Alloy powder, method for preparing a component based on the alloy and component
Through powder injection molding and heat treatment technology of titanium-based alloy powder, turbine components with excellent mechanical properties and low density at high temperatures are prepared, which solves the problems of component quality and cost in the prior art, and realizes controllable size and high temperature resistance aerospace components.
Patent Information
- Application Number
- CN202380023053.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-22
- Filing Date
- 2023-02-20
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art is difficult to prepare complex turbine nozzles or turbine blade/vane components with high mechanical resistance and low density, especially at high temperature conditions, and conventional casting processes lead to material losses and additional costs.
The components were prepared by powder injection molding using titanium-based alloy powder with chemical compositions of 32.0% to 33.5% aluminum, 4.50% to 5.10% niobium, 2.40% to 2.70% chromium, and thermal isostatic compaction and quenching. The treatment was obtained to obtain parts with good resistance and small mass at 700°C.
It realizes components with good traction, fatigue, creep and oxidation resistance at high temperatures, with a mass smaller than nickel-based alloy, with controllable size and good surface condition, and is suitable for aviation components.
Smart Images

Figure CN118900735A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a titanium-based alloy powder, which is particularly intended to be used in a preparation method by injection molding of metal.
[0002] The invention also relates to such a production process using this powder, and to a component produced by this process, in particular for use in aviation. Background Art
[0003] In a turbojet engine, the exhaust gases generated in the combustion chamber can reach very high temperatures, exceeding 1200° C., or even 1600° C. Therefore, the turbojet engine components that come into contact with these exhaust gases, such as turbine blades / vanes, must be able to maintain their mechanical properties at these high temperatures.
[0004] For this purpose, it is known to make certain parts of turbojets from "superalloys". Superalloys, usually nickel-based, are a class of highly resistant metal alloys that can operate at temperatures relatively close to their melting point (usually 0.7 to 0.9 times their melting point). However, these alloys are very dense and their mass limits the efficiency of the turbine.
[0005] The intermetallic casting alloy TiAl 48-2-2 has been used to prepare certain turbine components. More specifically, components made of TiAl can operate at up to 700°C while maintaining good mechanical resistance to creep, fatigue and traction, as well as good resistance to corrosion and oxidation. In addition, the intermetallic alloy TiAl also has the advantage of being less dense than nickel-based high-temperature alloys.
[0006] However, conventional casting processes still have difficulty in obtaining TiAl parts with good dimensions, especially when it comes to complex parts such as turbine nozzles or turbine blades / vanes with internal passages or housing components. The method involves starting with TiAl rods, resulting in significant loss of material and therefore unnecessary additional costs.
[0007] Another technique known in the art is metal powder injection molding (known as metal injection molding or MIM). This method can be advantageously used to produce complex turbine components with the required dimensions.
[0008] Several materials are commercially available for the production of turbomachinery components by the MIM process.
[0009] For example, nickel-based Inconel 718 is often used, but the resulting parts cannot operate above 650° C., which is too low a temperature for use in combustion chambers or turbines. In addition, the mass of the material is relatively large.
[0010] Another available material is Hastelloy X, which can produce components that can operate at temperatures up to 950° C. However, its mechanical properties are limited and it can only be used for very lightly loaded components.
[0011] Finally, Rene 77 can be used to obtain components capable of operating at temperatures up to 1000 ° C while withstanding high levels of fatigue and creep. However, since this material is also a nickel-based alloy, the mass of the components obtained is also relatively large.
[0012] Therefore, it is necessary to solve the above problems. Summary of the invention
[0013] Therefore, one object of the present invention is to provide a solution that allows to obtain complex components with controlled dimensions, such as turbine nozzles or turbine blades / vanes with internal channels, which are made of an alloy material that has the same properties as cast TiAl, namely good resistance to traction, fatigue, creep and oxidation / corrosion up to 700°C, while having a much lower mass than nickel-based alloys and can be used for MIM forming methods.
[0014] Another object of the invention is to obtain a component for aeronautics having a good surface condition.
[0015] For this purpose, the present invention provides a titanium-based alloy powder, characterized in that the titanium-based alloy powder includes, by weight percentage, 32.0% to 33.5% aluminum, 4.50% to 5.10% niobium, 2.40% to 2.70% chromium, 0 to 0.1% iron, 0 to 0.025% silicon, 0 to 100 ppm carbon, 0 to 100 ppm nitrogen, 0 to 1000 ppm dioxygen, 0 to 50 ppm dihydrogen and 0 to 500 ppm unavoidable impurities, and the balance is titanium, and the titanium-based alloy powder has:
[0016] - D10 particle size between 3 and 10 μm,
[0017] - a D90 particle size between 20 and 40 μm, and
[0018] - a particle size D50 between 10 and 25 μm,
[0019] The values of D10, D50 and D90 particle sizes are measured by laser diffraction according to ISO 13322-2 standard.
[0020] The chemical composition and the particle size of the alloy powder are chosen so that it can be used in a powder injection molding process and so as to obtain, at the end of the process, an alloy part having good resistance to traction, fatigue and creep at temperatures up to 700° C. and good resistance to corrosion and oxidation, while the mass of the alloy powder is less than that of nickel-based alloys.
[0021] The invention also relates to a method for producing a component, in particular for aviation, characterized in that the method comprises the following steps:
[0022] - a step of mixing a titanium-based alloy powder according to the invention with at least one plastic binder,
[0023] - a step of granulating the mixture so as to obtain granules of a mixture of alloy and plastic,
[0024] - a step of injection molding the granules of the mixture in a mold to obtain a green part,
[0025] - a debonding step to obtain a debonded part,
[0026] - A step of sintering the debound component to obtain a sintered component.
[0027] This method makes it possible to obtain complex parts with controlled dimensions and good surface conditions starting from the above alloy powders.
[0028] This method also makes it possible to obtain components having good resistance to traction, fatigue and creep at temperatures up to 700° C. and good resistance to corrosion and oxidation, while having a mass less than components made of nickel-based alloys.
[0029] Other advantageous and non-limiting features according to the invention, used alone or in combination:
[0030] - The method further comprises a hot isostatic compaction step comprising a heat treatment at a pressure between 125 MPa and 150 MPa, at a temperature between 1175°C and 1195°C, preferably at 1185°C, for a duration between 1 hour and 5 hours, preferably 3 hours, this step being carried out after sintering the E6.
[0031] - The method further comprises a step of quenching the sintered part, which step comprises heat treating the sintered part at a temperature between 1140°C and 1160°C for 3 hours, the first two hours at a pressure between 125 MPa and 150 MPa and the last hour at a pressure between 100 MPa and 125 MPa, this step being carried out after the sintering step or the hot isostatic compaction step.
[0032] - the alloy and plastic mixture has a volumetric alloy loading of between 50% and 75% and a melt flow index of 60 cm at a temperature between 190° C. and 230° C. 3 / 10min to 85cm 3 / 10min, the injection temperature during the molding step is between 160°C and 200°C, and the melt flow index is measured according to standard ISO 1133-1.
[0033] - the diameter of the particles of the alloy and plastic mixture is between 1 mm and 5 mm,
[0034] - the debonding step itself comprises two consecutive steps: a first chemical step of preliminary debonding of the green part, in order to obtain a partially debonded part, and a second step of thermal debonding of the partially debonded part, in order to obtain a debonded part,
[0035] - a preliminary debonding step is a catalytic debonding for a duration between 2 hours and 10 hours under nitrogen in the presence of nitric acid fumes, the flow rate of the nitric acid fumes being between 2 mL / min and 5 mL / min and the temperature being between 100° C. and 150° C.,
[0036] - a preliminary debinding step is a debinding by solvent for a duration between 100 and 400 hours using demineralized water under stirring of said water, the temperature of the water being between 20° C. and 100° C.,
[0037] - the thermal debonding step is carried out in two consecutive temperature stages under argon, the first temperature stage being carried out between 250° C. and 450° C. for 100 minutes to 300 minutes, the second temperature stage being carried out between 350° C. and 550° C. for 100 minutes to 300 minutes,
[0038] The step of sintering the debonded component is carried out under an argon atmosphere by applying a temperature between 1400° C. and 1450° C. for a duration of between 2 hours and 6 hours.
[0039] Finally, the present invention relates to a titanium-based alloy component, which is particularly used in aviation, and is characterized in that the titanium-based alloy component is prepared by the above preparation method.
[0040] Other advantageous and non-limiting features according to the invention, used alone or in combination:
[0041] - The component comprises, by weight percentage, 32.0% to 33.5% aluminum, 4.50% to 5.10% niobium, 2.40% to 2.70% chromium, less than 0.1% iron, less than 2000 ppm dioxygen, less than 0.025% silicon, less than 350 ppm carbon, less than 200 ppm nitrogen, less than 100 ppm dihydrogen and less than 500 ppm unavoidable impurities, the balance being titanium, and the component also has a duplex to low duplex microstructure with multiphase lamellar grains between 10% and 60% and gamma grains between 90% and 40%.
[0042] - The component is a turbine blade / vane or a turbine nozzle. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Other features and advantages of the present invention will become apparent from the following detailed description with reference to the accompanying drawings, in which:
[0044] - Figure 1 Electron microscope images of a component made from cast TiAl 48-2-2 after a series of heat treatments are shown.
[0045] - Figure 2 The various steps of the preparation method according to the present invention are schematically shown.
[0046] - Figure 3 is an electron microscope image of a component obtained at the end of the sintering step of the preparation method according to the invention.
[0047] - Figure 4 is an electron microscope image of a part obtained at the end of the hot isostatic compaction (CIC) step and the quenching step of the production method according to the invention. DETAILED DESCRIPTION
[0048] The casting alloy TiAl 48-2-2 comprises, by weight percentage, 32.0% to 33.5% of aluminum, 4.50% to 5.10% of niobium, 2.40% to 2.70% of chromium, less than 0.1% of iron, less than 0.015% of carbon, less than 0.02% of nitrogen, less than 0.01% of hydrogen, 0.04% to 0.13% of dioxygen, less than 0.05% of other elements constituting unavoidable impurities, and the balance is composed of titanium, which is the basic component of the alloy.
[0049] Figure 1 Schematic diagram of the microstructure of cast TiAl 48-2-2 with a dual-phase microstructure obtained after a series of heat treatments, in which gray two-phase lamellar grains and white single-phase γ grains are visible. The term "dual-phase" means that the microstructure includes two types of phases.
[0050] The intermetallic alloy TiAl 48-2-2 has mechanical and chemical properties of interest for applications in the turbine field. TiAl 48-2-2 components maintain good mechanical resistance to creep, fatigue and traction up to 700°C as well as good resistance to corrosion and oxidation. In addition, the density of TiAl alloys is lower than that of nickel-based high-temperature alloys.
[0051] On the other hand, metal injection molding makes it possible to obtain parts with excellent surface conditions and complex shapes, and to precisely control the dimensions of said parts. Furthermore, metal injection molding is a method characterized by its rapid implementation.
[0052] The invention relates to an alloy powder and to a method, the parameters of which are selected so as to obtain from the alloy powder and at the end of the method a component which advantageously combines the properties of a TiAl 48-2-2 alloy component and the properties of a component from a metal injection molding method.
[0053] The MIM method is a method of molding a component by injecting a mixture of metal powder and a plastic binder into a mold. The strength of the injected component is ensured by the plastic binder. The plastic binder is removed in a subsequent step, known as the debonding step. The debonded component is brittle because it is very porous. An additional sintering step is required, in which the metal powder grains are bonded together.
[0054] Titanium-aluminum alloy powder for metal injection molding
[0055] The invention relates to a titanium-based metal alloy powder. The chemical composition and particle size of the alloy powder are selected so that it can be used in a metal injection molding (MIM) process and at the end of the process a titanium-based alloy component is obtained whose chemical composition is close to that of the casting alloy TiAl 48-2-2 and whose mechanical properties are improved.
[0056] Chemical composition of powder
[0057] Even if the plastic binder is almost completely removed in the above-mentioned debinding step, residues of the plastic binder can impregnate the metal material.The contents of nitrogen, dioxygen and carbon are greater in the molded part from the powder injection molding process than in the powder injected at the beginning of the process.
[0058] However, the carbon, nitrogen and dioxygen contents given in the specification of TiAl 48-2-2 are relatively low in relation to the expected mechanical properties. For example, a high carbon content leads to the formation of carbides at the grain boundaries, which hinder the growth and movement of the grains. As a result, the ductility of the component is low and there is a risk of fracture during use. High contents of dioxygen and nitrogen also lead to reduced ductility of the component and rapid fracture under fatigue and traction.
[0059] The contents of the various elements of the alloy powder of the present invention are therefore selected, particularly the contents of nitrogen, oxygen and carbon.
[0060] The alloy powder according to the present invention comprises, by weight percentage, 32.0% to 33.5% of aluminum, 4.50% to 5.10% of niobium, 2.40% to 2.70% of chromium, 0 to 0.1% of iron, 0 to 0.025% of silicon, 0 to 100 ppm of carbon, 0 to 100 ppm of nitrogen, 0 to 1000 ppm of dioxygen, 0 to 50 ppm of dihydrogen and 0 to 500 ppm of unavoidable impurities, with the balance being titanium.
[0061] "Unavoidable impurities" are defined as elements that are inadvertently added to the composition of the powder and are contributed by other elements. For example, these unavoidable impurities may include yttrium from the crucible used for atomization of the powder.
[0062] Powder particle size
[0063] The particle size of the powder is chosen so that the powder can be used in the production process described below, in particular during the injection and sintering steps.
[0064] The implementation of the powder injection molding process requires control of the size of the powder grains to ensure good injection of the mixture of alloy powder and plastic binder into the mold of the component. More specifically, small-sized alloy powder grains result in a large contact interface between the alloy powder and the plastic binder in the mixture of alloy powder and plastic binder, and therefore a high level of friction when the mixture is injected into the mold of the component. Conversely, too large alloy powder grains are more difficult to transport through the plastic binder during the injection, and thus an uneven injected component is obtained.
[0065] Furthermore, particle size is important in order to obtain good sintering (a step during which the grains will diffuse and bond to each other, removing their interfaces and therefore reducing their entropy). Thus, fine powders are easier to sinter because, by grouping together, the small powder grains strongly reduce their interfaces and surfaces, causing their entropy to decrease significantly.
[0066] Therefore, the size of the alloy powder grains of the present invention has been defined by the range of acceptable values for the D10, D50 and D90 particle sizes of the alloy powder.
[0067] The D10 particle size corresponds to a 10% pass rate. In other words, 10% of the alloy powder grains have a diameter smaller than D10. Similarly, the D50 and D90 particle sizes correspond to 50% and 90% pass rates, respectively.
[0068] The alloy powder according to the invention has a D10 particle size between 3 and 10 μm, a D50 particle size between 10 and 25 μm, and finally a D90 particle size between 20 and 40 μm.
[0069] The values of D10, D50 and D90 particle sizes are measured according to standard ISO 13322-2. This standard envisages measurements using laser diffraction.
[0070] Powder preparation
[0071] For example, the titanium-based alloy powder as the object of the present invention can be obtained from the basic elements of the TiAl48-2-2 alloy by a powder atomization method. The atomization method can provide the chemical composition and particle size of the alloy powder obtained. In addition, it can ensure a good morphology of the powder, mostly spherical. Finally, it can limit the risk of contamination.
[0072] Metal Injection Molding Method
[0073] The invention also relates to a method for producing a component, in particular for aeronautics, using the titanium-based alloy powder described above.
[0074] Generally speaking, the process includes the sequential steps of mixing, granulation, injection molding, chemical debonding, thermal debonding, sintering and quenching. Figure 2 Describe these steps in more detail.
[0075] mix
[0076] In a first mixing step E1, a titanium-based alloy powder 1 according to the invention is mixed with at least one plastic binder 2, preferably two plastic binders. For example, the binder 2 is polyethylene (PE) or polyethylene glycol (PEG) or a mixture of the two. During the mixing step E1, the temperature is fixed at a value that makes the plastic paste-like so that it can be well mixed. The temperature depends on the composition of the plastic and is, for example, between 50°C and 150°C. In the mixing step E1, the titanium-based alloy powder 1 and the plastic binder 2 are mixed in a selected proportion so as to obtain, at the end of the granulation step E2 described below, the following particles 3 of the alloy and plastic mixture, which have a melt flow index that ensures effective injection of the particles 3 during the molding step E3. Preferably, the mixture of alloy powder 1 and at least one plastic binder 2 comprises, by volume percentage, between 50% and 75% of alloy powder 1 and between 50% and 25% of plastic binder 2, so that the mixture particles 3 have a melt flow index of 60 cm at a temperature between 190°C and 230°C. 3 / 10min to 85cm 3 The melt flow index is between 0.1 and 0.1 μm and is measured according to standard ISO 1133-1.
[0077] Granulation
[0078] In a second step E2 of granulating a mixture of alloy powder and at least one plastic binder, the mixture from step E1 is passed to an extruder to obtain granules 3 of alloy and plastic mixture, known to those skilled in the art as "raw material". The shape and size of the granules 3 of alloy and plastic mixture are determined by the parameter settings of the extruder. For example, the granules 3 of alloy and plastic mixture are cylinders with a base diameter preferably between 1 mm and 5 mm.
[0079] forming
[0080] In a third shaping step E3, the granules 3 of the alloy and plastic mixture are injected into the mold of the part to be produced, with an injection temperature between 160° C. and 200° C. Below 160° C., the mixture is too solid and does not enter the mold. Above 200° C., the mixture is too liquid, the alloy powder separates from the plastic binder and the alloy powder cannot be transported. Other parameters, such as injection speed, injection pressure, post-injection holding time or injection time, depend on the part to be injected.
[0081] After the forming step E3, a green part 4 is obtained, which is a part made of a mixture of alloy powder and plastic (alloy grains suspended in the plastic). Adjustment of the forming parameters makes it possible to obtain a part without pores. The plastic binder ensures the strength of the part.
[0082] Debonding combine
[0083] “Debinding” enables the plastic binder to be removed from the green part 4 previously obtained.
[0084] Two debonding steps are performed consecutively, one chemical debonding and the other thermal debonding.
[0085] Initial debonding combine
[0086] The preliminary debonding E4 is a chemical debonding. The preliminary debonding E4 makes it possible to obtain a partially debonded component 5.
[0087] The debinding can be selected as: debinding using a solvent E4B, or preferably catalytic debinding E4A. The latter has the advantage of being faster.
[0088] Catalytic debinding E4A involves vaporizing the plastic binder by injecting acidic fumes into an oven, which is then burned.
[0089] For example, the catalytic debinding is carried out under a nitrogen atmosphere in the presence of nitric acid fumes at a temperature between 100° C. and 150° C. for 2 to 10 hours, and the nitric acid flow rate is preferably between 2 mL / min and 5 mL / min.
[0090] Debonding using a solvent E4B involves immersing the green part 4 in a bath of said solvent to dissolve the plastic.
[0091] For example, debinding E4B is a debinding using water, where the green part 4 is immersed in a demineralized water bath under stirring at a temperature between 20° C. and 100° C., preferably at about 60° C., for 100 hours to 400 hours.
[0092] At the end of the chemical debonding step E4 , a partially debonded component 5 is obtained, the chemical debonding having resulted in the removal of more than 95% of the plastic binder.
[0093] Thermal debonding combine
[0094] Thermal debonding E5 is preferably carried out by applying two temperature stages successively to the partially debonded part under an argon atmosphere. In the first stage, a temperature between 250° C. and 450° C. is applied for 100 to 300 minutes. In the second stage, a temperature between 350° C. and 550° C. is applied for 100 to 300 minutes.
[0095] At the end of the thermal debonding step ( E5 ), a debonded part or “brown part” is obtained, the thermal debonding enabling the remaining plastic binder to be removed (in other words, less than 5% remains).
[0096] The debonded component 6 from the preliminary E4 and hot E5 debonding steps is a component of the same dimensions as the green component 4. However, the debonded component 6 is highly porous compared to the green component 4, since the plastic binder has been removed, and the density of the debonded component 6 is between 50% and 75% of the density of the cast TiAl alloy component. In addition, the debonded component 6 is very brittle, since the plastic binder that ensures the strength of the component has been removed.
[0097] sintering
[0098] Sintering of the debonded component 6 is carried out during step E6. Sintering consists in subjecting the debonded component 6 to a temperature close to the melting point of the alloy powder, so that the powder grains are bonded together. During sintering, the component shrinks and its density increases.
[0099] Sintering is performed in an oven, preferably under an argon atmosphere at a temperature between 1400° C. and 1450° C. for 2 to 6 hours.
[0100] The thermal debonding step E5 and the sintering step E6 are preferably carried out in the same oven, since the debonded part 6 is brittle.
[0101] At the end of the sintering step E6, a denser sintered part 7 is obtained, the density of which is preferably greater than 95% of the density of conventional cast TiAl alloys. The dimensions of the sintered part 7 are smaller than those of the debonded part or brown part 6. Typically, a reduction in size of 14% to 18% can be observed.
[0102] Figure 3 is an electron microscope image of a component obtained at the end of the sintering step of the method according to the invention. It can be seen that the microstructure is needle-shaped, which is characteristic of titanium-based alloys, the grains are connected, and the material is relatively dense. However, the material also includes residual pores (see small round black dots), which can impair the mechanical properties of the final component. A heat treatment can be performed to remove the residual pores.
[0103] Furthermore, the sintered component 7 made of the titanium-based alloy includes, by weight percentage, 32.0% to 33.5% aluminum, 4.50% to 5.10% niobium, 2.40% to 2.70% chromium, less than 0.1% iron, less than 2000 ppm of dioxygen, less than 0.025% of silicon, less than 350 ppm of carbon, less than 200 ppm of nitrogen, less than 100 ppm of dihydrogen, and less than 500 ppm of unavoidable impurities.
[0104] The chemical composition of the sintered component 7 is very close to that of the initial alloy powder. In the MIM process, only the contents of carbon, dioxygen and nitrogen increase significantly.
[0105] For example, if alloy powder 1 comprises 970 ppm of dioxygen, 90 ppm of nitrogen and 70 ppm of carbon, the sintered component 7 obtained at the end of the method according to the invention starting from alloy powder 1 comprises 1600 ppm of dioxygen, 120 ppm of nitrogen and 340 ppm of carbon.
[0106] The additional elements carbon, oxygen and nitrogen are residues of the plastic binder from which the metal material was impregnated. However, too high a content of said elements would have a negative impact on the mechanical properties of the alloy component from the MIM process, and the carbon, oxygen and nitrogen content of the alloy powder 1 must be much lower than that of the targeted TiAl 48-2-2.
[0107] Hot Isostatic Compacting
[0108] Optionally, a hot isostatic compaction step E7 of the sintered part can be performed to refill the residual pores, in particular when the density of the sintered part is less than 95% of the density of the cast TiAl alloy. The hot isostatic compaction step E7 can increase the density of the part 7 from sintering to 100% of the density of the cast TiAl and improve the mechanical characteristics of the part. In addition, the hot isostatic compaction step E7 can reduce the dimensional dispersion of the parts from the metal injection molding process.
[0109] In the hot isostatic compaction step E7, high pressure and high temperature are applied together under an inert atmosphere. For example, a temperature between 1175° C. and 1195° C., preferably a temperature of 1185° C., and a pressure between 125 MPa and 150 MPa, preferably between 132 MPa and 140 MPa, are applied under an inert atmosphere (e.g., a helium or vacuum atmosphere, preferably an argon atmosphere) for a duration of 1 hour to 5 hours, preferably 3 hours.
[0110] Quenching
[0111] Finally, a quenching heat treatment step E8 is carried out. The quenching heat treatment consists in heating the part to a temperature at which the good alloying elements titanium and aluminum dissolve, for a time long enough to allow said elements to redissolve and diffuse into the crystalline solid. The part is then cooled relatively quickly to allow said good alloying elements to reprecipitate. This step makes it possible to obtain a final part having the desired mechanical and chemical characteristics.
[0112] The quenching heat treatment step E8 is preferably carried out at a temperature of 1150°C for 3 hours. If a hot isostatic compaction step (E7) has been carried out beforehand, the temperature is reduced from 1185°C to 1150°C while maintaining an inert atmosphere. In parallel with this temperature application, a pressure of between 125 MPa and 150 MPa, preferably between 132 and 140 MPa, is applied for 2 hours, and then a pressure of between 100 and 125 MPa, preferably between 115 MPa and 125 MPa, is applied for 1 hour. Finally, the part is cooled at a rate of between 11°C / min and 70°C / min until a temperature of between 690°C and 710°C, preferably 700°C, is reached. Throughout the quenching heat treatment step E8 (including heating and then cooling of the part), an inert atmosphere, such as an argon atmosphere, is maintained, and cooling is carried out at atmospheric pressure.
[0113] Figure 4 is an electron microscope image of the component obtained at the end of steps E7 and E8 of the method according to the invention. The needle-like microstructure can be identified, but the points are no longer visible. Therefore, the hot isostatic compaction step E7 makes it possible to refill the last pores and obtain a completely healthy material.
[0114] Parts obtained by this method
[0115] The invention also relates to a component obtained by a production method using the alloy powder according to the invention.
[0116] The component is a titanium-based alloy component, the component in particular comprising less than 350 ppm of carbon, less than 200 ppm of nitrogen and less than 2000 ppm of dioxygen by weight, the chemical composition being measured by elemental analysis (e.g. by inductively coupled plasma spectroscopy). The properties of the component having the composition of carbon, nitrogen and dioxygen are comparable to or even superior to those of a component made of cast TiAl.
[0117] exist Figure 1 In FIG. 5 , a component made from cast TiAl is shown, which can be seen to have a dual-phase microstructure with two-phase lamellar grains and single-phase gamma grains.
[0118] In contrast, from Figure 4 As can be seen in the figures, the components obtained by the preparation method using the alloy powder according to the invention have a multiphase dual-phase to low-duplex microstructure, with multiphase lamellar grains between 10% and 60% and γ grains between 90% and 40%, which makes them better resistant to traction and fatigue than cast TiAl components. More specifically, for temperatures between 0°C and 800°C, the driven traction fracture R of the components obtained by the preparation method using the powder is m The ultimate stress is greater than 250 MPa. When the stress is greater than 150 MPa, the component reaches a residual plastic deformation Rp of 0.2%. 0.2 Compared to cast TiAl components, fatigue and elastic properties (with 0.2% plastic deformation) are increased by at least 10% up to 700°C.
[0119] The invention finds particular application in the preparation of components for aviation, such as turbine blades / vanes, including blades / vanes with internal passages, turbine nozzles or casing parts, which are subjected to high pressures, must resist corrosion and are used at temperatures exceeding 600°C.
Claims
1. A titanium-based alloy powder (1), characterized in that: The titanium-based alloy powder comprises, by weight percentage, 32.0% to 33.5% of aluminum, 4.50% to 5.10% of niobium, 2.40% to 2.70% of chromium, 0 to 0.1% of iron, 0 to 0.025% of silicon, 0 to 100 ppm of carbon, 0 to 100 ppm of nitrogen, 0 to 1000 ppm of dioxygen, 0 to 50 ppm of dihydrogen and 0 to 500 ppm of unavoidable impurities, and the balance is titanium, and the titanium-based alloy powder has: - D10 particle size between 3 and 10 μm, - a D90 particle size between 20 and 40 μm, and - a particle size D50 between 10 and 25 μm, The values of D10, D50 and D90 particle sizes are measured by laser diffraction according to ISO 13322-2 standard.
2. A method for producing a component, in particular for aviation, characterized in that: The method comprises the following steps: - a step (E1) of mixing the titanium-based alloy powder according to claim 1 with at least one plastic binder (2), - a step of granulating the mixture (E2) in order to obtain granules of a mixture of alloy and plastic (3), - a step (E3) of injection molding the mixture granules (3) in a mold to obtain a green part (4), - a debonding step (E4A, E4B, E5) to obtain a debonded part (6), - a step (E6) of sintering the debound part to obtain a sintered part (7).
3. The method according to claim 2, characterized in that The method further comprises a hot isostatic compaction step (E7), which comprises a heat treatment at a pressure between 125 MPa and 150 MPa, at a temperature between 1175°C and 1195°C, preferably at a temperature of 1185°C, for a duration between 1 hour and 5 hours, preferably 3 hours, said step being carried out after the sintering step (E6).
4. The method according to claim 2 or 3, characterized in that: The method further comprises a step (E8) of quenching the sintered component (7), the step comprising heat treating the sintered component (7) at a temperature between 1140°C and 1160°C for 3 hours, the first two hours at a pressure between 125MPa and 150MPa, and then the last hour at a pressure between 100MPa and 125MPa, the step being carried out after the sintering step (E6) or the hot isostatic compaction step (E7).
5. The method according to any one of claims 2 to 4, characterized in that The alloy and plastic mixture particles (3) have a volume alloy loading of between 50% and 75%, and a melt flow index of between 60 cm 3 / 10min to 85cm 3 / 10min, the injection temperature during the molding step (E3) is between 160°C and 200°C, the measurement of the melt flow index is carried out according to standard ISO 1133-1.
6. The method according to any one of claims 2 to 5, characterized in that The diameter of the particles of the alloy and plastic mixture is between 1 mm and 5 mm.
7. The method according to any one of claims 2 to 6, characterized in that The debonding step (E4A, E4B, E5) itself comprises two consecutive steps: a first chemical step (E4A, E4B) of preliminary debonding of the green part (4) to obtain a partially debonded part (5) and a second step (E5) of thermal debonding of the partially debonded part (5) to obtain a debonded part.
8. The method according to claim 7, characterized in that The preliminary debinding step is a catalytic debinding (E4A) performed under nitrogen for a duration between 2 hours and 10 hours in the presence of nitric acid fumes at a flow rate between 2 mL / min and 5 mL / min and at a temperature between 100°C and 150°C.
9. The method according to claim 7, characterized in that: The preliminary debinding step is a debinding by solvent (E4B) using demineralized water for a duration between 100 and 400 hours under stirring of said water, the temperature of said water being between 20°C and 100°C.
10. The method according to any one of claims 7 to 9, characterized in that The thermal debonding step (E5) is carried out in two consecutive temperature stages under argon, the first temperature stage being carried out between 250°C and 450°C for 100 minutes to 300 minutes and the second temperature stage being carried out between 350°C and 550°C for 100 minutes to 300 minutes.
11. The method according to any one of claims 2 to 10, characterized in that The step (E6) of sintering the debonded part is carried out under an argon atmosphere by applying a temperature between 1400° C. and 1450° C. for a duration of 2 hours to 6 hours.
12. A titanium-based alloy component, particularly for aviation, characterized in that: The titanium-based alloy component is produced by the production method according to any one of claims 2 to 11.
13. The component according to claim 12, characterized in that The component comprises, by weight percentage, 32.0% to 33.5% aluminum, 4.50% to 5.10% niobium, 2.40% to 2.70% chromium, less than 0.1% iron, less than 2000 ppm dioxygen, less than 0.025% silicon, less than 350 ppm carbon, less than 200 ppm nitrogen, less than 100 ppm dihydrogen and less than 500 ppm unavoidable impurities, with the balance being titanium, and the component also has a duplex to low duplex microstructure with multiphase lamellar grains between 10% and 60% and gamma grains between 90% and 40%.
14. A component according to claim 12 or 13, characterized in that The component is a turbine blade / vane or a turbine nozzle.