Metal foam and method for producing same

By forming stable foams or emulsions in aqueous suspensions, the pore structure can be controlled, solving the problem of difficult control over the porosity and size of porous metal structures, and achieving the mechanical stability and wide application of multi-level pores.

CN118900734APending Publication Date: 2024-11-05ETH ZURICH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027292.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-23
Filing Date
2023-02-22
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively control the porosity and pore size of porous metal structures, limiting their performance regulation and manufacturing efficiency in various applications.

Method used

A compound containing metal atoms is used as a suspension in water to form a stable foam or emulsion through foaming or emulsification. The pore structure is controlled by surfactants and lipophilic phases, and then a multi-level porous metal structure is formed through drying and reduction processes.

Benefits of technology

It achieves multi-level pore structures spanning multiple orders of magnitude, improving mechanical stability and porosity control, and is suitable for various applications such as resistance heating, cooling, oil absorption, multiphase catalysis, and electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900734A_ABST
    Figure CN118900734A_ABST
Patent Text Reader

Abstract

An aqueous suspension for producing a porous metal structure comprises: 2-49% by volume of a mixture of at least one compound comprising metal atoms wherein the at least one compound is solid at room temperature, in powder form, and suspended in water; and the aqueous suspension comprises from 10 to 9 to 0.1 mol of a surfactant per mol of the compound comprising metal atoms. The aqueous suspension is part of a foam; and / or a portion of an oil-in-water emulsion, the oil-in-water emulsion comprising 30-90% by volume of a lipophilic phase, the lipophilic phase being free of polymerizable compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aqueous suspension for producing porous metal structures, a method for producing porous metal materials and the use of such metal materials. Background Art

[0002] Porous metals have long been used as filters in chemical processes and electrodes in functional devices. Steel- and iron-based structures with highly tunable porosity have been explored as sustainable, lightweight materials for a variety of structural, biomedical, and energy-related applications.

[0003] Porous metals have been used as jewelry, filters, and battery components [1-2], and have been considered for use in lightweight structures, catalysis, thermal management, and tissue regeneration [3-9]. This wide range of existing and future applications relies on combining the unique set of properties provided by the percolating metal network with the low weight and open channels provided by the porous phase.

[0004] Control over the porosity and pore size of metallic structures allows the properties of porous metals to be tailored to meet the needs of specific applications. Fabrication techniques directly affect the porosity and pore size of the final structure and have therefore been studied to control the properties and functionality of porous materials [10-13].

[0005] The advent of 3D printing has opened up new opportunities for the design and fabrication of novel biomimetic hierarchical porous materials with antagonistic properties that are inaccessible through conventional manufacturing methods

[14] . This has the potential to produce bone-inspired structures that combine lightweight and high mechanical efficiency, as well as sponge-inspired filters that combine high efficiency with low pressure drop

[15] .

[0006] 3D printing technologies used to fabricate porous cellular metals include powder bed fusion technology [16-18], electron beam melting [19-20], various replication technologies [3,7,21], and direct ink writing [22-24]. Among the technologies that can produce large centimeter-scale objects, direct ink writing (DIW) has attracted particular attention because it can print complex structures at room temperature using readily available and low-cost desktop printers.

[0007] For printing cellular porous iron by DIW, metal or metal oxide precursor particles are suspended in a liquid phase containing a binder to produce a viscoelastic ink that is subsequently extruded through a submillimeter nozzle [23,25]. The printed cellular structure is then dried, reduced, and sintered to densify the deposited filaments

[26] . The resulting metal structure exhibits open pores, whose size and relative fraction are a result of the tool path and printing nozzle. Despite the demonstrated biocompatibility, mechanical properties, and electrochemical response to date [23,25], the potential of direct ink writing as a tool for fabricating metals with tunable multi-level porous structures has not yet been fully explored.

[0008] A strategy to control the porosity of materials at multiple length scales is to print inks or resins containing building blocks that generate pores through a predetermined self-assembly process [27-29]. In this approach, macropores generated by the tool path are combined with small pores generated by the self-assembling ink to generate structural features below the resolution of the printer. Bubbles, droplets, or organic particles have been used as self-assembling building blocks to print ceramics or polymers with programmable multi-level porosity [27,30-31]. Porous silica-like glasses with tunable multiscale pores have also been produced by digital light processing (DLP) of phase-separated resins containing self-assembling monomers and metal alkoxide precursors

[29] .

[0009] GB 339645 discloses the following process: suspending metal oxide powder in water, adding more than 1 wt% of a foaming agent, casting the resulting foam, drying the cast foam, and reducing the dried foam to a porous metal. The maximum porosity reaches 80%.

[0010] US 2009 / 0325780 A1 discloses the preparation of wet foams showing long-term stability, wherein colloidal particles, initially inherently partially lyophobic particles or partially lyophobicized particles having an average particle size of 1 nm to 20 μm, are used to stabilize the gas-liquid interface.

[0011] US 2021 / 0130244 A1 discloses another method for producing particle-stabilized foam.

[0012] WO 2016 / 187097 A1 discloses a particle-stabilized foam ink composition that can be used for 3D printing of multi-layered porous structures by continuous filament deposition of the particle-stabilized ink. In order to achieve partially open pores, fugitive particles comprising polymers or carbon must be added to the foam ink composition. If a metal foam is required, the foam ink composition may contain metal oxide or metal hydride particles, and a reduction or oxidation step is performed after the deposition and drying of the continuous filament.

[0013] C. Kenel et al., Addit. Manuf. 2021, 37, 101637 discloses the production of multi-level porous metal skeletons by 3D extrusion of oxide particle inks and reduction with salt templates. Metal structures with three-level multi-level pores can be printed using inks containing iron oxide particles as metal precursors and soluble salt templates as sacrificial templates

[32] . This process produces relatively low porosity (<38% for iron).

[0014] A. Verdooren et al., J. Mat. Sc. 2005, 40, 4333 discloses a method for producing ceramic foam using a precursor containing iron (III) oxide, calcium oxide, aluminum and carbon black in an acidic solution containing 50% by weight of aluminum orthophosphate. Foaming is caused by the generation of hydrogen. A similar method using a precursor containing iron (III) oxide, magnesium oxide, aluminum and carbon black is disclosed in A. Verdooren et al., J. Am. Ceram. Soc. 2006, 89, 3101.

[0015] C. Minas et al., Adv. Mat. 2016, 28, 9993 (reference 27) discloses a method for producing particle-stabilized foams and emulsions of metal oxide particles having closed or open pores.

[0016] US2015 / 0035209 A1 discloses a method of forming a metal, wherein a paste comprising metal oxide particles, a polymer binder and an organic solvent is extruded through a nozzle, thereby depositing layers of the metal oxide paste sequentially on a substrate to form a three-dimensional object. The object is exposed to a reducing gas at a temperature and for a time sufficient to reduce and sinter the metal oxide particles to form a three-dimensional metal object.

[0017] WO 2015 / 175880 A1 discloses a 3D printable ink composition comprising metal oxide particles and an elastic polymer binder.

[0018] WO 2020 / 243428 A1 discloses a wet foam composition for producing sintered open-cell ceramic foam.

[0019] US2006 / 0211802 A1 discloses a process for manufacturing a porous metal-containing material. Particles are dispersed in at least one solvent, the particles comprising at least one polymer material and at least one metal compound. The solvent is removed from the composition and the polymer material is decomposed, thereby converting the solvent-free particles into a porous metal-containing material.

[0020] There is a general need for improvement in this area. Summary of the invention

[0021] A general object of the present invention is to provide improvements in the manufacture of metal foams and porous metal structures.

[0022] In the context of the present description, the terms metal foam and porous metal structure are used synonymously.

[0023] It is an object of the present invention to provide advantageous aqueous suspensions for producing porous metal structures which enable the additive manufacturing of three-dimensional objects which can be transformed into the porous metal structure in a subsequent step.

[0024] Another object of the present invention is to provide a method for producing a porous metal material.

[0025] Yet another object of the present invention is to provide advantageous uses and applications of these porous metal materials.

[0026] These and other objects are substantially achieved by the features of the independent claims. Advantageous embodiments and variants are set forth in the dependent claims.

[0027] Other aspects of the invention will become apparent as the description proceeds.

[0028] The present invention may comprise one or more of the features recited in the accompanying claims and / or one or more of the following features and combinations thereof.

[0029] A first aspect of the invention relates to an aqueous suspension for producing a porous metal structure, which is in the form of a foam or an emulsion.

[0030] The aqueous suspension of the present invention comprises a mixture of 2-49% by volume of at least one compound containing metal atoms, wherein the at least one compound is solid at room temperature, is in powder form, and is suspended in water, and for each mol of the compound containing metal atoms, the aqueous suspension comprises 10 -9 The aqueous suspension is part of a foam and / or part of an oil-in-water emulsion comprising 30-90% by volume of a lipophilic phase which is free of polymerizable compounds.

[0031] Such polymerizable compounds may be, for example, monomeric compounds or oligomeric compounds that readily polymerize under the conditions of subsequent processing steps.

[0032] The relationship between the amount of surfactant required to obtain stable foam and the amount of powdered suspension compound containing metal atoms depends on factors such as the chain length of the surfactant. Using very low concentrations of long-chain surfactants can produce particle-stabilized foam. As described in AR Studart et al., "Unifying Model for the Electrokinetic and Phase Behavior of Aqueous Suspensions Containing Short and Long Amphiphiles", Langmuir 2011, 27, 11835-11844, the concentration of amphiphilic substances required to halve the Zeta potential is a good indicator of the minimum concentration required for foaming.

[0033] Such an aqueous suspension of the invention can be used as a stable wet foam or a stable emulsion, which is used as an ink for additive manufacturing, in particular for direct ink writing. This wet body can then be dried to a green body with a pore structure, which can subsequently be further processed.

[0034] The foamed aqueous suspension of the invention can be produced by foaming an aqueous suspension with a gas, for example air or, advantageously, an inert gas such as nitrogen.

[0035] The foamed aqueous suspension of the invention enables the production of mechanically stable metal structures with multiple levels of porosity spanning multiple orders of magnitude. On a first level, macroscopic, the porosity is controllably created during the additive manufacturing process. On a smaller second level, the porosity is created by the pores of the foamed aqueous suspension. In the micrometer range, tertiary porosity can be found on the walls of the pores of the second level, with holes in the pore walls connecting the pores. The result is an open-cell structure.

[0036] Without wishing to be bound by any particular theory, it is believed that this tertiary porosity is the result of a rearrangement process of metal atoms at high temperatures, such as during the sintering step.

[0037] The emulsified aqueous suspension of the present invention can be produced by emulsifying an aqueous suspension with a lipophilic phase.

[0038] Advantageously, the lipophilic phase of the oil-in-water emulsion is a lipophilic organic solvent, such as n-octane.

[0039] Similar to foam bubbles, the droplets of this oil-in-water emulsion provide a framework for the formation of macropores. The lipophilic organic solvent is advantageously selected so that the boiling point (n-octane: 125-127°C at normal pressure) is higher than the boiling point of water, but in a similar range. When the printed object is dried, the printed emulsion ink will remain mechanically stable, and the organic solvent can be removed in the same step as the water removal.

[0040] Since the droplets of such an oil-in-water emulsion do not affect the mechanical stability of the dried body, it is not necessary to stabilize them mechanically, for example by polymerizing the droplets. Such a polymerization would in fact be disadvantageous, since the polymer cannot be completely removed afterwards in the drying step. It is therefore advantageous if the lipophilic phase of the emulsion does not contain polymerizable compounds, for example monomeric or oligomeric compounds, which are easily polymerized in the drying step.

[0041] The particle size of the powdery compound containing metal atoms is advantageously 0.03 to 5 μm.

[0042] Advantageously, the aqueous composition of the invention is a foam or an emulsion.

[0043] More advantageously, the aqueous composition of the invention is a foam or an oil-in-water emulsion having a solids loading of 2-49% by volume.

[0044] Alternatively or additionally, the gas bubble size of the advantageous foamed aqueous composition of the invention is from 20 μm to 2 mm. Correspondingly, in the emulsion based on the aqueous suspension of the invention, the diameter of the emulsion droplets is from 5 μm to 2 mm.

[0045] Advantageously, in the aqueous suspension of the invention, one or more of said compounds comprising a metal atom is a compound reducible to a metal in a gaseous atmosphere.

[0046] Alternatively or additionally, in the aqueous suspension of the present invention, one or more of the compounds comprising a metal atom may be a metal oxide, a metal hydroxide, a metal chloride or a metal fluoride.

[0047] For example, oxides or hydroxides of Fe, Cr, Zn, Al, Mn, Sn, Pb, Co, Ni, Cu, Mo, Ta, W can be used as compounds containing metal atoms. Such compounds can be reduced at a temperature of 200 to 800° C. in a hydrogen atmosphere.

[0048] Iron oxides (eg magnetite), optionally in combination with NiO and / or Cr2O3, are particularly advantageous since they enable the production of steel foams, the necessary carbon being derived from organic compounds in aqueous suspension.

[0049] AgCl or PdCl2 can be used as the compound containing the metal atom, and can be reduced in a hydrogen atmosphere at 200-900°C (for AgCl) or 500-800°C (for PdCl2). In particular, the porous palladium structure can be used for heterogeneous catalysis.

[0050] In addition, MgF2 can be used as a compound containing metal atoms. The porous magnesium structure can be used as a biocompatible bone skeleton.

[0051] A metal structure can be obtained from such a suspension by reducing a dried structure that has been additively manufactured with such a suspension, and optionally sintering it.

[0052] The reduction parameters (especially the temperature) depend on the particle size. On the one hand, the kinetics depend on the surface area and thickness of the particles, and on the other hand, the sintering process can also be carried out simultaneously with the reduction process.

[0053] Advantageously, in such an aqueous suspension of the present invention, the metal oxide powder is Fe3O4 or NiO, or a mixture thereof. In particular, such a variant of the present invention is capable of producing iron-based metal foams and steel foams.

[0054] More advantageously, in such an aqueous suspension of the present invention, the metal oxide particles are oblong. This improves the rheological properties and stability of the aqueous suspension after foaming.

[0055] In another advantageous variant of the present invention, one or more of the compounds containing metal atoms in the aqueous suspension include metal hydrides.

[0056] Particularly advantageously, the metal hydride is TiH x , PdH x , ZrH x or MgH2.

[0057] For the metal hydride MH x , for example the TiH x , PdH x , ZrH x , the parameter x is the absorption ratio between H and M. In the case of Ti and Zr, 0 < x < 2; while in the case of Pd, 0 < x < 1.

[0058] Such a variant of the present invention is capable of obtaining a metal structure by applying a high temperature to a dried structure that has been additively manufactured with the suspension, at which temperature molecular hydrogen leaves the crystal structure of the metal.

[0059] For TiH x , the appropriate temperature range is 350 to 600 °C. For ZrH x , the appropriate temperature range is 600 to 1000 °C. For MgH2, the appropriate temperature range is 200 to 500 °C.

[0060] In yet another variant of the present invention, one or more of the compounds containing metal atoms are metal carbonyl compounds.

[0061] This variant of the invention makes it possible to obtain a metallic structure by subjecting a dried structure previously additively manufactured with the suspension to a high temperature at which the metal carbonyl compound decomposes into metal and carbon monoxide gas.

[0062] Particularly advantageously, the metal carbonyl compound is Rh2(CO)8 or Ru(CO)5.

[0063] For Rh2(CO)8, the appropriate temperature range is 200 to 600°C. For Ru(CO)5, the appropriate temperature range is 300 to 700°C.

[0064] Advantageously, a cationic surfactant, such as hexylamine, is used as the surfactant in the aqueous suspension of the present invention.

[0065] Nonionic surfactants (eg, octyl gallate) may also be advantageously used as surfactants in the aqueous suspensions of the present invention.

[0066] For hexylamine, advantageous surfactant concentrations are between 0.01 and 0.05 mmol / g. The amount of surfactant is advantageously adjusted according to the length of the surfactant hydrocarbon chain.

[0067] Depending on density and chain length, the aqueous suspension according to the invention preferably comprises 0.01 to 20 g / l of binder.

[0068] Particularly advantageously, the binder is methylcellulose, PVA (polyvinyl alcohol) or PVP (polyvinyl pyrrolidone), or a mixture thereof.

[0069] The use of such a binder stabilizes the foam or emulsion and also temporarily stabilizes the dried structure after the printed object has been dried.

[0070] A second aspect of the invention relates to a method of producing a porous metal material.

[0071] The method for producing porous metal material of the present invention comprises the following steps:

[0072] - providing an aqueous suspension as claimed in any one of claims 1 to 8; the aqueous suspension comprising a mixture of at least one compound comprising a metal atom;

[0073] - foaming the aqueous suspension into foam, or emulsifying the aqueous suspension with a lipophilic compound into an oil-in-water emulsion, the oil-in-water emulsion comprising 30-90% by volume of a lipophilic phase, the lipophilic phase not containing a polymerizable compound;

[0074] - foaming the foam or emulsion to form a three-dimensional structure;

[0075] - drying the three-dimensional structure to obtain a dried structure; and

[0076] - subjecting said dried structure to processing conditions such that said compound comprising metal atoms is converted into a metal, obtaining a metallic structure.

[0077] In the method according to the invention, the metal structure is advantageously sintered.

[0078] The method of the present invention has the advantage that small particles (e.g. 0.03-5 μm) of compounds containing metal atoms can be produced more cost-effectively than metal particles of similar size. In addition, these powdered compounds are non-flammable or less flammable than the corresponding powdered metals, and the particle surface is not easily oxidized.

[0079] The foaming step may be performed mechanically, for example by stirring. Alternatively, foaming may be achieved in situ by decomposing a suitable compound, such as hydrogen peroxide.

[0080] In an advantageous variant of the process of the invention, one or more of the compounds comprising metal atoms is a compound reducible to a metal in a gaseous atmosphere; and the metallic structure is obtained by reducing the dry structure by placing it in a reducing atmosphere.

[0081] More advantageously, the reduction is carried out under an atmosphere containing 0.5-100% by volume of H2 in an inert gas.

[0082] The temperature at which the reduction reaction is carried out depends on the metal ions to be reduced. For Fe3O4 as a metal-containing compound, the temperature is advantageously 600 to 1000°C.

[0083] The air content of the obtained iron foam can be 75-98% by volume. The density of the obtained iron foam can be 0.4-2 g / cm 2 . Compared with bulk iron, its relative density can be 0.03 to 0.5.

[0084] In another advantageous variant of the method of the invention, one or more of said compounds comprising metal atoms is an interstitial metal hydride; and the dried structure is brought to a temperature at which hydrogen is released in the form of hydrogen gas, obtaining a metallic structure.

[0085] Advantageously, in the method of the invention in question, the processing step of obtaining the metal structure and the sintering step are carried out in one processing step.

[0086] Also advantageously, in the method of the invention, the three-dimensional structure is formed by additive manufacturing, for example by three-dimensional printing.

[0087] In an advantageous variant of the method according to the invention, the surface of the metal structure is rendered hydrophobic or lipophilic. This enables the produced metal structure to be used for the efficient absorption of lipophilic compounds, such as oil spills floating on the water surface.

[0088] In a further advantageous variant of the method according to the invention, after the reduction step, the metallic structure is at least partially oxidized.

[0089] A third aspect of the invention relates to advantageous uses and applications of the porous metal structure of the invention.

[0090] The metal material of the present invention is produced according to the method of the present invention.

[0091] In an advantageous use of the invention, the metallic material of the invention is used as a resistance heating element.

[0092] The large surface area of ​​the porous metal material and its open-cell structure can efficiently heat the gas or liquid in the pores of the material when an electric current is passed through the material to generate heat in the metal matrix of the material. For example, the metal material of the present invention can be used to vaporize liquids by resistive heating.

[0093] In a further advantageous use of the invention, the metallic material according to the invention is used as a cooling element.

[0094] This advantageous use can be achieved by bringing the material into thermally conductive contact with a Peltier element.

[0095] In yet another advantageous use of the invention, the metal material of the invention is used to absorb lipophilic substances floating on water.

[0096] For this use, the metal material is hydrophobized before the corresponding metal foam is brought into contact with a lipophilic substance (e.g., oil spilled onto water). The hydrophobized surface of the porous metal structure increases the surface tension between its surface and water, which slows down the entry of water into the metal foam filled with air. The metal foam, which has an overall density less than that of water, floats on the water surface. The oil in contact with the metal foam will be sucked into the pores of the metal foam by the capillary effect of the open-cell structure. This enables efficient absorption of lipophilic substances on the enlarged surface, pores, and capillaries of the metal foam.

[0097] Then, the density of the metal foam whose pores are completely filled with oil will eventually be greater than that of water. The metal foam will no longer float but will sink. Therefore, such hydrophobized metal foam can clean up oil spills on water bodies (e.g., offshore) where it is difficult or impossible to collect oil from the surface. The metal foam will sink to the bottom together with the absorbed oil, where they will eventually be covered by sediment.

[0098] For this application, iron is preferably used as the metal since it is relatively cheap and non-toxic.

[0099] Alternatively, the floating metal foam, which is partially filled with oil, can be collected from the surface by using a magnet or a screen.

[0100] In yet another advantageous use of the invention, the metallic material of the invention is used as a heterogeneous catalyst or as a support structure for a heterogeneous catalyst.

[0101] In yet another advantageous use of the present invention, the metal material of the present invention is used as an electrode. To this end, the metal material can be used as a positive electrode and a negative electrode in batteries (including lithium iron phosphate batteries and iron-air batteries) with or without functional coatings.

[0102] In yet another advantageous use of the invention, the metallic material of the invention is used as a component in alkaline electrolysis. Components that can be made from the metallic material are anion and proton exchange membranes, proton transport layers and electrodes.

[0103] In yet another advantageous use of the invention, the metal material of the invention is used as a storage for gases, in particular molecular hydrogen. For example, due to the porosity of the metal material of the invention and the resulting large accessible active sites, it can be used for adsorptive storage of such molecular hydrogen or carbon dioxide. Another approach is to use the metal material of the invention for chemical storage of molecular hydrogen in an iron / iron oxide based storage cycle.

[0104]

[0105] In yet another advantageous use of the invention, the metal material of the invention is used as a filter element. BRIEF DESCRIPTION OF THE DRAWINGS

[0106] In order to facilitate a more complete understanding of the present invention, reference is now made to the accompanying drawings and diagrams. These references should not be construed as limiting the present invention and are merely illustrative.

[0107] Components which are identical or at least identical in their function are provided with identical or similar reference numerals in the following text.

[0108] Figure 1 The manufacturing process of the iron-based multi-level porous material of the present invention is schematically shown.

[0109] Figure 2 Strain-controlled oscillatory rheological measurements performed on foamed aqueous suspensions of the invention are shown.

[0110] Figure 3 A 3D printing process to form a wet foam body is shown.

[0111] Figure 4 shows (a) applied to Figure 5 The heating scheme of the reduction step of the green body, and (b) the XRD spectrum of the obtained fully reduced sample.

[0112] Figure 5 Shows the Figure 2 The multi-layer pore structure of the blank after 3D printing with ink.

[0113] Figure 6 Shows the Figure 5 The multi-level pore structure of the metal body after the green body is completely reduced.

[0114] Figure 7 The microstructure of the iron-based porous structure of the present invention to which different process parameters are applied is shown.

[0115] Figure 8 Shows Figure 7 Measurements of different mechanical properties of iron-based porous structures.

[0116] Fig. 9 It also shows Figure 7 Mechanical properties of iron foam, (a) stress-strain curves for an extended range of applied strain, (b) average mechanical properties of the samples obtained from the stress-strain data.

[0117] Fig.10 The XRD spectrum of the nickel-iron alloy-based metal foam of the present invention having a pure austenite atomic structure (7 wt % Ni, 850° C., 30 hours) is shown.

[0118] Fig.11 Shows Fig.10 SEM image of Ni-Fe alloy metal foam.

[0119] Fig.12 Shown are the (a) average relative density, (b) density, (c) compression modulus, and (d) strength of Ni-Fe alloy metal foams with different Ni contents at two different sintering temperatures.

[0120] Fig.13 The results show that the 28 wt% Ni-containing and sintered at 1000 °C for 30 hours Fig.12 Weibull distribution of the strength of Ni-Fe alloy metal foam.

[0121] Fig.14Different examples of iron-based foams of the present invention are shown, from left to right: unreduced magnetite foam; hematite foam obtained after oxidation of magnetite at 550°C for 2 hours; a foam of 37 wt% hematite and 63 wt% hematite obtained after oxidation of magnetite at 650°C for 2 hours; a sintered hematite foam obtained by sintering at 1000°C for 2 hours.

[0122] Fig.15 Shown are the compositions of the crystalline phases present in the iron porous structure (850° C., 30 hours) after corrosion in phosphate buffer (37° C.) for 1-90 days as determined by XRD spectra with Rietveld fitting.

[0123] Fig.16 SEM images of iron-based porous structure samples sintered at 850°C for 30 hours and subsequently corroded in phosphate buffer (37°C) for 3 days are shown.

[0124] Fig.17 The figures show (a) the compression modulus and (b) the strength of the iron-nickel metal foam of the present invention.

[0125] Fig.18 Shown are the surface areas of printed structures prepared from foams containing different iron oxide particle fractions and heat treated under different reduction / sintering conditions.

[0126] Fig.19 Shown are SEM images of printed structures prepared from metal foams containing different iron oxide particle fractions and heat treated under different reduction / sintering conditions.

[0127] Fig. 20 Resistive heating of Fe-based foams for liquid vaporization is shown. (a) shows an infrared image of a 35% Fe foam (5.6Ω at room temperature) with a voltage applied at 3W over time. (b) shows the average temperature curve of the marked area in (a), and the shooting time points in (a) are indicated by dotted lines in (f). (c) shows an optical image and thermal image (lower right inset) of liquid vaporization by resistive heating using foam infused with essential oil (limonene, 0.4mL / g) as needed.

[0128] Fig.21 It shows that the low density (<1g / cm 3 ) and an iron-based foam element whose surface is modified with hydrophobic fumed silica, which absorbs oil while floating on water.

[0129] Fig. 22 The figure shows the metal foam produced by 3D printing of emulsion ink, (a) is the metal foam after printing, and (b) is the SEM image before sintering.

[0130] Fig.23 Stress-strain measurements of iron-nickel based metal foams are shown.

[0131] Fig.24 The relative compression modulus and relative density of different metal foams after the first and second measurement are shown.

[0132] Fig.25 Different aspects of the measurement of the novel strengthening effect of the metal foam of the present invention are shown.

[0133] Fig.26 The variation of the compression modulus of a metal foam body of the invention after a series of uniaxial compressions along different axes is shown.

[0134] Fig. 27 The engineering strain of low-carbon metal foams extracted by digital image correlation (a, c, f) with the corresponding force-stroke curves (b) and stress-strain curves (d) are shown.

[0135] Fig.28 The assumed strain hardening mechanism is shown, where (a), (b), (c) are schematic stress-strain curves; (d) is a schematic description of the pores of the metal foam of the present invention at three different length scales; and (e) is a SEM image (second and third images) of a real metal foam sample after the first compression cycle.

[0136] Fig.29 Shown are: (a) stress-strain measurements of metal foam samples over the full range of elasticity, yielding and densification and repeated release of the sample; (b) a detailed view of the stress-strain curve of (a) measured in the elastic range; (c) a plot of the elastic modulus E obtained from the measurement in (a) versus strain; and (d) a plot of the elastic modulus obtained versus the solids ratio of the sample.

[0137] The present invention is not limited in scope to the specific embodiments described herein. Indeed, various modifications of the present invention, in addition to those described herein, will be apparent to those skilled in the art from the foregoing description and the accompanying drawings. Therefore, such modifications are intended to fall within the scope of the appended claims. In addition, various references are cited throughout the specification, the disclosures of which are incorporated herein by reference in their entirety. DETAILED DESCRIPTION

[0138] The aqueous suspension of precursor particles containing metal atoms of the present invention enables an extrusion-type 3D printing process for making metal foams (e.g., steel or iron-like porous structures with ultra-high porosity distributed on all three levels). The precursor particles also stabilize the foaming ink.

[0139] By using the particle stabilized foam of the aqueous suspension of the present invention as a 3D printing ink, pores can be generated on multiple length scales. On the first length scale, the pores can be directly controlled by the printing pattern of the foam fiber. On the smaller second length scale, the bubbles of the foaming ink serve as a template for forming a large number of mesopores in the printed fiber. The structure can be controlled by the concentration and distribution of the bubbles in the ink. On the smaller third length scale, pores are generated by heat treatment (e.g., reduction with hydrogen in the case of iron oxide particles) and an optional sintering process that leads to the conversion of the suspended precursor particles.

[0140] This enables, for example, the production of materials with an elastic modulus greater than 300 MPa and a density less than 1 g / cm 3 of iron and iron-based alloys, which is consistent with the expected mechanical efficiency of the porous structure.

[0141] An advantageous manufacturing process for such ferrous metal foam is schematically shown in Figure 1 The fabrication of the iron-based multi-level hierarchical porous structure is a two-step process: the first step involves preparing a stabilized wet foam ink from modified particles, and the second step involves 3D printing the wet foam ink into a three-dimensional structure, followed by reduction and sintering of the dried printed structure.

[0142] Stabilization of wet foams by particles is achieved by reducing the wettability of the particles in the liquid, thereby promoting their adsorption at the air / water interface. Particle adsorption reduces the total interfacial area and lowers the free energy of the system. This energy gain can easily be several orders of magnitude greater than the thermal energy, indicating that adsorption is an irreversible process

[33] . Irreversible particle adsorption makes the particles virtually immune to common foam destabilization processes such as drainage, disintegration due to lamellae rupture, and Oswald ripening

[34] .

[0143] The oval magnetite microparticles 11 are functionalized with short-chain amphiphilic molecules 12 ( Figure 1 (a)) to produce an aqueous suspension 13( Figure 1 (b)). After the suspension is foamed, a foamed ink 1 having bubbles 14 stabilized by oval magnetite particles 11 is obtained ( Figure 1 (c)).

[0144] It was found experimentally that functionalizing magnetite particles with hexylamine (3 μl / g particles) provides ideal wettability, thereby promoting adsorption at the air / water interface, thus producing a strong and stable foam after air incorporation. To prepare such a stable foam, magnetite particles are first suspended and deagglomerated in water containing short-chain amphiphilic hexylamine. The positively charged polar head groups of the molecules adsorb on the negatively charged particle surfaces due to electrostatic interactions. This causes the hydrophobic tails of the amphiphilic substance to protrude outward and makes the entire particle slightly hydrophobic. Mechanical foaming of the suspension of modified particles ultimately produces the desired ultra-stable foam. A particle volume fraction of 50% by weight and an optimized foaming process (10 minutes at 800 rpm) provide additional rheological requirements for printing.

[0145] The stabilized viscoelastic ink 1 can then be used in a direct ink writing (DIW) process to further form a three-dimensional structure 3a ( Figure 1 (d)). The particle-stabilized foaming ink is printed layer by layer by extruding it through a printing nozzle 21 at room temperature and depositing it as a continuous foam filament 31 .

[0146] The DIW method is particularly suitable for fabricating open-cell structures, such as grid-like and open-cell designs.

[0147] Most direct ink writing inks have the following three rheological requirements: First, the ink must be shear thinning, which enables the material to flow through the nozzle at low pressure. Second, the ink must have a high yield stress, below which the ink does not flow, to ensure that the material remains in place after printing. Third, the ink must also exhibit a high storage modulus to prevent sagging across the filament in a grid-like structure. For compressible foams, the printing conditions also need to be adjusted to ensure continuous deposition rather than intermittent extrusion

[35] .

[0148] After the printed wet foam 3a is dried, the resulting blank 3b ( Figure 1 (e)) The cellular structure of the foam is maintained. Figure 1 (e)) The green body 3b is reduced and sintered into a high-porosity lightweight iron foam element 3b ( Figure 1 (f)).

[0149] In order to quantify the rheological behavior and viscoelasticity of particle-stabilized wet foams, strain-controlled oscillatory rheological tests were performed (see Figure 2 The wet foam studied contained 50 wt % iron oxide particles (50 wt %) and 3 μl of hexylamine per gram of iron oxide. The foam exhibited a pronounced viscoelastic response with a storage modulus plateau at low strains and a well-defined yield stress (see Figure 2The measured yield stress of 70 Pa is not far from the recommended range for DIW inks (100-5000 Pa)

[36] . Due to the high plateau storage modulus of 4.86 kPa, the foam is also rigid enough for direct ink writing of grid-like structures.

[0150] DIW printing of viscoelastic wet foam using a desktop extrusion printer equipped with a syringe and a nozzle size of 0.84 mm produced a three-dimensional object 3a (see Figure 3 ). In order to produce a multi-level structure, a grid-like design is chosen, in which the printing path controls the size of the open pores, which will be referred to hereinafter as macropores 32. Such macropores constitute the first level of the multi-level porosity of the metal material of the present invention.

[0151] The ability to print distortion-free meshes verifies the appropriate rheological properties of the ink and suggests that the wet foam can resist the high shear forces applied during extrusion printing (which could otherwise lead to phase separation and bubble collapse). Additionally, the experiments revealed that the high stability and viscoelastic properties of the particle-stabilized wet foam mitigate any compressibility issues under conventional printing conditions.

[0152] After printing, the wet foam object 3a was dried at 60°C for 1 hour. Figure 5 (a)) only solid precursor particles and residual organic compounds remain. Figure 5 As can be seen in the SEM images in (b) and (c), drying results in the formation of a second level of structure consisting of spherical pores 33 originating from the foam cells of the previous wet foam. The dried structure of body 3b exhibits closed-cell pores with an average pore size of 45.6 μm. Since they fall into the medium size range, these spherical pores will be referred to as mesopores 33 below.

[0153] The size of these mesopores can be adjusted by the volume fraction of the particles, the concentration of the amphiphilic substance and the foaming speed. In general, an increase in the content of particles and amphiphilic substances will increase the viscosity of the suspension, thereby reducing the bubble size due to the higher shear stress generated during the mechanical foaming process. The increase in shear caused by a higher foaming speed may also lead to a decrease in bubble size.

[0154] The green body 3b can be converted into the multi-level porous metal body 3c by performing heat treatment at a temperature of 690°C to 1000°C in a reducing atmosphere. Figure 5 The blank 3b was heat treated at 850°C for 30 hours under a reducing gas flow of 5% H2 and 95% N2. The corresponding temperature curve is Figure 4The XRD spectrum of the fully reduced metal body 3c shows a clear correlation with the diffraction peaks expected for the ferrite (α-Fe) atomic structure, thus demonstrating that the initial magnetite was fully reduced to ferrite iron (see Figure 4 (b)). Under the given parameters, sintering was carried out simultaneously with the reduction of magnetite to iron particles. Chemical analysis of the reduced sample revealed that the porous iron structure contained 0.204±0.077 wt% carbon, of which the organic compounds in the wet foam were the carbon source.

[0155] If Figure 6 The metal foam body 3c shown in (a) is Figure 5 When compared with the green body 3b shown in (a), it can be seen that the combined reduction and sintering process results in a linear shrinkage of about 50%. Figure 6 As can be seen in the SEM images of (b) and (c), reduction and sintering also lead to the opening of the closed-cell mesopores 32 produced during the foaming process, so that micropores 34 are formed in the walls of the mesopores 33 templated by the bubbles. Combined with the macropores 32 produced by the printing path, this leads to a unique open-cell porous structure with three levels of multi-level porosity.

[0156] To demonstrate the possibility of adjusting the bubble size and thus the mesopores of the material of the present invention, the particle concentration of the foam was reduced from 50 wt % in the examples discussed above to 40 wt % while keeping the amphiphilic substance concentration and the foaming process unchanged. It was found that the foam with this lower particle concentration was still rigid enough to 3D print a grid-like structure. The foam with 40 wt % particles resulted in larger mesopores with an average particle size of 125.1 μm.

[0157] The reduction reaction is influenced by several factors, including sample volume, gas flow rate, H2 and H2O content of the reducing gas, oxide particle size and temperature. Depending on the temperature and particle size, the reduction is also accompanied by a sintering process of the metal particles and metal oxide particles. In order to explore this part of the sample processing parameter space, the influence of different reduction schemes on the microstructure, relative density and mechanical properties of the resulting multilayer porous materials was studied. To this end, samples produced with the 50 wt. % magnetite ink discussed above were systematically heat treated at 750°C, 850°C and 1000°C for 30 h and under optimized conditions (40 h at 690°C). SEM images of the green body before reduction and the metal foam after reduction and at Figure 7 Some mechanical properties of the samples have been measured and the results are shown in Figure 8 (a), (b) and (c). The symbols used in the figures correspond to Figure 7 Square, circle, diamond and hexagon symbols for the corresponding samples in .

[0158] Figure 8(a) shows the stress-strain curves of the sample reduced and sintered under optimized conditions (40 hours at 690°C) compared with the samples reduced at 750°C, 850°C and 1000°C for 30 hours. Fig. 9 (b) shows the stress-strain curves of the samples in the strain extension range, while Fig. 9 (b) shows the elastic modulus and yield strength obtained from the stress-strain data.

[0159] Figure 8 (b) shows a plot of absolute and relative compressive modulus (compared to solid materials) versus relative density (compared to solid metals). Figure 8 (c) shows the relationship between yield strength and relative density (compared to solid metal). Literature data for printed iron structures without templated macropores are shown for comparison (grey triangles, Taylor et al.

[26] ; grey stars, Sharma et al. [7]). The theoretical scaling dependence expected from the open-cell foam model is also shown (see LJ Gibson, MF Ashby, Proceedings of the Royal Society of London. Series A, Mathematical and Physical Sciences 1982, 382, ​​43).

[0160] Significant changes can be observed in the microstructure of samples heat treated between 750°C and 1000°C ( Figure 7 ). It was found that heat treatment at 750°C was sufficient to form micropores on the walls of the mesopores while maintaining the original foam-like structure of the green body. At 850°C, the size of the micropores increased significantly, but the mesopores templated by the foam remained visible. Increasing the temperature to 1000°C resulted in a lower surface area and caused the fusion of micropores with mesopores. This produced an open-cell network with only two levels of multi-level porosity.

[0161] Along with the changes in the microstructure, the measured carbon content decreased from 0.20 ± 0.08% at 850 °C to 0.05 ± 0.01% at 1000 °C. This decrease may be caused by the long-term exposure of the high surface area structure to high temperatures, which allows the carbon to diffuse out of the material. From this microstructural analysis, it was concluded that high temperatures should be avoided to maintain high carbon content and three levels of multi-level porosity.

[0162] A particularly advantageous multi-level steel structure with three levels of porosity was ultimately obtained by adopting a two-step process as follows: the sample was first fully reduced at 690° C. for 40 hours and then sintered at 850° C. for 2 hours. This provided the microstructure of the sample reduced at low temperature, but with thicker struts due to sintering.

[0163] Mechanical characterization revealed that the elastic modulus and compressive yield strength of the porous metal structure increased with heat treatment temperature ( Figure 8 (a) Fig. 9 (a), (b)). Since the relative density of all samples remained in a similar range of 0.053 to 0.268, the strengthening effect can be attributed to the formation of a stronger solid by the high temperature sintering. The best heat treatment scheme maintained 0.86 ± 0.03 g / cm 3 The extremely low average density provides the strongest structure with the greatest rigidity yet.

[0164] To compare these multi-level porous structures with other ferrous porous materials, mechanical data of previously reported structures are presented in an Ashby-type plot describing the effect of relative density on elastic modulus and compressive strength ( Figure 8 (b), (c)). Compared to the materials of the prior art [7,26], it was found that the presence of three levels in the porous structure of the present invention leads to a significantly lower relative density, which is within a parameter range that was previously difficult to achieve. Importantly, the elastic modulus and compressive strength of the material of the present invention depend on the relative density, which is similar to that observed in the reference structure. This dependence is highly consistent with the theoretical expectations of the Ashby-Gibson model of open-cell foams, thus indicating that the new material shown combines extremely low weight with the maximum possible properties. By reducing the relative density without affecting the expected properties, the multi-level porous structure achieves the mechanical efficiency of the prior art by reducing the amount of solid phase used by 30%.

[0165] The proposed multi-level pore design can be extended to a range of other iron oxides and iron-based alloys. To illustrate this, NiO and Fe3O4 particles were used as inorganic precursors in the initial printable foam as a multi-level porous Ni-Fe alloy. Nickel is a common alloying material for steel because it ensures that the steel retains its strong high-temperature crystal structure, austenite.

[0166] The nickel content of the alloy can be finely controlled by adjusting the relative fractions of the oxide powders used in the foam formulation. This was verified by elemental analysis (proton induced X-ray emission) of an alloy designed to contain 28 wt% (calculated) nickel. After heat treatment of the dried precursor foam, the alloy was found to contain 27.3 wt% Ni atoms. X-ray diffraction analysis confirmed the formation of austenite ( Fig.10 Interestingly, it was observed that the microstructure of the Ni-Fe porous structure was independent of the sintering parameters and the Ni alloying content ( Fig.11 ).

[0167] Figure 8 (d), (e) and (f) show the Figure 8 (a), (b), (c) are equivalent measurements of metal foam samples produced with different processing temperatures and with different nickel contents in the final metal foam, i.e., 0, 7, 14, 21, 28, and 35 wt. % Ni, the remainder being iron. Note that Figure 8 In (d), the curve for the 21 wt% Ni sample stops before the sample yields due to technical limitations. Again, all data are compared with literature data obtained for iron-based printed structures without templated macropores (grey triangles, Taylor et al.

[26] ; grey stars, Sharma et al. [7]). Theoretical scaling dependence expected from the open-cell foam model is also shown (Gibson, Ashby, 1993). Fig.12 Shown are (a) relative density, (b) density, (c) elastic modulus, and (d) yield strength of the same nickel-iron alloy metal foam at two different sintering temperatures. Fig.13 Shows Fig.12 Weibull distribution of the strength of Ni-Fe alloy metal foam containing 28 wt% Ni and sintered at 1000°C for 30 hours.

[0168] In terms of mechanical properties, measurements show that the addition of nickel significantly improves the elastic modulus and compressive strength of porous Fe-based alloys. Similar to the pure iron composition, the presence of three pore levels leads to a significantly lower relative density than previously reported iron-based porous materials. Because the measured mechanical properties still follow the trend expected by theoretical expectations, this reduction in relative density is achieved without affecting the mechanical efficiency of the porous structure. Compared with pure iron counterparts with similar density, it is found that the nickel present in the iron-based alloy increases the elastic modulus of the porous structure by 7.5 times and increases the compressive strength by 5 times.

[0169] The iron-based porous structure can be used as pure iron foam, as metal oxide foam or as a foam of a mixture of metal and metal oxide in a wide range of applications. Iron oxide foams with tailored chemical compositions can be obtained by heat treating the 3D printed green body object at an intermediate temperature of 550-650°C. Heat treatment at 550°C in an air atmosphere for 2 hours results in partial oxidation of magnetite to brown hematite. Red hematite structures can be obtained by heat treating the 3D printed magnetite foam at 650°C in air for 2 hours. Fig.14Variants of such lightweight, permeable, high surface area structures 3D printed according to the present invention are shown (from left to right): unreduced magnetite foam; hematite foam obtained after oxidation of magnetite at 550°C for 2 hours (brown); 37 wt% hematite / 63 wt% hematite foam obtained after oxidation of magnetite at 650°C for 2 hours (red); sintered hematite foam obtained by sintering at 1000°C for 2 hours (silver). Although these oxide foams are relatively soft, their mechanical properties can be improved by adding binders or by sintering. For example, sintering a hematite sample at 1000°C results in a more mechanically strong porous structure with a smooth and shiny surface, the silver color of which is characteristic of sintered hematite. Such oxide foams can be used as substrates for gas phase catalysis, for example for methanol oxidation

[37] , toluene cracking

[38] or formic acid decomposition

[39] .

[0170] The porous metal structure itself exhibits the intrinsic magnetism and resistivity of iron (0.00125Ωm).

[0171] The mixed iron / titanium oxide porous structure can be obtained by partial oxidation of the iron oxide body. The composition of the crystalline phase present in the iron porous structure (30 hours at 850°C) after 1-90 days of oxidative corrosion in phosphate buffer (37°C) determined by Rietveld fitting of the XRD spectrum is Fig.15 and are shown in Table 1. The SEM images of the iron-based porous structure samples sintered at 850°C for 30 hours and then corroded in phosphate buffer (37°C) for 3 days are shown in Fig.16 Shown in.

[0172] Table 1: Composition after 1-90 days of corrosion in phosphate buffer (37°C) determined by Rietveld fitting of XRD spectra

[0173]

[0174] Fig.17 The (a) relative and absolute compression modulus and (b) relative and absolute yield strength, as well as (b) strength of the iron-nickel metal foam of the present invention are shown, and the literature values ​​(grey triangles, Taylor et al.

[26] ) and the theoretical values ​​of the open-cell foam structure expected by Gibson-Ashby are also shown.

[0175] The measured surface areas of printed structures prepared from hybrid foams containing different iron oxide particle fractions and heat treated under different reduction / sintering conditions are Fig.18 Shown in.

[0176] Fig.19SEM images of metal foams containing different iron oxide particle fractions (containing 40, 45 and 50 wt.% iron oxide compared to iron) and heat treated under different reduction / sintering conditions are depicted in Figure 1. (a) 40 hours at 690°C and sintered; (b) 30 hours at 1000°C; (c) 30 hours at 850°C; (d) 30 hours at 815°C; (e) 30 hours at 730°C; (f) 15 hours at 730°C; (g) 70 hours at 650°C; (h) before reduction.

[0177] Since the mixed iron / iron oxide foams have a higher resistivity compared to their pure iron counterparts (0.7 Ωm for 35 wt% iron at room temperature), these porous materials can be used for resistive heating, for example as low-power resistive evaporators. In the experiments, it was observed that Joule heating with a power of only 3 W was sufficient to heat an 8 mm wide cubic porous structure to a stable temperature of 180 °C. The steady state is reached due to the combination of resistive heating and the high surface area of ​​the structure (1 m 2 / g) to achieve a balance between convection cooling.

[0178] Fig. 20 The use of the iron / iron oxide foam of the present invention as a resistive heating element is shown, for example for vaporization on demand of liquids. Fig. 20 (a) shows an experimental setup for liquid vaporization by resistive heating. A metal foam 3c with 35 wt% Fe injected with essential oil (limonene, 0.4 mL / g) is sandwiched between two electrodes 23 and 23'. A voltage is applied to the metal foam to obtain an output of 3 W of power. The inset at the lower right corner shows an infrared image of the area marked by the dashed line. Fig. 20 (b) shows the infrared image changing with time. The average temperature of the sampling area marked by the dotted line changes with time. Fig. 20 (c) is shown. The dotted line indicates Fig. 20 (b) Shooting time points.

[0179] In addition, the extremely low density (<1 g / cm 3 ) to make it light enough to float on water, considering the density of pure iron (about 8g / cm 3 ), which is unusual. The multi-level open-cell structure produced by the reduction process is responsive to liquids that wet the metal surface like a sponge. Under adverse wetting conditions, capillary forces allow at least 0.4 ml / g of liquid to be spontaneously absorbed into the porous structure. The capillary forces were observed to be strong enough to draw liquid not only into the micropores, but also into the 3D-printed channels.

[0180] Since such metal foams can float on water, they can be used as environmentally friendly oil absorbers. For this application, the surface of the metal structure is hydrophobized with fumed silica by dip coating. This hydrophobization process makes the surface wettable by oils and other non-polar solvents, ensuring that these liquids are absorbed into the porous structure at the same time. Fig.21 As can be seen in Figure 3, the hydrophobized iron foam can absorb hexane floating on the water surface very effectively (dyed for better visualization). The oil droplet 41 on the water surface is absorbed by the metal foam 3c within 20 seconds. The oil wets the hydrophobized surface of the metal foam, and the oil is contained in the structure within the micropores and macropores.

[0181] The specific advantage of using a porous structure as an oil absorbent comes from its ability to float on water, which enables the absorption of oil exactly where it is. As the oil replaces the air in the pores and channels, the density of the structure increases until it begins to sink. This enables the cleanup of crude oil spills where the oil is contained in a metal body and then deposited on the bottom of the ocean.

[0182] Another method for producing the metal foam of the present invention is to use an emulsion ink system instead of a wet foam ink system. Compared with the composition of the wet foam, the surfactant concentration is increased by 5-50 times (for example: 1mmol / g of hexylamine, 0.1mmol / g of octyl gallate). 30-80% by volume of a hydrophobic organic solvent (for example, n-octane) is added dropwise while mixing. The pH can be adjusted to the pKa of the surfactant (with NaOH or HCl, respectively) to improve emulsification. Binders such as methylcellulose, PVA (polyvinyl alcohol) and PVP (polyvinyl pyrrolidone) can be used to stabilize the resulting emulsion (1-7g / L). Emulsion inks can be processed in the same manner as foams (printing, drying, sintering, reduction). In this case, macropores are produced by organic solvent droplets in the emulsion, similar to bubbles in the foam. The metal foam produced by 3D printing of this emulsion ink system is Fig. 22 Shown in.

[0183] Furthermore, it has surprisingly been found that the porous metal structures of the present invention exhibit a particular strain hardening behavior.

[0184] The stress-strain measurements were carried out on the iron foam and the nickel-iron alloy, and the elastic modulus E1 was determined in a proportional range. The measurement was then repeated. Unexpectedly, the elastic modulus E2 was found to be significantly higher in this second run. For the nickel-iron alloy foam with 7 wt. % Ni reduced at 850° C. for 30 hours, the elastic modulus E1=565 MPa was measured in the first run, while the elastic modulus E2=2724 MPa was measured in the second run (see Fig.23 ). It was found that all investigated metal foams of the present invention have the same effect. Fig.24The relative elastic modulus versus relative density (compared to solid metal) of two iron foams (process parameter groups R2 and R7 in Table 2) and nickel-iron alloy foams with 7, 14, 21, 28 wt% Ni (process parameter groups R2 and R7 in Table 2) are shown. All samples show similar increases in elastic modulus and increases in density.

[0185] After compression 2-20 times with a Poisson's ratio of <0.01 in the compressive direction, the compression modulus will improve. This uniaxial strengthening will not be accompanied by a density change of more than 2.5% and is permanent as long as only uniaxial stress is applied ( Fig.24 , Fig.25 ). Changing the direction of the applied stress will reset the material and the effect will reappear ( Fig.26 ).

[0186] The data of stress-strain measurements of metal foams are shown in Fig.23 As can be seen in Figure 1, the effect of the increase in the elastic modulus is permanent. The sample was repeatedly released and the measurement was subsequently resumed. In contrast to the initial proportional increase (resulting in an elastic modulus E1), a significantly higher (almost 500%) elastic modulus E2 was found after the first and all subsequent release and recovery cycles. The sample itself remained undeformed (no increase in cross-sectional area).

[0187] Fig.25 (a) and (b) show the average elastic modulus and density determined in the first, second and third measurement runs for three metal foams (4 samples each) with different solid loadings. The solid loading always refers to the weight percentage of the magnetite powder, unless otherwise stated. For all metal foam types, both values ​​increase with the number of runs. However, the increase in density does not exceed 2.5%. Fig.25 (c) shows the corresponding results in a graph of relative modulus versus relative density. The ratio of the elastic modulus after the second run to that after the first run is Fig.25 (d) shows that Fig.25 (e) shows the corresponding density ratio. Fig.25 (f) shows these values ​​in a plot of modulus ratio versus density ratio. The results do not match Ashby's expectations (E spec =c1ρ spec 2 , c1=1, as a straight line drawn on Fig.25 (c), (f)).

[0188] The stress hardening effect is uniaxial. Fig.26The elastic modulus of a metal foam sample is shown as determined in a series of uniaxial stress-strain measurements (marked with circled numbers 1-8) along different axes, namely normal to the XY plane (Z axis), normal to the YZ plane (X axis), normal to the XZ plane (Y axis) and normal to the XY plane again (Z axis). The strain hardening effect occurs independently along these three axes, X, Y and Z. Interestingly, while the strain hardening effect is permanent in the case where the compressive axis remains unchanged (see Fig.23 ), but after compression along all three axes this effect seems to reset and the effect appears a second time (as shown by the pair of measurements 7 and 8).

[0189] Fig. 27 Results of measurements on metal foam samples are shown for studying local strengthening along the direction of applied stress. A first metal foam sample (mild steel treated at 850°C and with a relative density of 0.11) was subjected to two compression cycles (1) and (2). The measured force is plotted against the stroke length ( Fig. 27 For these two compression cycles, digital image correlation (DIC) shows the engineering strain along the compression direction at a force of 70 N in the color map (see Fig. 27 (a)), where the compression axis is along the vertical direction of the figure. A second metal foam sample (mild steel treated at 1000°C and with a relative density of 0.22) was subjected to two compression cycles (1) and (2), and the measured force was plotted against the stroke width ( Fig. 27 The DIC strain images of these two compression cycles at a force of 40 N were obtained again (see Fig. 27 (c)).

[0190] Fig. 27 (d) shows the stress-strain curve measured for a third metal foam sample (mild steel treated at 850°C, with a relative density of 0.21 and a hole with a diameter of 3.5 mm drilled in the middle) through two compression cycles (1) and (2). The compression modulus obtained is Fig. 27 (e) shows the corresponding DIC image of the dimensionless engineering strain along the compression direction. Fig. 27 (f) The holes are used to show the local strain hardening in response to the defect.

[0191] Without wishing to be bound by a particular theory, e.g. Fig.28 As shown (see Fig.28 (a, b, c)), it is believed that the strain hardening effect occurs due to the superposition of stress responses at two different length scales. During compression, the local stress is large enough to cause the densification of micropores in the walls of the macropores (see Fig.28(d, e)). This change is plastic and it increases the connectivity of the macropore walls, which affects the overall compression response. Since the densification of the microstructure occurs locally, it is anisotropic and only affects the modulus in the compression direction.

[0192] Fig.29 (a, b) show stress-strain measurement curves of a metal foam sample (mild steel treated at 850°C and with a relative density of 0.22) over the full range of elasticity, yielding and densification and repeated release of the sample. Fig.29 (c) shows the elastic modulus E value obtained from the applied strain measurement; and Fig.29 (d) shows the elastic modulus values ​​within the elastic range obtained according to the solid ratio of the sample. 表观 When the elastic state changes to the yield state, E reaches its maximum value E 真实 During the first compression, the stress-strain curve appears to contain the standard elastic phase, yielding and subsequent densification seen in foamed materials. However, the elastic phase is only pseudoelastic. Cyclic compression shows that the elastic modulus increases logarithmically with the compressive force until it reaches the true modulus E observed in the second compression. 真实 This effect does not appear as an obvious overall densification, but rather as an effect of microstructural improvement.

[0193] Nanoporous gold structures obtained by dealloying Ag97Au3 are known to exhibit similar effects at the nanoscale and in macropores [40,41]. However, to date, such effects are not known to exist in microstructures with low porosity in the micrometer length range (which can be obtained with the metal foams of the present invention) or at such low strains (<5%).

[0194] Materials and methods

[0195] Ink preparation : A suspension of 40-50 wt% metal oxide powder (magnetite, Fe3O4, E8840, DOWA; green nickel (II) oxide, 99%, abcr GmbH) and 3 μl / g of hexylamine (99%, ACROS Organics) was prepared by The samples were homogenized by ball milling with alumina beads (1-5 mm in diameter) at 2000 rpm for 6 min (divided into two 3-min sessions to avoid overheating) in a mixer (ARE-250). The standard component contains 50 wt% magnetite powder. The slurry was then formed with an electronic stirrer (Heidolph, RZR 2102) at 800 rpm until the desired hardness was achieved (5-15 min). The resulting foam was left in a sealed container overnight and then volume printed using a modified fused filament fabrication (FFF) printer (Ultimaker 2+) using a 20 mL syringe and a conical nozzle (0.84 mm in diameter). The printing speed was set to 10 mm / s, and the extrusion rate (100-150%) was manually adjusted to achieve the highest print quality. The samples were coated with a commercially available moisturizer to avoid adhesion. The PMMA plate was used as the substrate. The final sample was dried at room temperature overnight or in an oven at 60 °C for 1 h.

[0196] Print structure restoration The samples were reduced in a quartz tube oven (Gero, SR-A 100-500 / 12) with a forming gas flow (95% N2 and 5% H2, Pangas) of 12 l / min. Various heating schemes (Table 2) were used to study the effects of reduction and sintering conditions on the microstructure and properties of the resulting porous metals (see Figure 7 and Figure 8 ).

[0197] Table 2: Reduction and sintering parameters used to transform printed foam structures into porous metals

[0198]

[0199] Oxidation of printed structures : Magnetite foam printed as above was oxidized into different oxidation phases by heating the samples at 650°C, 750°C or 1000°C for 2 h (Naberthem, LE 6 / 11 / P300) (see Fig.14 In addition to thermal oxidation, the porous iron structures were partially oxidized in a wet state by placing them in Dulbecco's phosphate buffered saline (Sigma) at 37°C for 1-90 days (see Fig.16 , Table 1).

[0200] Surface hydrophobization The sample was dip-coated in a 1 wt % suspension of hydrophobic fumed silica (Wacker, HDK H18) in hexane (>95%, Sigma), and the coated sample was then vacuum-dried at room temperature to hydrophobize the multi-level porous structure (see Fig.21 ).

[0201] Microstructure characterization: High-resolution SEM images of the foams before and after reduction were collected using a scanning electron microscope (LEO 1530 instrument, Zeiss GmbH, Germany).

[0202] Composition characterization X-ray diffraction spectra were collected using a powder diffractometer (PANalytical Empyrean) equipped with a Cu Kα X-ray tube (15 kV, 40 mA) and a monochromator. The samples were prepared by crushing them into powder (if they were friable) or by compressing them into flat plates (if they were hard). Particle-induced X-ray emission (PIXE) measurements were performed by the Max Planck Institute of Technology at the Ion Beam Physics Laboratory of ETH Zurich. The carbon content of the iron samples was measured with a carbon / sulfur analyzer (LECO CS230) using four 1 g samples for each composition.

[0203] Mechanical characterization :Compressive strength and modulus were measured using a universal testing machine (AGS-X, Shimadzu) equipped with a 1000N load cell. To ensure that the relative faces were parallel, the samples were ground (Struers, LaboPol-25, 1000 mesh SiC paper) into a specific shape, and ethanol was used as a lubricant to prevent sample oxidation. The test was performed by applying a constant displacement rate of 12 mm / min. The raw data was corrected to take into account the mechanical compliance of the testing machine. The mechanical compliance was measured using an aluminum cube of 9 mm×9 mm×8 mm as a placeholder. Evaluation Data: The reported compressive yield strengths were determined using the 0.2% offset method.

[0204] Surface area characterization : N2 gas adsorption measurements were performed with a pore size analyzer (Quantachrome Autosorb iQ) at 77 K. Before the measurements, the samples were vacuum degassed at 80°C for 24 h. The surface area was determined by the Brunauer-Emmett-Teller method.

[0205] Absorption experiment The oil absorption capacity of the hydrophobized porous iron structure was evaluated by placing the sample floating on water in contact with hexane (>95%, Sigma) as an absorbent (see Fig.21 ). Hexane was dyed purple with 0.01 g / L of Nile red (Merck) and methylene blue (Merck).

[0206] Conductivity and Resistive Heating Experiments The resistive heating capability of the partially oxidized porous iron structure was evaluated by pressing the sample between copper tapes and applying current using a laboratory power supply (EA-PS-3032-05-B) (see Fig.21The temperature of the samples was measured by infrared imaging (IRCAM, Millenium 327k S / M). R-(+)-limonene (Merck) was used as the vaporizing agent.

[0207] The present invention is not limited in scope to the specific embodiments described herein. Indeed, various modifications of the present invention, in addition to those described herein, will be apparent to those skilled in the art from the foregoing description and the accompanying drawings. Therefore, such modifications are intended to fall within the scope of the appended claims. In addition, various references are cited throughout the specification, the disclosures of which are incorporated herein by reference in their entirety.

[0208] Reference numerals

[0209] 1 Foaming water suspension, wet foam ink

[0210] 11 Precursor particles

[0211] 12 Surfactant molecules

[0212] 13 Water

[0213] 14 bubbles, foam holes

[0214] 21 Printing nozzle

[0215] 22 Tube Oven

[0216] 23,23' electrode

[0217] 3a Three-dimensional structure

[0218] 3b Blank

[0219] 3c Metal foam element

[0220] 31 Foam filament

[0221] 32 First level hole, large hole

[0222] 33 Secondary pores, mesopores

[0223] 34 Third level holes, micro holes

[0224] 41 Oil Drop

[0225] References

[0226] [1]L.-P.Lefebvre,J.Banhart,DCDunand,Adv.Eng.Mater.2008,10,775.

[0227] [2]J.Erlebacher,MJAziz,A.Karma,N.Dimitrov,K.Sieradzki,Nature 2001,410,450.

[0228] [3]MECox,DCDunand,Mat Sci Eng a-Struct 2011,528,2401.

[0229] [4]E.Linul,L.Marsavina,PALinul,J.Kovacic,Compos Struct 2019,209,490.

[0230] [5]MHSun,SZHuang,LHChen,Y.Li,XYYang,ZYYuan,BLSu,Chem SocRev 2016,45,3479.

[0231] [6]N.Kleger,M.Zihova,K.Masania,ARSTudart,JFLoffler,Adv Mater2019,31.

[0232] [7]P.Sharma,PMPandey,Mater Design 2018,160,442.

[0233] [8]R.Orinakova,R.Gorejova,ZOKralova,L.Haverova,A.Orinak,I.Maskal'ova,M.Kupkova,M.Dzupon,M.Balaz,M.Khrubovcakova,T.Sopcak,A.Zubrik,M.Orinak,ApplScik,2050.

[0234] [9]S.Ray,U.Thormann,M.Eichelroth,M.Budak,J.Biehl,M.Rupp,U.Sommer,T.ElKhassawna,FIAlagso,M.Kampschulte,M.Rohn ke,A.Henss,K.Peppler,V.Linke,P.Quadbeck,A.Voigt,F.Stenger,D.Karl,R.Schnettler,J.Heiss,KSLips,V.Alt,Biomaterials 2018,157.1.

[0235]

[10] Y.Conde,JFDespois,R.Goodall,A.Marmottant,L.Salvo,C.San Marchi,A.Mortensen,Adv Eng Mater 2006,8,795.

[0236]

[11] ARStudart,A.Nelson,B.Iwanovsky,M.Kotyrba,AAKundig,FHDallaTorre,UTGonzenbach,LJGauckler,JFLoffler,Journal of Materials Chemistry2012,22,820.

[0237]

[12] YJQuan,FMZhang,H.Rebl,B.Nebe,O.Kessler,E.Burkel,Math Sci Eng-Struct 2013,565,118.

[0238]

[13] AEJakus,NRGeisendorfer,PLLewis,RNShah,Acta Biomater 2018,72,94.

[0239]

[14] ARStudart,Chemical Society Reviews 2016,45,359.

[0240]

[15] ARStudart,RMErb,R.Libanori,in Hybrid and HierarchicalComposite Materials,DOI:10.1007 / 978-3-319-12868-9_8(Eds:C.-S.Kim,C.Randow,T.Sano),Springer International Publishing 2015,Ch.8,p.287.

[0241]

[16] B.Gorny,T.Niendorf,J.Lackmann,M.Thoene,T.Troester,HJMaier,Materials Science and Engineering:A 2011,528,7962.

[0242]

[17] LSBertol,WKJúnior,FPdSilva,C.Aumund-Kopp,Materials&Design2010,31,3982.

[0243]

[18] L.Yang,O.Harrysson,D.Cormier,H.West,H.Gong,B.Stucker,JOM 2015,67,608.

[0244]

[19] LEMurr,SMGaytan,F.Medina,H.Lopez,E.Martinez,BIMachado,DHHernandez,L.Martinez,MILopez,RBWicker,J.Bracke,PhilosophicalTransactions of the Royal Society A:Mathematical,Physical and EngineeringSciences2010,368,1999.

[0245]

[20] P.Heinl,L.Müller,C. RFSinger,FAMüller,ActaBiomater.2008,4,1536.

[0246]

[21] C.Xu,QHWu,G.L'Esperance,LLLebel,D.Therriault,MaterDesign2018,160,262.

[0247]

[22] M.Calvo,AEJakus,RNShah,R.Spolenak,DCDunand,Adv Eng Mater2018,20.

[0248]

[23] AEJakus,SLTaylor,NRGeisendorfer,DCDunand,RNShah,AdvFunct Mater 2015,25,6985.

[0249]

[24] BYAhn,D.Shoji,CJHansen,E.Hong,DCDunand,JALewis,Adv.Mater.2010,22,2251.

[0250]

[25] SLTaylor,AEJakus,RNShah,DCDunand,Adv.Eng.Mater.2017,19,1600365.

[0251]

[26] SLTaylor,AEJakus,RNShah,DCDunand,Adv Eng Mater 2017,19.

[0252]

[27] J.Minas,D.Carnelli,E.Tervoort,ARSTudart,Adv Mater 2016,28,9993.

[0253]

[28] C.Minas,J.Carpenter,J.Freitag,G.Landrou,E.Tervoort,G.Habert,ARSTudart,Acs Sustain Chem Eng 2019,7,15597.

[0254]

[29] DGMoore,L.Barbera,K.Masania,ARSTudart,Nature Materials 2020,19,212.

[0255]

[30] L.Alison,S.Menasce,F.Bouville,E.Tervoort,I.Mattich,AOfner,ARSTudart,Sci Rep-Uk 2019,9.

[0256]

[31] MRSommer,M.Schaffner,D.Carnelli,ARSTudart,Acs AppliedMaterials&Interfaces 2016,8,34677.

[0257]

[32] J.Kenel,NRGeisendorfer,RNShah,DCDunand,Addit Manuf 2021,37.

[0258]

[33] R.Murakami,S.Kobayashi,M.Okazaki,A.Bismarck,M.Yamamoto,Front Chem2018,6.

[0259]

[34] U.T.Gonzenbach,A.R.Studart,E.Tervoort,L.J.Gauckler,AngewandteChemie-International Edition 2006,45,3526.

[0260]

[35] H.Ovaici,M.R.Mackley,G.H.McKinley,S.J.Crook,J Rheol 1998,42,125.

[0261]

[36] D.Kokkinis,M.Schaffner,A.R.Studart,Nat Commun 2015,6.

[0262]

[37] M.Bowker,E.K.Gibson,I.P.Silverwood,C.Brookes,Faraday Discuss2016,188,387.

[0263]

[38] X.H.Zou,T.H.Chen,H.B.Liu,P.Zhang,D.Chen,C.Z.Zhu,Fuel 2016,177,180.

[0264]

[39] S.A.Halawy,S.S.Al-Shihry,M.A.Mohamed,Catal Lett 1997,48,247.

[0265]

[40] S.Shi,Y.Li,B.N.Ngo-Dinh,J.Markmann,J.Weissmuller,Science 371,1026-1033(2021).

[0266]

[41] B.Zandersons,L.Lührs,Y.Li,J.Weissmüller,Acta Mater 2021,215,116979.

Claims

1. An aqueous suspension for producing a porous metal structure, the aqueous suspension comprising: A mixture of 2 to 49% by volume of at least one compound containing metal atoms, wherein The at least one compound is solid at room temperature, is in powder form, and is suspended in water; and For each mol of the compound comprising a metal atom, the aqueous suspension comprises 10 -9 To 0.1 mol of surfactant, wherein the aqueous suspension is part of a foam; and / or wherein the aqueous suspension is part of an oil-in-water emulsion comprising 30-90% by volume of a lipophilic phase, the lipophilic phase being free of polymerizable compounds.

2. The aqueous suspension according to claim 1, wherein One or more of the compounds comprising a metal atom is a compound that is reducible to a metal in a gas atmosphere.

3. The aqueous suspension according to claim 1 or 2, wherein The mixture of at least one compound comprising metal atoms is a metal oxide powder.

4. The aqueous suspension according to claim 3, wherein The metal oxide powder is Fe3O4 or NiO, or a mixture thereof.

5. The aqueous suspension according to claim 4, wherein The particles of the metal oxide powder are oblong.

6. The aqueous suspension according to claim 1, wherein One or more of the compounds comprising a metal atom is a metal hydride.

7. The aqueous suspension according to claim 6, wherein The metal hydride is TiH x , PdH x , ZrH x or MgH2.

8. The aqueous suspension according to claim 1, wherein One or more of the compounds comprising a metal atom is a metal carbonyl compound.

9. The aqueous suspension according to claim 8, wherein The metal carbonyl compound is Rh2(CO)8 or Ru(CO)5.

10. An aqueous suspension as claimed in any one of the preceding claims, wherein The surfactant is a cationic surfactant or a nonionic surfactant.

11. An aqueous suspension as claimed in any one of the preceding claims, wherein The aqueous suspension contains 1-7 g / l of binder.

12. The aqueous suspension according to claim 11, wherein The binder is methylcellulose, PVA (polyvinyl alcohol) or PVP (polyvinyl pyrrolidone), or a mixture thereof.

13. A method for producing a porous metal material, the method comprising the following steps: - Providing an aqueous suspension as described in any one of claims 1 to 11; the aqueous suspension comprises: a mixture of at least one compound containing a metal atom; - foaming the aqueous suspension into foam, and / or emulsifying the aqueous suspension with a lipophilic compound into an oil-in-water emulsion, the oil-in-water emulsion comprising 30-90% by volume of a lipophilic phase, the lipophilic phase being free of polymerizable compounds; - forming a three-dimensional structure with the foam or emulsion; - drying the three-dimensional structure to obtain a dry structure; and - subjecting said dried structure to processing conditions causing said compound comprising metal atoms to be converted into a metal, obtaining a metallic structure.

14. The method of claim 13, wherein: The metal structure is sintered.

15. The method according to claim 13 or 14, wherein: One or more of the compounds comprising metal atoms are compounds that are reducible to metal in a gas atmosphere; and wherein the metallic structure is obtained by reducing the dried structure by placing it in a reducing atmosphere.

16. The method of claim 15, wherein: The reduction is carried out in an atmosphere of an inert gas containing 0.5-100 vol % of H 2 .

17. The method according to any one of claims 13 to 16, wherein: One or more of the compounds comprising metal atoms is an interstitial metal hydride; and the dried structure is subjected to a temperature such that hydrogen is released in the form of hydrogen gas, resulting in a metallic structure.

18. The method according to any one of claims 13 to 17, wherein: The processing step to obtain the metal structure and the sintering step are performed in one processing step.

19. The method according to any one of claims 13 to 18, wherein: The three-dimensional structure is formed by additive manufacturing, for example, by three-dimensional printing.

20. The method of any one of claims 13 to 19, wherein: The surface of the metal structure is made hydrophobic or lipophilic.

21. The method of any one of claims 13 to 20, wherein: After the reduction step, the metal structure is at least partially oxidized.

22. A material produced by the method of any one of claims 13 to 21.

23. Use of the material of claim 22 as a resistive heating element.

24. Use of the material of claim 22 as a cooling element.

25. Use of the material according to claim 22 for absorbing lipophilic substances floating on water.

26. Use of the material according to claim 22 as a heterogeneous catalyst or as a support structure for a heterogeneous catalyst.

27. Use of the material according to claim 22 as an electrode.

28. Use of the material of claim 22 as a component in alkaline electrolysis.

29. Use of the material according to claim 22 as a gas storage material, in particular as a storage material for molecular hydrogen.