Method for producing assembled blank, assembled blank, and method for producing clad steel sheet

By adjusting the aiming position of the welding beam when welding high-energy beams in assembly blanks, the problems of high cost and low yield caused by the manufacturing of intermediate spacers and fillers by hot-rolled clad steel plates are solved, deeper and more uniform welding is achieved, and the finished product is improved quality.

CN118900739APending Publication Date: 2024-11-05NIPPON STEEL STAINLESS STEEL CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380025687.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-10
Filing Date
2023-02-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the manufacturing process of hot-rolled clad steel plates, the prior art requires spacers and fillers, resulting in high procurement and processing costs, insufficient welding depth and difficult to grasp the boundaries, which affects the yield rate.

Method used

By using the manufacturing method of assembled blanks, the base material raw material and the contact part of the interlayer material raw material is welded by high-energy beam welding, and the aiming position of the welding beam is staggered from the side of the high-thermal conductivity material to ensure that the ratio of welding depth and width is 3.5 < D/W < Within the range of 5.0, electron beam or laser welding is performed to avoid the use of fillers and spacers.

Benefits of technology

It reduces welding deviation, improves welding depth, reduces costs, avoids deterioration in yield, and ensures the mechanical characteristics and corrosion resistance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900739A_ABST
    Figure CN118900739A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing an assembled blank, an assembled blank, and a method for manufacturing a clad steel sheet. The method for manufacturing an assembled blank as a rolling material for manufacturing a clad steel sheet provided with a base material and an interlayer material bonded to the base material, a contact portion (6) between a base material (1) and an interlayer material (2) of an end surface (12) of an assembly blank (10) is welded using high-energy beam welding, and during the high-energy beam welding, an aiming position (8) of a welding beam (7) is shifted from the contact portion (6) toward a high-thermal-conductivity material side. Consequently, in the assembled blank (10), the deviation between the welded section (9) and the contact surface (11) can be eliminated, and therefore, when the contact sections of dissimilar metals are joined using high-energy beam welding, the penetration of the welded metal can be formed so as not to be deflected toward one material side, and the welding quality can be improved. Provided are a method for manufacturing an assembled blank, an assembled blank, and a method for manufacturing a clad steel sheet, wherein filler does not need to be supplied to welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a clad steel plate having a base material and an interlayer material joined to the base material, and to an assembled billet as a rolling raw material for manufacturing the clad steel plate, a method for manufacturing the assembled billet, and a method for manufacturing the clad steel plate. Background Art

[0002] Stainless steel has excellent corrosion resistance and is therefore suitable for use in harsh corrosive environments. Examples of such harsh corrosive environments include oil well environments, factory equipment exposed to seawater, high chloride environments such as soda, and chemical tankers exposed to various acid solutions. Examples of such harsh corrosive environments include desalination plants, flue gas desulfurization devices, chemical storage tanks, pumps and valves, heat exchangers, and other structural components of oil well pipelines. Stainless steel is used in examples of such harsh corrosive environments.

[0003] On the other hand, stainless steel is a high alloy steel containing more alloying elements such as Cr, Ni, and Mo in order to ensure corrosion resistance. Compared with carbon steel and low alloy steel, the material cost is of course higher, and the cost of processing, welding, etc. is also higher. The steel used in the above-mentioned parts not only requires excellent corrosion resistance, but also requires good mechanical properties such as strength and toughness as structural materials. Therefore, in order to meet these requirements, the amount of alloy used will be further increased. In addition, the situation of price fluctuations due to the rise of alloying elements, etc. is also considered. Therefore, mainly from the cost aspect, the use of these alloying elements is sometimes restricted.

[0004] As described above, in consideration of the cost, it is effective to use a clad steel plate as a material from the viewpoint of processing, welding, etc. The so-called clad steel plate is a material formed by bonding two or more different metals, and is a material in which any one of the two or more metals or all of them are steel plates. In a clad steel plate formed by bonding two metals, the metal on one side is recorded as "parent material", and the metal (raw material) on the other side bonded to the parent material is recorded as "sandwich material". In addition, in the following, the steel plate that is not bonded is referred to as a "solid steel plate". For a solid steel plate composed only of high-alloy steel, the entire steel plate is high-alloy steel, and it is necessary to have both the required surface corrosion resistance and the mechanical properties of the steel plate. In comparison, the clad steel plate makes the surface of one side that is required to have excellent corrosion resistance become a sandwich material of high-alloy steel, and the thickness of the sandwich material is thinner than the thickness of the clad steel plate as a whole, so the amount of high-alloy steel used can be reduced, and the material cost can be reduced. In addition, by increasing the ratio of the thickness of the base material to the overall thickness of the steel plate, and using carbon steel or low alloy steel as the base material, which has sufficient mechanical properties but does not have corrosion resistance, the mechanical properties required of the steel plate can be met. Furthermore, since the number of welded parts that become dissimilar materials can be reduced, the cost of welding materials during welding can also be reduced.

[0005] As described above, by using a clad steel plate formed by laminating a base material and an interlayer material, an interlayer material having excellent corrosion resistance and a base material having excellent mechanical properties can be laminated, thereby obtaining a steel plate having both excellent properties of the interlayer material and the base material.

[0006] For example, the following situation can be considered: as the interlayer material, a high alloy steel or Ni-based alloy having the properties (corrosion resistance, etc.) required as the surface properties of the steel plate in its use environment is used, and as the base material, a carbon steel or low alloy steel having the toughness and strength required in its use environment is used. In such a case, as described above, not only can the cost be reduced, but also the properties (corrosion resistance, etc.) equivalent to the solid steel plate using high alloy steel, as well as the strength and toughness equivalent to carbon steel and low alloy steel can be ensured. Therefore, both economy and functionality can be taken into account.

[0007] In the manufacture of clad steel plates using hot rolling, the rolled raw material before hot rolling is hereinafter referred to as an “assembled billet.” In the assembled billet, the portion that will become the base material of the clad steel plate is referred to as a base material raw material, and the portion that will become the interlayer material of the clad steel plate is referred to as an interlayer material raw material.

[0008] For example, as described in Patent Document 1, the sandwich material raw material and the base material raw material are stacked in a manner that the pressing surface becomes a vacuum, and the pressing surface is sealed around by welding to assemble the clad rolling raw material. Examples include a method of performing electron beam welding in a vacuum, a method of pre-opening a hole for vacuuming, and a method of vacuuming by a vacuum pump after welding around by arc welding or laser welding in the atmosphere. The obtained clad rolling raw material can be directly provided for hot rolling, or a material obtained by overlapping and assembling the sandwich material and the sandwich material in a manner of becoming a base material raw material-sandwich material raw material-stripping agent-sandwich material raw material-base material raw material by applying a stripping agent between the sandwich materials and the sandwich materials as an assembled blank can be provided for hot rolling.

[0009] Patent document 2 discloses an assembly blank, in which a release agent is applied between interlayer materials and interlayer materials to overlap them in a manner of base material raw material-interlayer material raw material-release agent-interlayer material raw material-base material raw material, and then spacers made of the same material as the base material raw material are arranged on the four sides of the interlayer material raw material, and laser beam welding is performed on the mating surfaces of the spacers and the base material raw material.

[0010] Patent document 3 discloses a composite billet for hot rolling, characterized in that when a base material and a sandwich material are directly overlapped and welded all around, when high energy density welding such as electron beam or laser welding is performed, the penetration depth ω is adjusted.

[0011] Patent Document 4 discloses a method for manufacturing a clad steel plate, in which a filler metal is supplied to the periphery of a joint surface of a composite metal plate and an electron beam is irradiated in parallel or at an oblique angle to the joint surface to perform closed welding.

[0012] Prior art literature

[0013] Patent Literature

[0014] Patent Document 1: Japanese Patent Application Publication No. 2021-143387

[0015] Patent Document 2: International Publication No. WO2020 / 175573

[0016] Patent Document 3: Japanese Patent Application Laid-Open No. 52-13456

[0017] Patent Document 4: Japanese Patent Application Laid-Open No. 62-45485 Summary of the invention

[0018] Problems to be solved by the invention

[0019] In the manufacture of clad steel plates using hot rolling, when a material obtained by applying a stripping agent between interlayer materials and interlayer materials in a manner of base material raw material-stripping agent-stripping agent-stripping agent raw material-base material raw material is provided as an assembled billet for hot rolling, the following method is described in Patent Document 2: As described above, spacers made of the same material as the base material raw material are arranged on the four sides of the interlayer material raw material, and the butt surfaces of the spacers and the base material raw material are laser beam welded. When this method is used, the cost of purchasing and processing the spacers is required. In addition, when this method is used, the spacer arrangement portion needs to be cut off after rolling, which causes the deterioration of the rolling processing yield, and it is difficult to grasp the boundary between the spacer and the product part, and there is a possibility that the spacer remains in the product part.

[0020] As described in Patent Document 3, it can be seen that when high-energy beam welding is used to join the contact portions of dissimilar metals, penetration is formed obliquely to one side of the contact portions of the dissimilar metals. Therefore, it is known that the contact portions of the dissimilar metals cannot be welded to a sufficient depth. In addition, when joining is performed while supplying a filler (filling material) to high-energy beam welding as described in Patent Document 4, the purchase cost of the filler and the cost of a device for supplying the filler to the high-energy beam welding machine are incurred.

[0021] The present invention relates to a clad steel plate having a base material and a sandwich material joined to the base material, and its purpose is to provide a method for manufacturing an assembled billet, an assembled billet and a method for manufacturing a clad steel plate. In the assembled billet as a rolled raw material for manufacturing the clad steel plate and the method for manufacturing the assembled billet, it is not necessary to arrange spacers made of the same material as the base material on the four sides of the sandwich material raw material, and when high-energy beam welding is used to join the contact parts of dissimilar metals, penetration is not formed obliquely to one side of the contact parts of the dissimilar metals, and it is not necessary to supply filler to the weld.

[0022] Means for solving problems

[0023] That is, the gist of the present invention is as follows.

[0024] [1] A method for manufacturing an assembled billet as a rolling material for manufacturing a clad steel plate having a base material and a sandwich material joined to the base material, characterized in that, in the assembled billet, a portion of the base material to be the clad steel plate is referred to as a base material material, and a portion of the sandwich material to be the clad steel plate is referred to as a sandwich material material.

[0025] The above-mentioned assembly blank is composed of a base material raw material, a sandwich material raw material, a release agent, a sandwich material raw material and a base material raw material stacked in sequence.

[0026] The contact portion between the base material and the sandwich material in the end face of the assembly blank is welded using high energy beam welding. In the high energy beam welding, the aiming position of the welding beam is shifted from the contact portion to the high thermal conductivity material side in accordance with the thermal conductivity of the base material and the sandwich material.

[0027] [2] In the manufacturing method of the assembly blank described in [1], it is characterized in that the ratio γ of the thermal conductivity of the above-mentioned base material and the sandwich material (taking the side with larger thermal conductivity as the numerator) is greater than 2.5, and the aiming position of the above-mentioned welding beam and the offset of the above-mentioned contact part toward the side of the high thermal conductivity material are greater than 1 mm.

[0028] [3] In the method for manufacturing an assembled blank described in [1], it is characterized in that, for the weld portion between the above-mentioned base material and the above-mentioned interlayer material based on the above-mentioned high-energy beam welding, in the cross section perpendicular to both the surface formed by the above-mentioned contact portion and the end face of the above-mentioned assembled blank, the ratio of the weld bead width W and the penetration depth D of the weld metal satisfies the following formula (1).

[0029] 3.5<D / W<5.0 (1)

[0030] Here, the welding depth of the contact portion between the sandwich material raw material and the base material raw material is referred to as “penetration D”, and the width of the weld metal at the end surface is referred to as “bead width W”.

[0031] [4] In the method for manufacturing an assembled blank described in [2], it is characterized in that, for the weld portion between the above-mentioned base material and the above-mentioned interlayer material based on the above-mentioned high-energy beam welding, in a cross section perpendicular to both the surface formed by the above-mentioned contact portion and the end face of the above-mentioned assembled blank, the ratio of the weld bead width W and the penetration depth D of the weld metal satisfies the following formula (1).

[0032] 3.5<D / W<5.0 (1)

[0033] Here, the welding depth of the contact portion between the sandwich material raw material and the base material raw material is referred to as “penetration D”, and the width of the weld metal at the end surface is referred to as “bead width W”.

[0034] [5] In the method for manufacturing an assembly blank described in any one of [1] to [4], it is characterized in that the high-energy beam welding is electron beam welding, the welding is performed in a vacuum of less than 0.1 kPa, the beam is deflected into a circular shape, and the deflection diameter is is greater than 3 mm, and the offset between the aiming position of the welding beam and the contact portion is the deflection diameter Less than half of.

[0035] [6] In the method for manufacturing an assembly blank described in any one of [1] to [4], it is characterized in that the high-energy beam welding is laser welding.

[0036] [7] An assembled billet as a rolling material for manufacturing a clad steel plate having a base material and an interlayer material joined to the base material, characterized in that, in the assembled billet, a portion of the base material to be the clad steel plate is referred to as a base material material, and a portion of the interlayer material to be the clad steel plate is referred to as an interlayer material material,

[0037] The above-mentioned assembly blank is composed of a base material raw material, a sandwich material raw material, a release agent, a sandwich material raw material, and a base material raw material stacked in sequence, and the ratio γ of the thermal conductivity of the above-mentioned base material raw material and the sandwich material raw material (taking the larger thermal conductivity as the numerator) is greater than 2.5,

[0038] The contact portion between the base material and the sandwich material in the end surface of the assembly blank is welded by high energy beam.

[0039] In a cross section perpendicular to both the surface of the contact portion and the end surface of the assembly blank, the penetration D of the weld metal of the weld portion is 22 mm or more, and the ratio of the weld bead width W to the penetration D satisfies the following formula (1).

[0040] 3.5<D / W<5.0 (1)

[0041] Here, the welding depth of the contact portion between the sandwich material raw material and the base material raw material is referred to as “penetration D”, and the width of the weld metal at the end surface is referred to as “bead width W”.

[0042] [8] A method for manufacturing a clad steel plate, characterized in that an assembled billet manufactured by the method for manufacturing an assembled billet described in any one of [1] to [6] or the assembled billet described in [7] is rolled in a hot rolling step.

[0043] [9] In the method for manufacturing clad steel plates described in [8], it is characterized in that after hot rolling, the welded parts around the clad steel plates are cut off and removed, and the individual clad steel plates are separated starting from the release agent coated on the boundary surface between the interlayer materials.

[0044] The present invention is a method for manufacturing an assembled billet as a rolled raw material for manufacturing a clad steel plate having a base material and an interlayer material joined to the base material, wherein high-energy beam welding is used to weld the contact portion between the base material and the interlayer material in the end face of the assembled billet. In the high-energy beam welding, the aiming position of the welding beam is shifted from the contact portion to the high thermal conductivity material side, thereby eliminating the deviation between the weld portion and the contact surface in the assembled billet. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a cross-sectional view of the assembled blank.

[0046] Figure 2A This is a cross-sectional view showing the welding condition (before welding) of the welded portion when the base material and the interlayer material are of the same nature.

[0047] Figure 2B It is a cross-sectional view showing the welding condition (after welding) of the welded portion when the base material and the interlayer material are of the same nature.

[0048] Figure 3A This is a cross-sectional view showing the welding condition of the welded portion when the base material and the interlayer material are of different natures (when there is a deviation between the welded portion and the contact surface).

[0049] Figure 3B This is a cross-sectional view showing a welding condition (condition where deviation is eliminated) of a weld portion when a base material and an interlayer material are of different natures. DETAILED DESCRIPTION

[0050] The present invention relates to a clad steel plate having a base material and an interlayer material joined to the base material, and targets an assembled billet as a rolling raw material for manufacturing the clad steel plate, a method for manufacturing the assembled billet, and a method for manufacturing the clad steel plate.

[0051] exist Figure 1 1 is a cross-sectional view of an assembled blank 10. In the assembled blank 10, the portion that will become the parent material of the clad steel plate is referred to as the parent material raw material 1, and the portion that will become the sandwich material of the clad steel plate is referred to as the sandwich material raw material 2. Figure 1 As shown, the assembled blank 10 is stacked in order of a base material 1, a sandwich material 2, a release agent 3, a sandwich material 2, and a base material 1. After the assembled blank 10 is hot-rolled, the contact portion 6 between the base material 1 and the sandwich material 2 becomes a bonding surface 14, and the contact surfaces of the sandwich material 2 sandwiched with the release agent 3 become a separation surface 15.

[0052] In the assembly blank of the present invention, if Figure 1 As shown, no spacers made of the same material as the base material 1 are arranged on the four sides of the sandwich material raw material 2. Therefore, on the end face 12 of the assembly blank 10, the sandwich material raw material 2 is in contact with the base material 1 and exposed. In the welding joining, the contact portion 6 between the sandwich material raw material 2 and the base material 1 is welded to form a welded portion 9. High-energy beam welding is used for welding the contact portion 6. Figure 2BThe weld 9 will be described in detail. In the assembled blank 10, when the ratio of the bead width W of the weld metal 4 in the weld 9 to the weld depth Dmax satisfies the following formula (2), it can be estimated that welding was performed by high energy beam welding.

[0053] 2.0≤Dmax / W (2)

[0054] Here, the method for determining the weld bead width W is described. Figure 2B As shown in FIG. 1 , as the depth from the end face 12 increases, the width of the weld metal gradually decreases. Therefore, the width of the weld metal at the end face 12 is defined as the bead width W. In addition, the distance to the maximum depth of the weld metal is defined as the weld depth Dmax. In addition, regarding the extension of the weld metal 4 of the weld, as shown in FIG. Figure 2B As shown in the example of FIG. 1 , the cross section in the direction of weld penetration is etched with an appropriate etching solution and visually confirmed.

[0055] Assuming that the parent material 1 and the sandwich material 2 are homogeneous materials, Figure 2A When welding is performed by aligning the aiming position 8 of the welding beam 7 of the high energy beam irradiation device 5 with the contact portion 6 of the sandwich material raw material 2 and the base material raw material 1 as shown in FIG. Figure 2B As shown, in the welded portion 9 , the weld metal 4 formed by penetration coincides with the position of the contact portion 6 .

[0056] However, the base material 1 and the sandwich material 2 are of course different metals. It can be seen that when the contact portion 6 of different metals is joined by high energy beam welding, Figure 3A When the aiming position 8 of the welding beam 7 of the high-energy beam irradiation device 5 is aligned with the contact portion 6 of the sandwich material raw material 2 and the base material raw material 1 as shown, in the weld portion 9, the weld metal 4 formed by penetration does not coincide with the position of the contact portion 6, but is formed with the metal biased toward one side. Therefore, the contact portion 6 of the sandwich material raw material 2 and the base material 1 cannot be welded to a sufficient depth. Here, the weld depth at the contact portion 6 of the sandwich material raw material 2 and the base material 1 is referred to as "penetration D". When the weld metal 4 coincides with the position of the contact portion 6, the penetration D coincides with the above-mentioned weld depth Dmax (refer to Figure 2B , Figure 3B ), when the position of the weld metal 4 and the contact portion 6 is offset, the penetration D becomes shallower than the weld depth Dmax (refer to Figure 3A ).

[0057] Therefore, the reason for the phenomenon that the welded portion 9 is formed obliquely from the position of the contact portion 6 to one side of the metal is explained. With regard to the position of the weld metal 4 of the welded portion 9, the above-mentioned penetration D is used as an index in the cross section perpendicular to both the surface (contact surface 11) formed by the contact portion 6 and the end surface 12 of the assembly blank 10. If the penetration D is 22 mm or more, it is good.

[0058] Next, when the aiming position 8 of the welding beam 7 of the high-energy beam irradiation device 5 is aligned with the contact portion 6 of the sandwich material raw material 2 and the base material raw material 1, various studies were conducted on the physical properties of the base material 1 and the sandwich material raw material 2, to which side the weld 9 is offset from the contact portion 6, and the degree of offset. Regarding the degree of offset, the penetration depth D is used as an index. As the combined welded materials, the four materials shown in Table 1 (A (ordinary steel), B (ferrite·austenitic stainless steel), C (copper), D (nickel)) are used. The respective component compositions and representative physical properties are shown in Table 1. As a result, it can be determined that the offset of the weld 9 from the contact portion 6 is shifted to the B side in the combination of A and B, to the A side in the combination of A and C, and to the B side in the combination of B and D. The result of comparing this result with the physical properties of the material can be determined for the first time that the difference in thermal conductivity is not the difference in magnetic properties or melting point, but the difference in thermal conductivity. Furthermore, it can be seen that when the thermal conductivity of the base material 1 and the sandwich material 2 is different, the welding offset distance increases in accordance with the degree of difference in thermal conductivity (hereinafter referred to as "ratio γ of the thermal conductivity difference between the base material and the sandwich material (γ = thermal conductivity of the high thermal conductivity material / thermal conductivity of the low thermal conductivity material"). The weld metal 4 is offset to the low thermal conductivity side.

[0059] [Table 1]

[0060]

[0061] Therefore, then, Figure 3B As shown in FIG. 1 , an experiment was conducted in which the aiming position 8 of the welding beam 7 of the high energy beam irradiation device 5 was made inconsistent with the contact portion 6 between the sandwich material raw material 2 and the base material raw material 1, and the aiming position 8 was offset from the contact portion 6 by a distance z (hereinafter referred to as "offset distance z"). As a result, it was found that by offsetting the aiming position 8 toward the high thermal conductivity material side, the deviation of the weld metal 4 from the contact portion 6 can be reduced, and as a result, the penetration depth D can be increased. The manufacturing method of the assembly blank of the present invention was completed based on such a finding, and is characterized in that the base material 1 at the end face 12 of the assembly blank 10 and the contact portion 6 of the sandwich material raw material 2 are welded by high energy beam welding, and in the high energy beam welding, the aiming position 8 of the welding beam 7 is offset from the contact portion 6 to the high thermal conductivity material side.

[0062] Here, the thermal conductivity ratio γ between the base material and the sandwich material and the offset distance z were varied to investigate the relationship between the two that can increase the penetration depth D. As a result, the above-mentioned method for manufacturing an assembly blank of the present invention can clearly exert its effect when the thermal conductivity ratio γ between the base material 1 and the sandwich material 2 is 2.5 or more. At this time, the effect can be effectively achieved by making the offset (offset distance z) between the aiming position 8 of the welding beam 7 and the contact portion 6 to the high thermal conductivity material side be 1 mm or more. More specifically, when the offset distance z to the high thermal conductivity material side is within the range of the following formula (3) corresponding to the thermal conductivity ratio γ, the penetration depth D can be brought within a preferred range.

[0063] 0.35×γ-0.86≤z≤0.35×γ+0.14 (3)

[0064] In the manufacturing method of the assembly blank of the present invention, it is preferred that, with respect to the weld 9 between the base material 1 and the interlayer material 2 based on high-energy beam welding, in a cross section perpendicular to both the surface formed by the contact portion 6 (contact surface 11) and the end face 12 of the assembly blank, the ratio of the weld bead width W and the penetration depth D of the weld metal satisfies the following formula (1).

[0065] 3.5<D / W<5.0 (1)

[0066] Here, as described above, the welding depth of the contact portion between the sandwich material raw material and the base material raw material is referred to as “penetration D”, and the width of the weld metal at the end surface is referred to as “bead width W”.

[0067] By satisfying the inequality on the left side of equation (1), cracks in the weld during hot rolling can be suppressed, and by satisfying the inequality on the right side of equation (1), the excess welding amount can be reduced and manufacturing can be performed efficiently. In addition, the present invention can also be applied by giving an incident angle to the welding beam of high-energy beam welding or defocusing the welding beam as needed.

[0068] As high-energy beam welding, electron beam welding or laser welding can be used.

[0069] When electron beam welding is used as high energy beam welding, it is preferable to perform welding in a vacuum of 0.1 kPa or less. If welding is performed in a vacuum of 0.1 kPa or less, welding sealing can be performed after the pressing surfaces of the base material 1 and the sandwich material 2 are well pressed. In addition, when electron beam welding is used, beam deflection can be used. Preferably, the beam is deflected into a circle with a deflection diameter of By deflecting the beam into a circular shape, the stirring effect of the weld metal can be exerted. The above-mentioned offset distance z is preferably set to the deflection diameter. Thus, the two raw materials can be melted.

[0070] When laser welding is used as high-energy beam welding, a method can be used in which a hole for evacuation is previously opened in the base material 1, and after the surroundings are welded by laser welding, evacuation is performed by a vacuum pump.

[0071] In the method for manufacturing an assembly blank of the present invention, high energy beam welding can also be used to join the sandwich material raw materials 2 at the end surface 12 of the assembly blank 10. In this case, welding can be performed with an offset distance z=0.

[0072] The assembly blank of the present invention manufactured by the above-mentioned method for manufacturing the assembly blank of the present invention is characterized in that the base material 1, the interlayer material 2, the release agent 3, the interlayer material 2, and the base material 1 are stacked in sequence, the thermal conductivity ratio γ of the base material 1 and the interlayer material 2 (taking the larger thermal conductivity as the numerator) differs by more than 2.5, the contact portion 6 between the base material 1 and the interlayer material 2 at the end face 12 of the assembly blank 10 is high-energy beam welded, and in the cross section perpendicular to both the surface formed by the contact portion 6 and the end face 12 of the assembly blank 10, the penetration depth D of the weld metal 4 of the weld portion 9 is more than 22 mm, and the ratio of the weld width W to the penetration depth D satisfies the above-mentioned formula (1). When the ratio γ of the thermal conductivity of the base material 1 and the sandwich material 2 differs by 2.5 or more, when the aiming position 8 of the welding beam 7 of the high energy beam irradiation device 5 is made to coincide with the contact portion 6 of the sandwich material 2 and the base material 1 as in the conventional method, a deviation occurs between the width center of the weld metal and the above-mentioned contact portion, and the penetration depth D becomes less than 22 mm. In contrast, the assembly blank of the present invention, by applying the above-mentioned method for manufacturing the assembly blank of the present invention, can reduce the deviation between the width center of the weld metal and the above-mentioned contact portion, and make the penetration depth D become 22 mm or more, even when the ratio γ of the thermal conductivity of the base material 1 and the sandwich material 2 differs by 2.5 or more.

[0073] The manufacturing method of the clad steel plate of the present invention is characterized in that the assembled billet manufactured by the manufacturing method of the assembled billet of the present invention or the assembled billet of the present invention is rolled in the hot rolling process. In the present invention, the spacer described in Patent Document 2 is not used in the assembled billet, so the cost of purchasing and processing the spacer is not required, and the spacer configuration portion does not need to be cut off after rolling, so it will not become a cause of deterioration of the rolling processing yield, and there is no need to worry about the remaining spacer in the product part. In addition, since it is not a joining performed while supplying filler (filling material) as described in Patent Document 4, the purchase cost of the filler and the cost of the device for supplying the filler into the high-energy beam welding machine are not incurred.

[0074] The manufacturing method of the clad steel plate of the present invention is to further cut and remove the welded parts around the clad steel plate after hot rolling, and separate them into individual clad steel plates starting from the release agent coated on the boundary surface between the interlayer materials.

[0075] As the sandwich material of the clad steel plate and the sandwich material raw material of the assembled blank, high alloy steel such as stainless steel and Ni-based alloy can be used well. In addition, as the parent material of the clad steel plate and the parent material raw material of the assembled blank, steel such as carbon steel and low alloy steel can be used well.

[0076] Example

[0077] Materials A (ordinary steel), B (austenitic stainless steel), C (copper), and D (nickel) shown in Table 1 were used as the joining materials, and electron beam welding was used as the high-energy beam welding, and welding was performed in the combinations shown in Table 2. As the conditions for high-energy beam welding, electron beam welding was performed in a vacuum of 0.1 kPa or less, and the beam was deflected into a circular shape with a deflection diameter of 1. In Table 2, No. 1 to No. 11 is 3 mm, and in No. 12 is 2 mm. The output standard of electron beam welding is set to 16.8 kW. No. 1, 4 to 12 in Table 2 are the standard outputs, and No. 2 and 3 reduce the output to 14.0 kW. Figure 3B As shown, welding was performed by shifting the aiming position 8 of the welding beam 7 of the high energy beam irradiation device 5 from the contact portion 6 by the offset distance z shown in Table 2.

[0078] In a cross section perpendicular to both the surface (contact surface 11) of the contact portion 6 and the end surface 12 of the assembly blank, the weld metal 4 was made clear by etching, and the bead width W and penetration D of the weld metal 4 were measured. Table 2 shows the results.

[0079] [Table 2]

[0080]

[0081] The quality of the obtained welding materials was evaluated.

[0082] Whether rolling is possible or not is evaluated based on the penetration depth D and formula (1). D ≥ 22 mm and conforming to formula (1) is set as S (pass), D ≥ 22 mm and not conforming to formula (1) is set as G (pass), and D < 22 mm is set as X (fail).

[0083] The yield loss was evaluated based on the weld depth Dmax, with Dmax≤40 mm being designated as S (acceptable), Dmax≤50 mm being designated as G (acceptable), and Dmax>50 mm being designated as X (unacceptable).

[0084] Regarding the comprehensive evaluation, in the evaluation of rolling feasibility and yield loss, the case where both are S is set to S (qualified), the case where either or both are G and do not include X is set to G (qualified), and the case where either one includes X is set to X (unqualified).

[0085] Inventive Examples No. 1, 4 to 7, the aiming position 8 of the welding beam 7 was shifted from the contact portion 6 to the high thermal conductivity material side, and the penetration D was 22 mm or more, and good results were obtained. The output of the electron beam welding in Inventive Examples No. 2 and 3 was below the preferred range, and the results were out of the good range of formula (1).

[0086] Comparative Example No. 8 is a result of welding the same materials, which is out of the scope of the present invention. Comparative Examples Nos. 9 and 10 did not set an offset when welding different materials, and Comparative Examples Nos. 11 and 12 shifted the aiming position of the welding beam from the contact portion to the low thermal conductivity material side, and the penetration depth D was less than 22 mm.

[0087] Explanation of symbols

[0088] 1: base material; 2: sandwich material; 3: stripping agent; 4: welding metal; 5: high energy beam irradiation device; 6: contact part; 7: welding beam; 8: aiming position; 9: welding part; 10: assembly blank; 11: contact surface; 12: end surface; 14: joint surface; 15: separation surface.

Claims

1. A method for producing an assembled billet as a rolling material for producing a clad steel plate having a base material and a sandwich material joined to the base material, It is characterized in that In the above-mentioned assembled blank, the part which will become the above-mentioned base material of the above-mentioned clad steel plate is called base material raw material, and the part which will become the above-mentioned sandwich material of the above-mentioned clad steel plate is called sandwich material raw material. The above-mentioned assembly blank is composed of a base material raw material, a sandwich material raw material, a release agent, a sandwich material raw material and a base material raw material stacked in sequence. The contact portion between the base material and the sandwich material at the end face of the assembly blank is welded using high energy beam welding. In the high energy beam welding, the aiming position of the welding beam is shifted from the contact portion to the high thermal conductivity material side in accordance with the thermal conductivity of the base material and the sandwich material.

2. The method for manufacturing an assembly blank according to claim 1, It is characterized in that The thermal conductivity ratio (γ) of the above-mentioned base material and the sandwich material is greater than 2.5, and the aiming position of the above-mentioned welding beam and the offset of the above-mentioned contact portion toward the high thermal conductivity material side are greater than 1 mm, wherein the above-mentioned thermal conductivity ratio uses the side with greater thermal conductivity as the numerator.

3. The method for manufacturing an assembly blank according to claim 1, It is characterized in that For the welded portion between the base material and the sandwich material by the high energy beam welding, in a cross section perpendicular to both the surface formed by the contact portion and the end surface of the assembly blank, the ratio of the weld bead width W to the penetration D of the weld metal satisfies the following formula (1): 3.5<D / W<5.0 (1) Here, the welding depth at the contact portion between the sandwich material raw material and the base material raw material is referred to as the penetration D, and the width of the weld metal at the position of the end surface is referred to as the weld bead width W.

4. The method for manufacturing an assembly blank according to claim 2, It is characterized in that For the welded portion between the base material and the sandwich material by the high energy beam welding, in a cross section perpendicular to both the surface formed by the contact portion and the end surface of the assembly blank, the ratio of the weld bead width W to the penetration D of the weld metal satisfies the following formula (1): 3.5<D / W<5.0 (1) Here, the welding depth at the contact portion between the sandwich material raw material and the base material raw material is referred to as the penetration D, and the width of the weld metal at the position of the end surface is referred to as the weld bead width W.

5. The method for manufacturing an assembly blank according to any one of claims 1 to 4, It is characterized in that The high-energy beam welding is electron beam welding, which is carried out in a vacuum below 0.1 kPa, so that the beam is deflected into a circle with a deflection diameter of is greater than 3 mm, and the offset between the aiming position of the welding beam and the contact portion is the deflection diameter Less than half of.

6. The method for manufacturing an assembly blank according to any one of claims 1 to 4, It is characterized in that The above-mentioned high energy beam welding is laser welding.

7. An assembled blank as a rolling material for producing a clad steel plate having a base material and a sandwich material joined to the base material, It is characterized in that In the above-mentioned assembled blank, the part which will become the above-mentioned base material of the above-mentioned clad steel plate is called base material raw material, and the part which will become the above-mentioned sandwich material of the above-mentioned clad steel plate is called sandwich material raw material. The above-mentioned assembled blank is a base material raw material, a sandwich material raw material, a release agent, a sandwich material raw material, and a base material raw material stacked in sequence, and the ratio (γ) of the thermal conductivity of the above-mentioned base material raw material and the sandwich material raw material is greater than 2.5, wherein the above-mentioned thermal conductivity ratio uses the side with a larger thermal conductivity as a numerator, The contact portion between the base material and the sandwich material at the end surface of the assembly blank is welded by high energy beam. In a cross section perpendicular to both the surface formed by the contact portion and the end surface of the assembly blank, the penetration depth D of the weld metal of the weld portion is 22 mm or more, and the ratio of the weld bead width W to the penetration depth D satisfies the following formula (1), 3.5<D / W<5.0 (1) Here, the welding depth at the contact portion between the sandwich material raw material and the base material raw material is referred to as the penetration D, and the width of the weld metal at the position of the end surface is referred to as the weld bead width W.

8. A method for manufacturing a cladding steel plate, It is characterized in that In the hot rolling step, the assembled billet produced by the method for producing an assembled billet according to any one of claims 1 to 4 is rolled.

9. A method for manufacturing a cladding steel plate, It is characterized in that In the hot rolling step, the assembled billet manufactured by the method for manufacturing an assembled billet according to claim 5 is rolled.

10. A method for manufacturing a cladding steel plate, It is characterized in that In the hot rolling step, the assembled billet manufactured by the method for manufacturing an assembled billet according to claim 6 is rolled.

11. A method for manufacturing a cladding steel plate, It is characterized in that The assembled billet according to claim 7 is rolled in the hot rolling step.

12. The method for manufacturing a clad steel plate according to claim 8, It is characterized in that After hot rolling, the welded parts around the clad steel plate are cut off and removed, and the clad steel plate is separated from the interlayer material using the release agent applied on the interface between the interlayer materials as a starting point to form individual clad steel plates.

13. The method for manufacturing a clad steel plate according to claim 11, It is characterized in that After hot rolling, the welded parts around the clad steel plate are cut off and removed, and the clad steel plate is separated from the interlayer material using the release agent applied on the interface between the interlayer materials as a starting point to form individual clad steel plates.

Citation Information

Patent Citations

  • Clad steel plate and manufacturing method thereof

    JP2021143387A

  • Assembled slab, method for manufacturing same, and method for manufacturing clad steel material

    WO2020175573A1