fabrics using a wet chemical method. This method solves the problem of insufficient performance of existing fabric-based thermoelectric materials and improves both flexibility and thermoelectric properties, making it suitable for wearable electronic products.
Patent Information
- Application Number
- CN202410929004.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
Existing flexible fabric-based thermoelectric materials have low performance and are difficult to meet the practical application requirements of wearable electronic devices.
Flexible Ag2Se/fabric thermoelectric composites were prepared using a wet chemical method, including fabric pretreatment, silver plating, and the preparation of the flexible Ag2Se/fabric thermoelectric composites. This was achieved by depositing an Ag2Se layer on the fabric, combined with a reduction reaction involving glucose, sodium potassium tartrate, and Tollens' reagent.
The prepared flexible Ag2Se/fabric composite material has good flexibility and thermoelectric properties, making it suitable for wearable electronic products. Moreover, the preparation process is simple and low-cost, making it suitable for large-scale production.
Smart Images

Figure CN118900612A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of flexible thermoelectric materials, and in particular to a flexible Ag 2 Se / textile thermoelectric composite material and preparation method thereof. Background Art
[0002] Flexible fabrics have the advantages of good flexibility, high air permeability, certain elastic stretchability and recovery, etc. They are suitable for skin contact and have good wearing comfort. Flexible thermoelectric materials based on fabrics can combine the comfort of fabrics and the functionality of thermoelectric conversion, and have important application prospects and needs in wearable electronic products. However, at present, the performance of flexible fabric-based thermoelectric materials is low and it is difficult to meet the needs of practical applications of wearable electronic devices. Therefore, it is urgent to develop flexible fabric-based thermoelectric functional materials with good thermoelectric properties. Summary of the invention
[0003] The purpose of the present invention is to provide a new flexible Ag 2 Se / fabric thermoelectric composite material and preparation method thereof, prepared Ag 2 Se / fabric composite thermoelectric material has good flexibility and thermoelectric properties, and the preparation process of the invention is universal.
[0004] The purpose of the present invention is achieved through the following technical solutions:
[0005] The purpose of the present invention is to provide a flexible Ag 2 Se / textile thermoelectric composite material and preparation method thereof, comprising the following steps:
[0006] (1) Fabric pretreatment: The fabric was ultrasonically treated in acetone and then washed with deionized water; sodium hydroxide was weighed and dissolved in deionized water to obtain a sodium hydroxide (NaOH) solution, the fabric was placed in the NaOH solution and allowed to stand, then taken out and washed twice with deionized water; stannous chloride dihydrate was weighed and dissolved in deionized water, and an appropriate amount of concentrated hydrochloric acid solution was added dropwise until the solution was clear to obtain Sn 2+ Solution, place the fabric in Sn 2+ The solution was allowed to stand for 2 h, and then washed with deionized water and dried naturally to obtain a dry fabric;
[0007] (2) Silver plating of fabric: firstly, glucose monohydrate, potassium sodium tartrate tetrahydrate and polyethylene glycol 1000 are dissolved in a mixed solution of ethanol and deionized water to prepare a reducing agent; then, silver nitrate and sodium hydroxide are dissolved in ammonia water to prepare a Tollens reagent; the reducing agent and the Tollens reagent are mixed evenly to obtain a mixed solution of the reducing agent and the Tollens reagent, the fabric dried in step (1) is placed in the mixed solution of the reducing agent and the Tollens reagent, left to stand, then taken out, washed with deionized water, and then vacuum dried to obtain a silver-plated fabric;
[0008] (3) Flexible Ag 2 Preparation of Se / textile thermoelectric composite material: weigh sodium sulfide nonahydrate and selenium powder and dissolve them in deionized water to obtain a selenium solution, then put the silver-plated fabric obtained in step (2) into the selenium solution, let it stand, then take it out, wash it with deionized water and vacuum dry it to obtain the flexible Ag 2 Se / textile thermoelectric composites.
[0009] Furthermore, the preparation method comprises the following steps:
[0010] (1) Fabric pretreatment: A 5 cm*5 cm fabric was ultrasonically treated in an acetone solution for 30 minutes and then washed with deionized water; 8 g of sodium hydroxide (NaOH) was weighed and dissolved in 100 mL of deionized water, the fabric was placed in the sodium hydroxide solution and allowed to stand for 30 minutes, then taken out and washed twice with deionized water; a certain amount of stannous chloride dihydrate (SnCl 2 ·2H 2 O) was dissolved in 100 mL of deionized water, and an appropriate amount of concentrated hydrochloric acid solution was added dropwise until the solution was clear to obtain Sn 2+ Place the fabric in Sn 2+ The solution was allowed to stand for 2 h, then taken out, washed with deionized water and dried naturally;
[0011] (2) Fabric silver plating: First, 4 g of glucose monohydrate (C 6 H 12 O 6 ·H 2 O), 1.4 g potassium sodium tartrate tetrahydrate (C 4 H 4 O 6 KNa·4H 2 O) and 10 μL polyethylene glycol 1000 (PEG 1000) were dissolved in a mixed solution of 100 mL ethanol and deionized water to prepare a reducing agent; then 5 g silver nitrate (AgNO 3) and 2.5g NaOH are dissolved in 100mL ammonia water to prepare Tollens reagent. The reducing agent and Tollens reagent are mixed evenly, and the fabric dried in step (1) is placed in the mixed solution of the reducing agent and Tollens reagent and allowed to stand for a certain period of time, then taken out, washed with deionized water, placed in a vacuum drying oven, and vacuum dried at 60°C for 12h;
[0012] (3) Flexible Ag 2 Preparation of Se / textile thermoelectric composite materials: Weigh 6 g of sodium sulfide nonahydrate (Na 2 S·9H 2 O) and 2g of selenium powder (Se) are dissolved in 100mL of deionized water, and then the silver-plated fabric obtained in step (2) is placed in the selenium solution and allowed to stand, then taken out, washed with deionized water, and placed in a vacuum drying oven for drying. The drying conditions are the same as those in step (2), to obtain the flexible Ag 2 Se / textile thermoelectric composites.
[0013] Preferably, the fabric used in step (1) is nylon.
[0014] Preferably, in step (1), Sn 2+ The concentration of the solution is 0.18~0.22mol / L.
[0015] Preferably, in step (2), the concentration of the mixed solution of ethanol and deionized water is 2.5 to 5 mol / L.
[0016] Preferably, in step (2), the concentration of the ammonia water is 9 to 13 mol / L.
[0017] Preferably, in step (2), the volume ratio of the reducing agent to the Tollens reagent is 1:1.
[0018] Preferably, in step (2), the fabric is allowed to stand in the mixed solution of the reducing agent and Tollens reagent for 4 to 6 hours.
[0019] Preferably, in step (3), the silver-plated fabric is allowed to stand in the selenium solution for 8 to 12 hours.
[0020] Compared with the prior art, the beneficial effects of the present invention are embodied in the following aspects:
[0021] 1) The present invention adopts a simple and economical wet chemical method to synthesize flexible Ag 2 Se / textile thermoelectric composites, unlike the preparation process of traditional thermoelectric materials or devices, the manufacturing technology hardly relies on complex equipment, which makes Ag 2Se / fabric can be produced at low cost and on a large scale and processed into special shapes to match different applicable surfaces. The preparation process of the invention is universal.
[0022] 2) Ag of the present invention 2 Se / textile composite thermoelectric materials have good flexibility and have broad application prospects in wearable electronic products. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The flexible Ag of Example 1 2 Digital photo showing the flexibility of Se / nylon thermoelectric composites;
[0024] Figure 2 The flexible Ag of Example 1 2 Scanning electron microscope image of Se / nylon thermoelectric composite material. DETAILED DESCRIPTION
[0025] The present invention is described in detail below in conjunction with specific embodiments, but is by no means intended to limit the present invention. Features such as preparation methods, materials, structures or composition ratios not explicitly described in this technical solution are considered to be common technical features disclosed in the prior art.
[0026] The present invention provides a flexible Ag 2 Se / textile thermoelectric composite material and preparation method thereof, comprising the following steps:
[0027] (1) Fabric pretreatment: The fabric was treated in acetone and sodium hydroxide solution respectively, then placed in dihydrate stannous chloride solution and left to stand, then washed with deionized water and dried naturally; (2) Fabric silver plating: The pretreated fabric was placed in a mixed solution of reducing agent and Tollens reagent to be silver plated, then washed and dried; (3) Flexible Ag 2 Preparation of Se / textile thermoelectric composite materials: Sodium sulfide nonahydrate and selenium powder are dissolved in deionized water to obtain a selenium solution, and the silver-plated fabric in step (2) is placed in the selenium solution to prepare a flexible Ag 2 Se / textile thermoelectric composite material. The preparation process of the present invention has universal applicability, and the prepared flexible Ag 2 Se / textile thermoelectric composites have good flexibility and thermoelectric properties and have broad application prospects in the field of wearable electronics.
[0028] The conception of this technical solution is as follows:
[0029] Thermoelectric materials are functional materials that can convert heat energy and electrical energy into each other. They are green and environmentally friendly energy conversion materials. Thermoelectric devices assembled from thermoelectric materials also have the advantages of small size, light weight, no noise during operation, and long life. 2Se, as an N-type thermoelectric material with important application potential, has high electrical conductivity and low thermal conductivity near room temperature. In addition, Ag and Se elements are abundant in the earth's crust and have become one of the research hotspots in the field of thermoelectrics. Although traditional inorganic thermoelectric materials have good electrical properties, they have poor mechanical processing and deformation capabilities. They usually show intrinsic brittleness and are easy to break under tensile, compressive or bending loads. They are not easy to make into flexible thermoelectric devices. Fabrics have the advantages of good flexibility, high air permeability, certain elastic stretchability and recovery. In daily life, fabrics can provide a comfortable touch, fit the skin, have good wearing comfort, and have important application prospects in wearable electronic products. Therefore, Ag is used in 2 By combining Se with fabrics, it is possible to obtain composite thermoelectric materials with good thermoelectric properties and flexibility, which will accelerate the application of flexible thermoelectric materials in wearable electronic products.
[0030] The following examples will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several modifications and improvements may be made without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.
[0031] The practice of the present invention may employ conventional techniques of chemistry within the skill of the art. In the following examples, efforts have been made to ensure accuracy with respect to numbers used (including amounts, temperatures, reaction times, etc.), but some experimental errors and deviations should be accounted for.
[0032] In the following examples, unless otherwise specified, each reagent may be a commercially available product that can be routinely obtained by a person skilled in the art.
[0033] In the following examples, acetone (C 3 H 6 O), NaOH, SnCl 2 ·2H 2 O, concentrated hydrochloric acid (HCl, 36-38%), C 6 H 12 O 6 ·H 2 O.C 4 H 4 O 6 KNa·4H 2 O, PEG 1000, anhydrous ethanol (C 2 H 5 OH), ammonia (NH 4 OH, 25-28%) and Na 2 S·9H 2 O was purchased from Shanghai Titan Technology Co., Ltd., selenium powder was purchased from Alfa Aesar (China) Chemical Co., Ltd., AgNO 3Purchased from Sinopharm Chemical Reagent Co., Ltd.
[0034] Example 1
[0035] This embodiment provides a flexible Ag 2 Se / textile thermoelectric composite material and preparation method thereof, comprising the following steps:
[0036] (1) Nylon pretreatment: 5 cm*5 cm nylon was ultrasonically washed in acetone solution for 30 min, then taken out and washed twice with deionized water. 8 g NaOH was weighed and dissolved in 100 mL deionized water, and the nylon was placed in the solution and allowed to stand for 30 min. After that, it was taken out and washed twice with deionized water. 4 g SnCl 2 ·2H 2 O was dissolved in 100 mL of deionized water, and an appropriate amount of concentrated hydrochloric acid solution was added dropwise until the solution was clear to obtain Sn 2+ Solution. Put nylon into Sn 2+ After the solution was left to stand for 2 hours, it was taken out and washed twice with deionized water. Finally, the cleaned nylon sample was taken out and dried naturally.
[0037] (2) Nylon silver-plated: 4g C 6 H 12 O 6 ·H 2 O, 1.4 g C 4 H 4 O 6 KNa·4H 2 O and 10 μL PEG 1000 were dissolved in 100 mL ethanol (2.5 mol / L) to prepare the reducing agent; 5 g AgNO 3 and 2.5 g NaOH dissolved in 100 mL ammonia (13 mol / L) solution to prepare Tollens reagent; then the reducing agent and Tollens reagent were mixed evenly (V / V = 1:1), the nylon dried in (1) was placed in the mixed solution of the reducing agent and Tollens reagent and allowed to stand for 6 h, taken out and washed twice with deionized water, and then vacuum dried at 60 ° C for 12 h;
[0038] (3) Flexible Ag 2 Preparation of Se / nylon thermoelectric composite materials: weigh 6 g Na 2 S·9H 2 O and 2g of selenium powder were dissolved in 100mL of deionized water, and then the silver-plated nylon obtained in step (2) was placed in the selenium solution and allowed to stand for 10 hours. After washing with deionized water, it was placed in a vacuum drying oven and dried under the same conditions as step (2) to prepare a flexible Ag 2 Se / nylon thermoelectric composites.
[0039] like Figure 1As shown, the flexible Ag of Example 1 2 Digital photo showing the flexibility of Se / nylon thermoelectric composites. The composite can be bent well, indicating good flexibility.
[0040] like Figure 2 As shown, the flexible Ag of Example 1 2 Scanning electron microscope image of Se / nylon thermoelectric composite material, showing that Ag 2 Se can grow on the surface of nylon and has a good bonding effect with the fabric.
[0041] Example 2
[0042] This embodiment provides a flexible Ag 2 Se / textile thermoelectric composite material and preparation method thereof, comprising the following steps:
[0043] (1) The pretreatment steps of the nylon fabric are the same as those in Example 1, specifically see step (1) in Example 1;
[0044] (2) Nylon silver plating: weigh 4g C 6 H 12 O 6 ·H 2 O, 1.4 g C 4 H 4 O 6 KNa·4H 2 O and 10 μL PEG 1000 were dissolved in 100 mL ethanol (5 mol / L) to prepare the reducing agent; 8 g AgNO 3 and 4g NaOH dissolved in 100mL ammonia (13mol / L) solution to prepare Tollens reagent; then the reducing agent and Tollens reagent were mixed evenly (V / V=1:1), the nylon dried in step (1) was placed in the mixed solution of the reducing agent and Tollens reagent and allowed to stand for 6h, taken out and washed twice with deionized water, and then vacuum dried at 60°C for 12h;
[0045] (3) Flexible Ag 2 Preparation of Se / nylon thermoelectric composite materials: 9g Na 2 S·9H 2 O and 3g of selenium powder were dissolved in 100mL of deionized water, and then the silver-plated nylon obtained in step (2) was placed in the selenium solution and allowed to stand for 10h, washed with deionized water and placed in a vacuum drying oven, and dried under the same conditions as step (2) to obtain a flexible Ag 2 Se / nylon thermoelectric composites.
[0046] Example 3
[0047] This embodiment provides a flexible Ag 2 Se / textile thermoelectric composite material and preparation method thereof, comprising the following steps:
[0048] (1) The pretreatment steps of the nylon fabric are the same as those in Example 1, specifically see step (1) in Example 1;
[0049] (2) Nylon silver plating: weigh 4g C 6 H 12 O 6 ·H 2 O, 1.4 g C 4 H 4 O 6 KNa·4H 2 O and 10 μL PEG 1000 were dissolved in 100 mL ethanol (2.5 mol / L) to prepare the reducing agent; 5 g AgNO 3 and 2.5 g NaOH dissolved in 100 mL ammonia (9 mol / L) solution to prepare Tollens reagent; then the reducing agent and Tollens reagent were mixed evenly (V / V = 1:1), the nylon dried in step (1) was placed in the mixed solution of the reducing agent and Tollens reagent and allowed to stand for 6 h, taken out and washed twice with deionized water, and then vacuum dried at 60 ° C for 12 h;
[0050] (3) Flexible Ag 2 Preparation of Se / nylon thermoelectric composite materials: weigh 6 g Na 2 S·9H 2 O and 2g of selenium powder were dissolved in 100mL of deionized water, and then the silver-plated nylon obtained in step (2) was placed in the selenium solution and allowed to stand for 10h, washed with deionized water and placed in a vacuum drying oven, and dried under the same conditions as step (2) to prepare a flexible Ag 2 Se / nylon thermoelectric composites.
[0051] Example 4
[0052] This embodiment provides a flexible Ag 2 Se / textile thermoelectric composite material and preparation method thereof, comprising the following steps:
[0053] (1) Nylon pretreatment: 10 cm*10 cm nylon was ultrasonically washed in acetone solution for 30 min, then taken out and washed twice with deionized water. 32 g NaOH was weighed and dissolved in 400 mL deionized water, the nylon was placed in the solution and allowed to stand for 1 h, then taken out and washed twice with deionized water. 16 g SnCl 2 ·2H 2 O was dissolved in 400 mL of deionized water, and an appropriate amount of concentrated hydrochloric acid solution was added dropwise until the solution was clear to obtain Sn 2+Solution. Put nylon into Sn 2+ After the solution was left to stand for 2 hours, it was taken out and washed twice with deionized water. Finally, the cleaned nylon sample was taken out and dried naturally.
[0054] (2) Nylon silver plating: weigh 16g C 6 H 12 O 6 ·H 2 O, 5.6 g C 4 H 4 O 6 KNa·4H 2 O and 40 μL PEG 1000 were dissolved in 400 mL ethanol (2.5 mol / L) to prepare the reducing agent; 32 g AgNO 3 and 16 g NaOH dissolved in 400 mL ammonia (9 mol / L) solution to prepare Tollens reagent; then the reducing agent and Tollens reagent were mixed evenly (V / V = 1:1), the nylon dried in step (1) was placed in the mixed solution of the reducing agent and Tollens reagent and allowed to stand for 6 h, taken out and washed twice with deionized water, and then vacuum dried at 60 ° C for 12 h;
[0055] (3) Flexible Ag 2 Preparation of Se / nylon thermoelectric composite materials: weigh 36 g Na 2 S·9H 2 O and 12g of selenium powder were dissolved in 400mL of deionized water, and then the silver-plated nylon obtained in step (2) was placed in the selenium solution and allowed to stand for 12h, washed with deionized water and placed in a vacuum drying oven, and dried under the same conditions as step (2) to prepare a flexible Ag 2 Se / nylon thermoelectric composites.
[0056] The above is a description of the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above-mentioned description of the embodiments for the convenience of ordinary technicians in the technical field to understand and use the invention. It is obvious that those familiar with the technology in the field can easily make various modifications to these embodiments and apply the general principles described here to other embodiments without creative work. Therefore, the present invention is not limited to the above-mentioned embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A flexible Ag2Se / textile thermoelectric composite material and a preparation method thereof, characterized in that: The steps include: (1) Fabric pretreatment: The fabric was ultrasonically treated in acetone and then washed with deionized water; sodium hydroxide was weighed and dissolved in deionized water to obtain a sodium hydroxide solution, the fabric was placed in the sodium hydroxide solution and allowed to stand, then taken out and washed twice with deionized water; stannous chloride dihydrate was weighed and dissolved in deionized water, and an appropriate amount of concentrated hydrochloric acid solution was added dropwise until the solution was clear to obtain Sn 2+ Solution, place the fabric in Sn 2+ The solution was allowed to stand for 2 h, and then washed with deionized water and dried naturally to obtain a dry fabric; (2) Silver plating of fabric: firstly, glucose monohydrate, potassium sodium tartrate tetrahydrate and polyethylene glycol 1000 are dissolved in a mixed solution of ethanol and deionized water to prepare a reducing agent; then, silver nitrate and sodium hydroxide are dissolved in ammonia water to prepare a Tollens reagent; the reducing agent and the Tollens reagent are mixed evenly to obtain a mixed solution of the reducing agent and the Tollens reagent, the fabric dried in step (1) is placed in the mixed solution of the reducing agent and the Tollens reagent, left to stand, then taken out, washed with deionized water, and then vacuum dried to obtain a silver-plated fabric; (3) Preparation of flexible Ag2Se / textile thermoelectric composite material: Weigh sodium sulfide nonahydrate and selenium powder and dissolve them in deionized water to obtain a selenium solution, then put the silver-plated fabric obtained in step (2) into the selenium solution, let it stand, then take it out, wash it with deionized water and vacuum dry it to obtain the flexible Ag2Se / textile thermoelectric composite material.
2. A flexible Ag2Se / textile thermoelectric composite material and a preparation method thereof according to claim 1, characterized in that: The steps include: (1) Fabric pretreatment: A 5 cm*5 cm fabric was ultrasonically treated in an acetone solution for 30 minutes and then washed with deionized water; 8 g of sodium hydroxide was weighed and dissolved in 100 mL of deionized water, the fabric was placed in the sodium hydroxide solution and allowed to stand for 30 min, then taken out and washed twice with deionized water; a certain amount of stannous chloride dihydrate was weighed and dissolved in 100 mL of deionized water, and an appropriate amount of concentrated hydrochloric acid solution was added dropwise until the solution was clear to obtain Sn 2+ Solution; Place fabric in Sn 2+ The solution was allowed to stand for 2 h, then taken out, washed with deionized water and dried naturally; (2) Fabric silver plating treatment: First, 4 g of glucose monohydrate, 1.4 g of potassium sodium tartrate tetrahydrate and 10 μL of polyethylene glycol 1000 were dissolved in a mixed solution of 100 mL of ethanol and deionized water to prepare a reducing agent; then, 5 g of silver nitrate and 2.5 g of sodium hydroxide were dissolved in 100 mL of ammonia water to prepare a Tollens reagent; the reducing agent and the Tollens reagent were mixed evenly, and the fabric dried in step (1) was placed in the mixed solution of the reducing agent and the Tollens reagent, allowed to stand for a certain period of time, and then taken out, washed with deionized water, and placed in a vacuum drying oven for vacuum drying at 60°C; (3) Preparation of flexible Ag2Se / textile thermoelectric composite material: Weigh 6g of sodium sulfide nonahydrate and 2g of selenium powder and dissolve them in 100mL of deionized water. Then, place the silver-plated fabric obtained in step (2) into the selenium solution and let it stand for a suitable time before taking it out. After washing it with deionized water, place it in a vacuum drying oven and dry it under the same drying conditions as those in step (2) to obtain the flexible Ag2Se / textile thermoelectric composite material.
3. A flexible Ag2Se / textile thermoelectric composite material and a preparation method thereof according to claim 1, characterized in that: The fabric used in step (1) is nylon.
4. A flexible Ag2Se / textile thermoelectric composite material and a preparation method thereof according to claim 1, characterized in that: In step (1), Sn 2+ The concentration of the solution is 0.18~0.22mol / L.
5. The flexible Ag2Se / textile thermoelectric composite material and the preparation method thereof according to claim 1, characterized in that: In step (2), the concentration of the mixed solution of ethanol and deionized water is 2.5 to 5 mol / L.
6. The flexible Ag2Se / textile thermoelectric composite material and the preparation method thereof according to claim 1, characterized in that: In step (2), the concentration of the ammonia water is 9 to 13 mol / L.
7. The flexible Ag2Se / textile thermoelectric composite material and the preparation method thereof according to claim 1, characterized in that: In step (2), the volume ratio of the reducing agent to the Tollens reagent is 1:
1.
8. The flexible Ag2Se / textile thermoelectric composite material and the preparation method thereof according to claim 1, characterized in that: In step (2), the dried fabric is placed in the mixed solution of the reducing agent and the Tollens reagent for 4 to 6 hours.
9. The flexible Ag2Se / textile thermoelectric composite material and the preparation method thereof according to claim 1, characterized in that: In step (3), the silver-plated fabric is allowed to stand in the selenium solution for 8 to 12 hours.
10. A flexible Ag2Se / textile thermoelectric composite material prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Preparation method of silver selenide three-dimensional structure thermoelectric material
CN120210907A