Surface-treated copper foil, and copper-clad laminate and printed wiring board using same

By forming a combination of roughened, heat-resistant and chromate treatment layers on the surface of the copper foil, the problems of adhesion and insertion loss of low dielectric constant resin substrates at high temperatures are solved, and high adhesion and heat-resistant are achieved It is suitable for high-frequency signal transmission printing plate manufacturing.

CN119013437AActive Publication Date: 2024-11-22FUKUDA METAL FOIL & POWDER CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380031225.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-28
Filing Date
2023-08-08
Publication Date
2024-11-22
Estimated Expiration
2043-08-08

AI Technical Summary

Technical Problem

The prior art is difficult to provide sufficient adhesion and heat resistance to low dielectric constant resin substrates at high temperatures, while suppressing insertion losses in high-frequency signal transmission, especially at the molding temperature of 300°C or above. The surface of the copper foil is prone to oxidation and deformation, resulting in a decrease in adhesion and an increase in insertion loss.

Method used

Using a combination technology of forming a roughening treatment layer, a heat-resistant treatment layer and a chromate treatment layer on the surface of the copper foil, the roughening treatment layer consists of copper particles from 0.5 μm to 0.9 μm, and the heat-resistant treatment layer contains cobalt, molybdenum, and chromium. The gloss of the acid salt-treated layer is 60 to 80, and a silane coupling agent is added to the chromate treatment layer to form a surface-treated copper foil.

Benefits of technology

It is realized that high adhesion and heat resistance are maintained on a low dielectric constant resin substrate above 300°C, and insertion loss is significantly suppressed, which is suitable for the manufacturing of printed wiring boards for high-frequency signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013437A_ABST
    Figure CN119013437A_ABST
Patent Text Reader

Abstract

Provided is a surface-treated copper foil which has an excellent anchoring effect on an insulating resin base material, can maintain high adhesion even with respect to a low dielectric constant resin base material having a high molding temperature, can achieve high heat resistance, can suppress insertion loss to a low level, and can be used as a surface-treated copper foil. Therefore, the resin composition can be applied to the production of a printed wiring board for high-frequency signal transmission using a low-dielectric-constant resin base material having a molding temperature of 300 DEG C or higher. A surface-treated copper foil which is provided with a roughened layer on at least one surface of an untreated copper foil, a heat-resistant layer on the roughened layer, and a chromate-treated layer on the heat-resistant layer, and wherein: the roughened layer is formed of copper particles having a primary particle diameter of 0.5-0.9 [mu] m; the heat-resistant treatment layer contains cobalt and molybdenum, and the glossiness (Gs (85 DEG)) of the treated surface of the chromate-treated layer is 60-80 (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a surface-treated copper foil. Specifically, the surface-treated copper foil relates to a surface-treated copper foil as follows: since a roughening treatment layer is formed by copper particles having a primary particle size of 0.5 μm to 0.9 μm, the anchoring effect to an insulating resin substrate is excellent, and since a heat-resistant treatment layer containing cobalt and molybdenum is formed on the roughening treatment layer, and a chromate treatment layer containing chromium is formed on the heat-resistant treatment layer, the surface of the roughening treatment layer is not easily oxidized, and the copper particles are not easily deformed, so that high adhesion can be maintained even for a low dielectric constant resin substrate having a high molding temperature, and high heat resistance can be achieved, and since the glossiness Gs (85°) of the treated surface of the chromate treatment layer is 60 to 80 and copper particles are sparsely formed, the insertion loss can be suppressed to a very low level, and therefore, the surface can be applied to the manufacture of a printed wiring board for high-frequency signal transmission using a low dielectric constant resin substrate having a molding temperature of 300° C. or more. Background Art

[0002] In Japan, the fifth-generation mobile communication system (5G) service started in March 2020. Although it is limited to limited places in cities, high-speed communication can now be used.

[0003] In addition, cars equipped with advanced driver assistance systems (ADAS) have expanded to light vehicles in addition to luxury cars. For example, when driving at a constant speed on a highway using a constant speed control device, the system detects the approach of the vehicle in front and automatically controls the distance between vehicles. Or it detects the sudden appearance of pedestrians, bicycles, etc. in urban areas and automatically activates the braking device. This is becoming popular, helping to reduce the burden on drivers and prevent traffic accidents.

[0004] Currently, 5G mostly uses a frequency band called Sub6, which is between 3.6 GHz and less than 6 GHz, but it is expected that the use of high-frequency bands called millimeter waves, which are above 28 GHz, will increase in the future.

[0005] In addition, the number of cars equipped with ADAS is expected to increase in the future. As the demand for millimeter-wave radars in the 24 GHz to 79 GHz frequency band, which is one of the sensors supporting ADAS, increases, the demand for millimeter-wave radars with higher performance is also increasing.

[0006] For communication systems using these high frequency bands, it is required not only to transmit signals at high speed but also to transmit them with low loss.

[0007] Whether or not a signal can be transmitted with low loss is greatly affected by the physical properties of an insulating resin substrate or copper foil constituting a printed wiring board, an antenna, or the like, namely, dielectric properties or conductor resistance.

[0008] Typically, insertion loss is the sum of dielectric loss and conductor loss.

[0009] Dielectric loss is mainly caused by the insulating resin base material. Because it is affected by the dielectric properties, the insertion loss tends to increase as the dielectric constant or dielectric loss tangent value increases. This tendency is more significant at high frequencies.

[0010] Conductor loss is mainly caused by copper foil, and is affected not only by the surface roughness of the copper foil but also by the type of dissimilar metal or the amount of attached metal. Therefore, if the surface roughness is large or magnetic metal is used, the insertion loss tends to increase, and this tendency becomes more significant at high frequencies.

[0011] Therefore, in order to transmit signals with a frequency of about 30 GHz or above, which is called millimeter waves, with low loss, the insulating resin substrate is preferably a material with excellent dielectric properties, and a low dielectric constant resin substrate composed of a liquid crystal polymer resin or a fluororesin with a small dielectric constant and dielectric loss tangent is particularly desirable.

[0012] In addition, copper foil with smaller surface roughness and less magnetic metal adhesion is preferred, and many copper foils with fine roughening treatment or copper foils with significantly reduced amounts of different metal treatment have been proposed.

[0013] When using liquid crystal polymer or fluorine-containing resin substrate to make copper-clad laminates, it is necessary to heat to a high temperature of 300°C or above for molding. However, it is impossible to adhere fine roughened copper foil or heterogeneous metal with a primary particle size below submicron level, or there are problems with the following treated copper foil with very small adhesion amount: the surface of the roughened layer is easily oxidized at high temperature, and the shape of the roughened particles is easily changed, and the physical anchoring effect is weak and cannot ensure sufficient adhesion.

[0014] In addition, even if the adhesion is high under normal conditions, there is a problem that significant deterioration occurs when a long-term heat resistance test is performed.

[0015] Even when molding is performed at a high temperature of 300° C. or higher, if one wishes to suppress oxidation of the surface of the roughened layer or deformation of the roughened particles to ensure sufficient adhesion, it is necessary to increase the amount of the dissimilar metal treatment or to increase the size of the roughened particles.

[0016] However, if the amount of dissimilar metal processed is increased or the size of the roughened particles is increased, there is a problem that the insertion loss increases.

[0017] Therefore, it is hoped to develop a surface-treated copper foil that has sufficient adhesion and heat resistance to a low dielectric constant resin substrate with a molding temperature of 300°C or above, thereby being able to suppress insertion loss during high-frequency signal transmission, and the surface-treated copper foil can be used in a printed wiring board for high-frequency signal transmission using a low dielectric constant resin substrate.

[0018] Prior art literature

[0019] Patent Literature

[0020] Patent document 1: Japanese Patent Application Laid-Open No. 2015-147978.

[0021] Patent document 2: Japanese Patent Application Laid-Open No. 2021-098892. Summary of the invention

[0022] Problems to be solved by the invention

[0023] Patent document 1 describes a surface-treated copper foil, characterized in that, within a range of 30 μm in width direction of the surface-treated copper foil cut in the width direction, there are at least 1 and less than 5 roughened particles with a roughening height of 1.5 μm or more, and there are at least 10 roughened particles with a roughening height of 1.0 μm or less. It is recorded that the surface-treated copper foil can also obtain high adhesion to a low dielectric constant resin substrate with a molding temperature of 300°C or more, and as a copper foil for high-frequency circuits, it also has excellent transmission characteristics.

[0024] However, even if the roughening height is 1.0 μm or less, there is a problem that the insertion loss increases if the number of roughening particles is large.

[0025] Patent document 2 describes a surface-treated copper foil, characterized in that it includes a surface-treated layer formed on at least one side of an untreated copper foil and an anti-oxidation layer formed on the surface-treated layer, wherein the surface-treated layer contains copper particles with an average particle size of about 10 nm to 100 nm, a ten-point average roughness Rz of about 0.2 μm to 0.5 μm, a glossiness Gs (60°) of about 200 or more, and the anti-oxidation layer contains nickel and phosphorus. It is recorded that the surface-treated copper foil has excellent bonding strength with an insulating resin substrate, low insertion loss, and is excellent as a high-frequency foil.

[0026] However, for low dielectric constant resin substrates formed at a molding temperature of 300° C. or higher, copper particles are easily deformed at high temperatures during molding, thereby reducing adhesion to the resin substrate. Furthermore, there is a problem that adhesion is reduced when the particles are exposed to high temperatures for a long time after molding.

[0027] The present inventors set the solution of the above-mentioned problems as a technical task, repeatedly carried out a large number of trials and evaluations, and as a result, a surface-treated copper foil was formed as follows: at least one side of an untreated copper foil is provided with a roughening treatment layer, a heat-resistant treatment layer is provided on the roughening treatment layer, and a chromate treatment layer is provided on the heat-resistant treatment layer, the roughening treatment layer is formed of copper particles having a primary particle size of 0.5 μm or more and 0.9 μm or less, the heat-resistant treatment layer is a heat-resistant treatment layer containing cobalt and molybdenum, and the surface-treated copper foil has a glossiness Gs (85°) of 60 or more and 80 or less, and exhibits high adhesion even to a low dielectric constant resin substrate having a molding temperature of 300°C or more, and can maintain high adhesion without any practical problems even when exposed to high temperature for a long time, and can achieve the above-mentioned technical task by utilizing the low conductor loss based on the excellent transmission characteristics of the low dielectric constant resin substrate.

[0028] Technical solutions to solve problems

[0029] The above technical problems are as follows, and can be solved by the present invention.

[0030] The present invention is a surface-treated copper foil, comprising a roughening treatment layer on at least one side of an untreated copper foil, a heat-resistant treatment layer on the roughening treatment layer, and a chromate treatment layer on the heat-resistant treatment layer, wherein the roughening treatment layer is formed by copper particles having a primary particle size of 0.5 μm or more and 0.9 μm or less, the heat-resistant treatment layer is a heat-resistant treatment layer containing cobalt and molybdenum, and the glossiness Gs (85°) of the treated surface of the chromate treatment layer is 60 or more and 80 or less.

[0031] Furthermore, the present invention provides the surface-treated copper foil in which the arithmetic mean height Sa of each treated surface of the roughening treated layer, the heat-resistant treated layer, and the chromate treated layer is 0.08 μm or more and 0.16 μm or less.

[0032] Moreover, the present invention provides the surface-treated copper foil including a silane coupling agent-treated layer on the chromate-treated layer.

[0033] Furthermore, the present invention provides a copper-clad laminate in which the surface-treated copper foil is bonded to an insulating resin substrate.

[0034] In addition, the present invention is the copper-clad laminate in which the insulating resin substrate is a low dielectric constant resin substrate.

[0035] Furthermore, the present invention provides a printed wiring board using the copper-clad laminate.

[0036] Effects of the Invention

[0037] Since the roughening treatment layer on the surface-treated copper foil of the present invention is formed of relatively large copper particles having a primary particle size of 0.5 μm to 0.9 μm, the surface-treated copper foil has an excellent anchoring effect on the insulating resin substrate.

[0038] In addition, since the heat-resistant treatment layer contains cobalt and molybdenum, and the chromate treatment layer contains chromium, the surface of the roughened treatment layer is not easily oxidized even at high temperatures, and the copper particles are not easily deformed. Therefore, it is a surface-treated copper foil that can maintain high adhesion and excellent heat resistance even for a low dielectric constant resin substrate with a molding temperature of more than 300°C.

[0039] Furthermore, since the glossiness Gs (85°) of the treated surface of the chromate treatment layer is a relatively high value of 60 to 80 and the copper particles are sparsely formed, the surface-treated copper foil can suppress the insertion loss to a low level.

[0040] Furthermore, when the arithmetic mean height Sa of each treated surface of the roughened layer, the heat-resistant treated layer, and the chromate treated layer is 0.08 μm to 0.16 μm, the surface-treated copper foil can further suppress the insertion loss.

[0041] Furthermore, when a silane coupling agent treatment layer is provided on the chromate treatment layer, a surface-treated copper foil having further excellent adhesion and heat resistance can be obtained.

[0042] Therefore, the surface-treated copper foil of the present invention can be suitably used in the production of a printed wiring board for high-frequency signal transmission using a low dielectric constant resin base material having a molding temperature of 300° C. or higher. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a schematic diagram of the surface-treated copper foil of the present invention.

[0044] Figure 2 This is a scanning electron microscope photograph (10,000 times) of the surface-treated copper foil (Example 1) of the present invention. DETAILED DESCRIPTION

[0045] The present invention is a surface-treated copper foil, comprising a roughening treatment layer on at least one side of an untreated copper foil, a heat-resistant treatment layer on the roughening treatment layer, and a chromate treatment layer on the heat-resistant treatment layer.

[0046] <Untreated copper foil>

[0047] The copper foil before surface treatment (hereinafter referred to as "untreated copper foil") of the present invention is not particularly limited, and any copper foil with no distinction between the front and back sides, such as rolled copper foil or electrolytic copper foil, or copper foil with distinction between the front and back sides can be used.

[0048] The surface to be surface treated is not particularly limited, and any surface of a rolled copper foil may be used, and any surface of an electrolytic copper foil may be used, i.e., the deposited surface or the drum surface.

[0049] The surface subjected to the surface treatment preferably has a glossiness Gs (60°) of 500 or more when the 60-degree specular gloss is measured in accordance with JIS Z8471.

[0050] When a rolled copper foil is used, it is preferred to immerse the foil in a hydrocarbon-based organic solvent or an alkaline degreasing liquid and perform a surface treatment after removing the rolling oil.

[0051] When an electrolytic copper foil is used, it is preferred to immerse it in dilute sulfuric acid and perform surface treatment after removing the oxide film.

[0052] The thickness of the untreated copper foil is not particularly limited as long as it is a thickness that can be used for a printed wiring board after surface treatment, but is preferably 6 μm to 300 μm, and more preferably 12 μm to 35 μm.

[0053] <Roughening treatment layer>

[0054] The surface-treated copper foil of the present invention includes a roughening-treated layer having copper particles as roughening particles on an untreated copper foil.

[0055] The primary particle size of the copper particles is preferably 0.5 μm to 0.9 μm, more preferably 0.6 μm to 0.8 μm.

[0056] In the present invention, the lower limit of the primary particle size is set to 0.5 μm, but the inclusion of copper particles of 0.5 μm or less is not excluded.

[0057] However, when the primary particle size is mostly less than 0.5 μm, the surface of the roughened layer may be oxidized or the copper particles may be deformed during bonding with a low dielectric constant resin substrate at a molding temperature of 300° C. or above, thereby reducing the anchoring effect on the low dielectric constant resin substrate and possibly significantly reducing the adhesion or heat resistance.

[0058] In addition, when there are many primary particle diameters exceeding 0.9 μm, the surface roughness increases, and there is a possibility that the conductor loss increases.

[0059] The primary particle size can be determined by selecting 10 copper particles observed with a scanning electron microscope at an inclination angle of 0° and a magnification of 10,000 times, measuring the maximum length of each copper particle, and averaging the measured values.

[0060] The roughening treatment layer in the present invention can be formed by forming a copper particle layer on an untreated copper foil and then electroplating the copper particle layer.

[0061] The copper particle layer can be formed by using an aqueous solution at a temperature of 40°C containing 20 g / L to 110 g / L of copper sulfate pentahydrate, 45 g / L to 150 g / L of sulfuric acid, 4 mg / L to 60 mg / L of tungsten ions, and 225 mg / L to 1200 mg / L of titanium ions as an electrolyte, immersing an insoluble electrode of titanium coated with a platinum group oxide as an anode in the electrolyte, and immersing an untreated copper foil as a cathode on the opposite side at a certain interval, and conducting the electrolytic reaction at a current density of 10 A / dm 2 ~40A / dm 2 , power 20C / dm 2 ~100C / dm 2 Perform electrolysis.

[0062] For copper plating, an aqueous solution containing 150 g / L to 300 g / L of copper sulfate pentahydrate and 50 g / L to 400 g / L of sulfuric acid at a temperature of 40°C is used as an electrolyte, an insoluble electrode of titanium coated with a platinum group oxide is immersed in the electrolyte as an anode, and a copper foil provided with a copper particle layer is immersed as a cathode on the opposite side at a certain interval, and a current density of 2 A / dm is applied. 2 ~10A / dm 2 , power 60C / dm 2 ~240C / dm 2 Just carry out electrolysis.

[0063] <Heat-resistant treatment layer and chromate treatment layer>

[0064] The present invention is a surface-treated copper foil including a heat-resistant treatment layer containing cobalt and molybdenum on a roughening treatment layer, and a chromate treatment layer containing chromium on the heat-resistant treatment layer.

[0065] This is because if a heat-resistant treatment layer or a chromate treatment layer is not formed, after being bonded to a low dielectric constant resin substrate to form a copper-clad laminate, if it is exposed to a high temperature of 150°C or above, the adhesion to the low dielectric constant resin substrate may be significantly reduced.

[0066] The heat-resistant treated layer can be formed by electrolyzing the copper foil having the roughened treated layer formed on the untreated copper foil while immersing the copper foil in an electrolytic solution.

[0067] The electrolyte for forming the heat-resistant treatment layer is preferably an electrolyte prepared by adjusting an aqueous solution containing 20 g / L to 70 g / L of a cobalt-containing compound, 10 g / L to 50 g / L of a molybdenum-containing compound, and 10 g / L to 100 g / L of sodium citrate dihydrate to pH 4 to pH 10.

[0068] For electrolysis, it is preferred to immerse an insoluble electrode such as a platinum group oxide-coated titanium as an anode in an electrolyte solution, and immerse a copper foil having a roughened layer as a cathode at a predetermined interval on the opposite side, and conduct the electrolysis at a current density of 3 A / dm 2 ~14A / dm 2 , power 7C / dm 2 ~30C / dm 2 , the electrolysis is carried out under the conditions of liquid temperature of 25℃~45℃.

[0069] The cobalt-containing compound is not particularly limited, and examples thereof include cobalt sulfate heptahydrate and cobalt dichloride hexahydrate.

[0070] The molybdenum-containing compound is not particularly limited, but sodium molybdate dihydrate is exemplified.

[0071] The chromate treatment layer can be formed by electrolyzing the copper foil having the heat-resistant treatment layer formed thereon while immersing the copper foil in an electrolytic solution.

[0072] Regarding the electrolyte for forming the chromate treatment layer, it is preferred that an aqueous solution containing 10 g / L to 60 g / L of a chromium-containing compound, or an aqueous solution containing 10 g / L to 60 g / L of a chromium-containing compound and 0.2 g / L to 4.0 g / L of zinc ions be modulated to a pH of 2 to pH 12 using sulfuric acid or sodium hydroxide.

[0073] For electrolysis, it is preferred that an insoluble electrode such as titanium coated with a platinum group oxide is immersed in the electrolyte as an anode, and a copper foil having a heat-resistant treatment layer is immersed in the opposite side as a cathode at a certain interval, and the current density is 0.5 A / dm 2 ~5A / dm 2 , power 1C / dm 2 ~6C / dm 2 , the electrolysis is carried out under the conditions of liquid temperature of 25℃~50℃.

[0074] The chromium-containing compound is not particularly limited, but sodium dichromate is exemplified.

[0075] The zinc ion source is not particularly limited, but zinc oxide is exemplified.

[0076] <Glossiness>

[0077] The present invention is a surface treated copper foil having a glossiness Gs (85°) of 60 to 80 on the treated surface of the chromate treatment layer.

[0078] This is because if the glossiness is less than 60, the number of copper particles becomes too large, resulting in increased conductor loss, while if it exceeds 80, the number of copper particles becomes too small, resulting in insufficient adhesion and heat resistance to the low dielectric constant resin substrate.

[0079] Gs (85°) can be measured based on JIS Z8741 as 85-degree specular gloss.

[0080] <Surface roughness>

[0081] The arithmetic mean height Sa of each treated surface of the roughening treated layer, the heat resistant treated layer, and the chromate treated layer of the surface treated copper foil of the present invention is preferably 0.08 μm to 0.16 μm, more preferably 0.09 μm to 0.15 μm.

[0082] This is because if the arithmetic mean height Sa is less than 0.08 μm, there is a possibility that the adhesion to the low dielectric constant resin substrate or heat resistance is insufficient, and if it exceeds 0.16 μm, the conductor loss is likely to increase.

[0083] <Silane coupling agent treatment layer>

[0084] The surface-treated copper foil of the present invention may include a silane coupling agent treatment layer on the chromate treatment layer.

[0085] By forming a silane coupling agent treatment layer on the chromate treatment layer, a surface-treated copper foil having further excellent adhesion and heat resistance can be obtained.

[0086] The silane coupling agent treatment layer can be formed by immersing the copper foil having the chromate treatment layer in an aqueous solution of a silane coupling agent adjusted to a temperature of 20° C. to 50° C. or by applying the silane coupling agent by spraying or the like and then washing with water.

[0087] The silane coupling agent used for the silane coupling agent layer is not particularly limited, and silane coupling agents containing vinyl, epoxy, styryl, methacryloyl, acryl, amino, urea and mercapto groups can be used. However, silane coupling agents containing amino, epoxy or vinyl groups have excellent effects on moisture absorption resistance and rust resistance, so they are more suitable for use.

[0088] The silane coupling agent may be used alone or in combination of two or more.

[0089] Examples of the composition and conditions of the aqueous solution for forming the silane coupling agent treatment layer include 1 mL / L to 5 mL / L of γ-aminopropyltriethoxysilane, a liquid temperature of 25° C. to 35° C., and an immersion time of 15 seconds.

[0090] <Insulating resin base material>

[0091] The insulating resin substrate used in the copper-clad laminate of the present invention is not particularly limited, and examples thereof include epoxy resin substrates and polyimide resin substrates. In addition, examples of low dielectric constant resin substrates include polyphenylene ether resin substrates, bismaleimide triazine resin substrates, and cycloolefin polymer resin substrates.

[0092] Furthermore, the surface-treated copper foil of the present invention can also be applied to a low dielectric constant resin substrate having a molding temperature of 300° C. or higher.

[0093] Examples of the low dielectric constant resin substrate having a molding temperature of 300° C. or higher include a liquid crystal polymer resin substrate and a fluorine-containing resin substrate.

[0094] Example

[0095] Examples of the present invention are shown below, but the present invention is not limited thereto.

[0096] <Untreated copper foil>

[0097] As the untreated copper foil of the examples and comparative examples, an electrolytic copper foil having a nominal thickness of 18 μm and a glossiness Gs (60°) of 500 or more was used.

[0098] The electrolytic copper foil is immersed in dilute sulfuric acid to remove the oxide film and then subjected to various treatments.

[0099] (Example 1)

[0100] <Formation of Roughening Layer>

[0101] As an electrolyte, an aqueous solution containing 47 g / L of copper sulfate pentahydrate, 95 g / L of sulfuric acid, 15 mg / L of tungsten ions, and 500 mg / L of titanium ions at a temperature of 40°C was used, and an insoluble electrode of titanium coated with platinum group oxide was immersed as an anode in the electrolyte. In addition, an untreated copper foil was immersed as a cathode on the opposite side at a certain interval, and the current density was 25 A / dm 2 , power 50C / dm 2 Electrolysis was performed to form a copper particle layer on the untreated copper foil. The formed copper particle layer was in a dendritic shape.

[0102] As an electrolyte, an aqueous solution containing 220 g / L of copper sulfate pentahydrate and 110 g / L of sulfuric acid at a temperature of 40°C was used, and an insoluble electrode of titanium coated with platinum oxide was immersed as an anode in the electrolyte. In addition, a copper foil provided with a copper particle layer was immersed as a cathode on the opposite side at a certain interval, and the current density was 10 A / dm 2 , power 120C / dm 2 Electrolysis is performed to form a roughening treatment layer by copper plating on the copper particle layer.

[0103] <Formation of heat-resistant treatment layer>

[0104] As the electrolyte solution, an aqueous solution containing 39 g / L of cobalt sulfate heptahydrate, 24 g / L of sodium molybdate dihydrate, and 45 g / L of sodium citrate dihydrate adjusted to pH 5.6 was used.

[0105] For electrolysis, an insoluble electrode of titanium coated with platinum group oxide was immersed in the electrolyte as an anode, and a copper foil with a roughened layer was immersed in the opposite side as a cathode at a certain interval, and the current density was 7A / dm 2 , power 14C / dm 2 , the electrolysis is carried out under the conditions of liquid temperature of 30°C to form a heat-resistant treatment layer.

[0106] <Chromate treatment layer>

[0107] As the electrolytic solution, an aqueous solution containing 12.5 g / L of sodium dichromate and 2.5 g / L of zinc ions was prepared to pH 12 and used.

[0108] For electrolysis, an insoluble electrode of titanium coated with platinum group oxide was immersed in the electrolyte as the anode, and a copper foil with a heat-resistant treatment layer was immersed in the opposite side as the cathode at a certain interval. 2 , power 10C / dm 2 , the electrolysis is carried out under the conditions of a liquid temperature of 25°C to provide a chromate treatment layer.

[0109] <Silane coupling agent treatment layer>

[0110] The copper foil having the chromate treatment layer is immersed in an aqueous solution containing 5 ml / L of γ-aminopropyltriethoxysilane at a liquid temperature of 25° C. for 10 seconds, and then pulled out and dried to form a silane coupling agent treatment layer, thereby obtaining a surface-treated copper foil ( Figure 2 ).

[0111] (Example 2)

[0112] In addition to the electrolysis conditions for forming the first stage copper particle layer, the current density was set to 22 A / dm 2 , power 55C / dm 2 The conditions for forming the roughening layer were the same as those in Example 1 except for the above.

[0113] (Example 3)

[0114] In addition to the electrolysis conditions for forming the first stage copper particle layer, the current density was set to 23A / dm 2 , power 52C / dm 2 The roughening treatment layer was formed under the same conditions as in Example 1 except that the silane coupling agent treatment layer was not provided.

[0115] (Comparative Example 1)

[0116] In addition to the electrolysis conditions for forming the first stage copper particle layer, the current density was set to 16A / dm 2 , power 40C / dm2 The conditions for forming the roughening layer were the same as those in Example 1 except for the above.

[0117] (Comparative Example 2)

[0118] In addition to the electrolysis conditions for forming the first stage copper particle layer, the current density was set to 24A / dm 2 , power 60C / dm 2 The conditions for forming the roughening layer were the same as those in Example 1 except for the above.

[0119] (Comparative Example 3)

[0120] As the electrolyte for forming the first-stage copper particle layer, an aqueous solution containing 57 g / L of copper sulfate pentahydrate, 100 g / L of sulfuric acid, 15 mg / L of tungsten ions, and 35 mg / L of chloride ions at a temperature of 40°C was used, and the electrolysis conditions were set to a current density of 50 A / dm 2 , power 125C / dm 2 In addition, the electrolytic conditions for copper plating on the copper particle layer in the second stage are set to a current density of 5A / dm 2 、Power 440C / dm 2 , except for this, the formation conditions of the roughening treatment layer were prepared under the same conditions as in Example 1.

[0121] (Comparative Example 4)

[0122] As the electrolyte for forming the first-stage copper particle layer, an aqueous solution containing 100 g / L of copper sulfate pentahydrate, 100 g / L of sulfuric acid, 150 mg / L of indium sulfate, and 5 g / L of starch decomposition product at a temperature of 40°C was used, and the electrolysis conditions were set to a current density of 50 A / dm 2 , power 130C / dm 2 , and the formation conditions of the roughening treatment layer were prepared under the same conditions as in Example 1 except that the copper plating treatment was not performed.

[0123] (Comparative Example 5)

[0124] The electrolysis conditions for forming the first-stage copper particle layer were set to a current density of 22 A / dm 2 , power 55C / dm 2 , and the conditions for forming the roughening treatment layer were prepared under the same conditions as in Example 1, except that the heat-resistant treatment layer was not formed.

[0125] (Comparative Example 6)

[0126] The electrolysis conditions for forming the first-stage copper particle layer were set to a current density of 22 A / dm 2 , power 55C / dm 2The conditions for forming the heat-resistant treatment layer are as follows: an electrolyte solution containing 30 g / L of nickel sulfate hexahydrate, 2 g / L of sodium phosphate monohydrate, and 10 g / L of sodium acetate trihydrate is used as the electrolyte solution, and the electrolysis conditions are set to a current density of 5 A / dm 2 , power 10C / dm 2 , the roughening layer formation conditions were prepared under the same conditions as in Example 1 except that the liquid temperature was 30°C.

[0127] (Comparative Example 7)

[0128] The electrolysis conditions for forming the first-stage copper particle layer were set to a current density of 23 A / dm 2 , power 52C / dm 2 , and the roughening treatment layer is not provided. Except for this, the formation conditions of the roughening treatment layer are prepared under the same conditions as in Example 1.

[0129] (Comparative Example 8)

[0130] The electrolysis conditions for forming the first-stage copper particle layer were set to a current density of 23 A / dm 2 , power 52C / dm 2 , and there is no chromate treatment layer and silane coupling agent treatment layer. Except for this, the formation conditions of the roughening treatment layer are prepared under the same conditions as in Example 1.

[0131] The treatment conditions of each surface-treated copper foil of Examples and Comparative Examples are shown in [Table 1].

[0132] [Table 1]

[0133]

[0134] <Manufacturing of copper-clad laminate A>

[0135] The treated surface of each surface-treated copper foil of the embodiment and the comparative example is used as the bonding surface, and is laminated to one or both sides of a fluorine-containing resin substrate (manufactured by Rogers Corporation / RO3003 / nominal thickness 100 μm), and a vacuum hot press (manufactured by Kitagawa Seiki Co., Ltd. / KVHC-II) is used to heat and pressurize the substrate under vacuum at a temperature of 370°C and a surface pressure of 3 MPa for 45 minutes to obtain a copper-clad laminate A.

[0136] <Production of copper-clad laminate B>

[0137] The treated surface of each surface-treated copper foil of the embodiment and the comparative example is used as the bonding surface, and is laminated to one or both sides of a liquid crystal polymer resin substrate (CTQ-50 manufactured by KURARAY Co., Ltd. / nominal thickness 50 μm), and a vacuum hot press (KVHC-II manufactured by Kitagawa Seiki Co., Ltd.) is used to heat and press mold for 10 minutes at a temperature of 300°C and a surface pressure of 4 MPa under vacuum to obtain a copper-clad laminate B.

[0138] The surface-treated copper foil was evaluated by the following method.

[0139] <Measurement of primary particle size>

[0140] The surface on which the roughening layer was formed was observed using a scanning electron microscope SEM (JSM-6010LA manufactured by JEOL Ltd.) at an inclination angle of 0° and a magnification of 10,000 times. The maximum length of each of 10 copper particles was measured from the obtained SEM image and the average was used to obtain the primary particle size.

[0141] <Measurement of glossiness>

[0142] The glossiness of the treated surface was determined by measuring 85-degree specular gloss (Gs (85°)) in accordance with JIS Z8741 using a gloss meter (GM-268A manufactured by Konica Minolta, Inc.).

[0143] <Measurement of surface roughness>

[0144] Using a confocal microscope, i.e. a laser microscope (LEXT OLS5000 manufactured by OLYMPUS CORPORATION) in accordance with ISO25178-607, the arithmetic mean height Sa was measured in accordance with JPCA-KHS01 (2021) when the evaluation area was set to 125 μm × 125 μm, the S filter was set to 0.5 μm, the L filter was set to 50 μm, and the F operation was set to a multiple surface (3 times).

[0145] <Normal peel strength>

[0146] A copper circuit having a width of 10 mm was formed on the copper-clad laminate A produced above using an etching apparatus (manufactured by Ninomiya Co., Ltd. / SPE-40) to prepare a test piece.

[0147] The peel strength was measured using a universal testing machine in accordance with JIS C6481, and a value of 0.53 kN / m or more was evaluated as "0", and a value of less than 0.53 kN / m was evaluated as "×".

[0148] <Peel strength after heat treatment>

[0149] A test piece in which a circuit having a width of 10 mm was formed on the copper-clad laminate A produced above was subjected to a heat treatment at 177° C. for 5 days in an air atmosphere using a thermostat to obtain a test piece.

[0150] The peel strength after the heat treatment was measured using a universal testing machine in accordance with JIS C6481, and a value of 0.53 kN / m or more was evaluated as "0", and a value of less than 0.53 kN / m was evaluated as "×".

[0151] <Transmission characteristics>

[0152] A single-ended microstrip circuit was formed on the copper-clad laminate B obtained above using an etching apparatus (manufactured by Ninomiya Systems Co., Ltd. / SPE-40) to prepare a test piece.

[0153] Regarding the test piece, the circuit length was set to 100 mm, and the circuit width was set so that the characteristic impedance would be 50Ω.

[0154] The insertion loss (S21) of the test piece at a frequency of 20 GHz was measured using a network analyzer (manufactured by KEYSIGHT TECHNOLOGIES, INC. / E5071C), and a value of -4.4 dB / 100 mm or more was evaluated as "0", and a value of less than -4.4 dB / 100 mm was evaluated as "×".

[0155] <Overall Evaluation>

[0156] The normal peel strength, the peel strength after heat treatment, and the transmission characteristics were evaluated comprehensively, and the test in which any of the evaluations in the above tests was 0 was evaluated as "0", and the test in which one or more of the above tests was evaluated as × was evaluated as "×".

[0157] The results of adhesion, heat resistance, and transmission characteristics of each surface-treated copper foil of Examples and Comparative Examples are shown in [Table 2].

[0158] [Table 2]

[0159]

[0160] As shown in Examples 1 to 3, the surface-treated copper foil of the present invention has a peel strength of 0.53 kN / m or more in normal state and after heat treatment, which is a high value that is not a problem in practical use, and even at a high frequency of 20 GHz, the insertion loss S21 is -4.4 dB / 100 mm or more, which has good transmission characteristics.

[0161] Industrial Applicability

[0162] The surface-treated copper foil of the present invention is a surface-treated copper foil as follows: since the roughening treatment layer is formed by copper particles having a primary particle size of 0.5 μm to 0.9 μm, an excellent anchoring effect is exhibited on an insulating resin substrate. Furthermore, since a heat-resistant treatment layer containing cobalt and molybdenum is formed on the roughening treatment layer, and a chromate treatment layer containing chromium is formed on the heat-resistant treatment layer, the surface of the roughening treatment layer is not easily oxidized and the copper particles are not easily deformed. Therefore, high adhesion can be maintained and high heat resistance can be achieved even for a low dielectric constant resin substrate having a high molding temperature. Furthermore, since the glossiness Gs (85°) of the treated surface of the chromate treatment layer is 60 to 80 and the copper particles are sparsely formed, the insertion loss can be suppressed to a low level. Therefore, the surface of the surface-treated copper foil can be applied to the manufacture of a printed wiring board for high-frequency signal transmission using a low dielectric constant resin substrate having a molding temperature of 300° C. or above.

[0163] Therefore, the present invention has high industrial applicability.

Claims

1. A surface-treated copper foil, comprising a roughening treatment layer on at least one side of an untreated copper foil, a heat-resistant treatment layer on the roughening treatment layer, and a chromate treatment layer on the heat-resistant treatment layer, wherein: The roughening layer is formed of copper particles having a primary particle size of 0.5 μm or more and 0.9 μm or less, the heat-resistant layer is a heat-resistant layer containing cobalt and molybdenum, and the glossiness Gs (85°) of the treated surface of the chromate treatment layer is 60 or more and 80 or less.

2. The surface-treated copper foil according to claim 1, wherein The arithmetic mean height Sa of each treated surface of the roughened layer, the heat-resistant treated layer, and the chromate treated layer is greater than or equal to 0.08 μm and less than or equal to 0.16 μm.

3. The surface-treated copper foil according to claim 1 or 2, wherein A silane coupling agent treatment layer is provided on the chromate treatment layer.

4. A copper-clad laminate, wherein: The surface-treated copper foil according to claim 1 or 2 is laminated on an insulating resin substrate.

5. The copper-clad laminate according to claim 4, wherein: The insulating resin substrate is a low dielectric constant resin substrate.

6. A printed wiring board, wherein: The copper-clad laminate according to claim 4 is used.

Citation Information

Patent Citations

  • Copper foil for processing copper clad laminate, copper clad laminate and printed wiring board equipped with copper clad laminate

    CN102215635A

  • Treatment copper foil, copper-clad laminate using the treatment copper foil, and print circuit board

    CN106211567A

  • Treated copper foil for low dielectric resin substrate and copper-clad laminate and printed writing board using the same

    CN106413248A

  • Method of manufacturing printed wiring board

    CN107003257A

  • Copper foil for electromagnetic wave shield filter in plasma display, and its manufacturing method

    JP2006324546A