Method for producing water-absorbent resin

By manufacturing water-absorbing resin through the method of reducing the molecular weight of starch and introducing acidic groups, the problems of insufficient water absorption and poor operability in the existing technology are solved, and the efficient production of high-performance water-absorbing resin is realized.

CN118900850APending Publication Date: 2024-11-05NAGASE & CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028631.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-30
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing water-absorbing resins made from polysaccharides have insufficient water absorption capacity, poor operability during manufacturing, high viscosity, and low production efficiency.

Method used

A method for manufacturing water-absorbing resins by reducing the molecular weight of starch, introducing acidic groups, and drying in the presence of water to form a physical gel includes starch partial decomposition, introduction of acidic groups, and drying processes, with optimized crosslinking conditions.

Benefits of technology

It improves the water absorption performance and production efficiency of water-absorbing resin, reduces viscosity, and improves operability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049542300000071
    Figure BDA0005049542300000071
  • Figure BDA0005049542300000072
    Figure BDA0005049542300000072
  • Figure BDA0005049542300000073
    Figure BDA0005049542300000073
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for producing a water-absorbent resin having high production efficiency and excellent water absorption performance. The present invention relates to a method for producing a water-absorbent resin that forms a physical gel by absorbing water, the method comprising: a step (a1) for obtaining a partial decomposition product of starch by reducing the molecular weight of starch; a step (a2) for obtaining a water-soluble polymer by introducing an acidic group into the partial decomposition product of the starch obtained in the step (a1); and a step (a3) in which the water-soluble polymer is dried in the presence of water at 70-180 DEG C until the solid content reaches 90% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a water-absorbent resin. Background Art

[0002] Water-absorbent resins are widely used in various fields such as sanitary products, food, agriculture, forestry, civil engineering, etc. As such water-absorbent resins, partially neutralized salts of polyacrylic acid and polymethacrylic acid are widely used, and water-absorbent resins made of polysaccharides such as starch are also known.

[0003] Patent Document 1 discloses a method for producing a water-absorbent resin by heating and drying carboxyalkylated starch to crosslink the starches, and states that it is preferable to suppress a decrease in the molecular weight of the starch during the carboxyalkylation reaction.

[0004] Patent Document 2 discloses a method of producing a water-absorbent resin by surface-treating carboxyalkylated polysaccharide particles with a non-crosslinking acid such as hydrochloric acid and then drying them by heating or allowing a crosslinking agent to act to crosslink the polysaccharides.

[0005] Patent Document 3 discloses a method for producing a water-absorbing material by reacting starch with an anhydride of a polybasic acid in an extruder, and states that it is preferable to suppress a decrease in the molecular weight of starch during the reaction with the anhydride of a polybasic acid.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: U.S. Patent No. 5079354

[0009] Patent Document 2: Japanese Patent Application No. 2010-504414

[0010] Patent Document 3: Japanese Patent Application Laid-Open No. 2007-222704 Summary of the invention

[0011] Problems to be solved by the invention

[0012] The water absorption performance of the existing water-absorbent resins made of polysaccharides is not sufficient. In addition, since they are made of high molecular weight polysaccharides, the viscosity of the raw materials is high, and there are problems with the workability during production. The object of the present invention is to provide a method for producing a water-absorbent resin with high production efficiency and excellent water absorption performance.

[0013] Means for solving problems

[0014] The present inventors have completed the present invention by focusing on the molecular weight and cross-linking conditions of starch used as a raw material of a water-absorbent resin.

[0015] That is, the present invention relates to a method for producing a water-absorbent resin that forms a physical gel by absorbing water, comprising: a step (a1) of reducing the molecular weight of starch to obtain a partial decomposition product of starch; a step (a2) of introducing an acidic group into the partial decomposition product of starch obtained in the step (a1) to obtain a water-soluble polymer; and a step (a3) ​​of drying the water-soluble polymer at 70° C. to 180° C. in the presence of water until the solid content reaches 90% or more.

[0016] Preferably, the method further comprises a step (aa) of desalting the water-soluble polymer after the step (a2).

[0017] Preferably, the step (ab) of partially neutralizing the acidic groups of the water-soluble polymer is included in the step (a2) or after the step (a2) and before the step (a3).

[0018] Preferably, a step of partially neutralizing the acidic groups of the water-soluble polymer is not included after the step (a2) and before the step (a3).

[0019] Preferably, in the step (a3), drying is performed until the solid content reaches 90% or more and 99% or less.

[0020] The acidic group is preferably a carboxyalkyl group, a carboxyalkenyl group or a sulfoalkyl group.

[0021] Preferably, in the step (a1), a partially decomposed product of starch having a weight average molecular weight (Mw) of 7,500,000 or less and / or a degree of dispersion (weight average molecular weight (Mw) / number average molecular weight (Mn)) of 5 or more is obtained.

[0022] Preferably, in the step (a1), the molecular weight of starch is reduced by enzyme treatment.

[0023] Preferably, in the step (a2), an acidic group is introduced into a mixture of the partial decomposition product of starch obtained in the step (a1) and the starch whose molecular weight has not been reduced.

[0024] The water-soluble polymer obtained in the step (a2) preferably has a pullulan-equivalent weight average molecular weight (Mw) of 500,000 to 40,000,000 as measured by aqueous size exclusion chromatography.

[0025] Preferably, the obtained water-absorbent resin has the following characteristics:

[0026] (a) the water absorption capacity of ion exchange water without pressure is 100 g / g to 500 g / g;

[0027] (b) The water retention rate of ion exchange water is 80g / g to 300g / g;

[0028] (c) a water absorption capacity of 10 g / g to 70 g / g for physiological saline without pressure; and / or

[0029] (d) The water retention rate of physiological saline is 5g / g to 65g / g.

[0030] Effects of the Invention

[0031] According to the method for producing a water-absorbent resin of the present invention, a water-absorbent resin having excellent water absorption performance can be obtained with high production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a photograph of the gel state of the water-absorbent resin. DETAILED DESCRIPTION

[0033] <<Method 1 for producing water-absorbent resin>>

[0034] The method for producing a water-absorbent resin of the present invention is characterized in that it comprises: a step (a1) of reducing the molecular weight of starch to obtain a partial decomposition product of starch; a step (a2) of introducing an acidic group into the partial decomposition product of starch obtained in the step (a1) to obtain a water-soluble polymer; and a step (a3) ​​of drying the water-soluble polymer at 70° C. to 180° C. in the presence of water until the solid content reaches 90% or more, thereby producing a water-absorbent resin that forms a physical gel by absorbing water.

[0035] <Step (a1) of reducing the molecular weight of starch to obtain a partially decomposed product of starch>

[0036] In this step, the starch is reduced in molecular weight to reduce viscosity. The type of starch used as the raw material is not particularly limited, and examples thereof include waxy corn starch, tapioca starch, potato starch, corn starch (including waxy corn starch and high-amylose starch), wheat starch, rice starch, sweet potato starch, and the like.

[0037] Starch may be a derivative (also called processed starch or chemical starch) or bleached starch in which the hydrogen atoms of some hydroxyl groups of the glucose unit are replaced by functional groups. The position of the hydroxyl group whose hydrogen atoms are replaced may be any of the 1st, 2nd, 3rd, 4th and 6th positions of the glucose unit, preferably the 2nd, 3rd and 6th positions. Examples of the functional group include hydrocarbon groups such as methyl and ethyl; substituents having a hydroxyl group such as hydroxypropyl and hydroxyethyl; substituents having a carboxyl group such as carboxymethyl; and acyl groups such as formyl, acetyl and propionyl.

[0038] Specific examples of starch derivatives include acetylated starch, acetylated adipic acid cross-linked starch, acetylated phosphorylated cross-linked starch, oxidized acetylated starch, sodium octenyl succinate starch, acetic acid starch, oxidized starch, hydroxypropyl starch, hydroxypropyl phosphate cross-linked starch, phosphoric acid monoesterified phosphoric acid cross-linked starch, phosphorylated starch, phosphoric acid cross-linked starch, cationized starch, urea phosphate esterified starch, etc., which are used for food and industrial use and are known as so-called processed starch. In addition, methyl ethylated starch, hydroxypropyl methylated starch, etc. substituted with two or more functional groups may also be used. Among them, acetic acid starch, oxidized starch, acetylated starch, oxidized acetylated starch, hydroxypropyl starch, hydroxypropyl phosphate cross-linked starch, sodium octenyl succinate starch are preferred from the perspective of easy control of the properties of the water-absorbing resin.

[0039] The method of reducing the molecular weight of starch is not particularly limited, and methods such as enzyme treatment, acid treatment, physical crushing, etc. can be cited. In addition, these methods can also be combined. Preferably, a part of the glycosidic bonds of the α-glucose molecules constituting the starch are hydrolyzed by these methods, but there is no limitation on the position and mode of decomposition. As a reaction apparatus, a reactor, an extruder, etc. can be used.

[0040] In the case of reducing the molecular weight of starch by enzyme treatment, the enzyme used is not particularly limited, but in order to efficiently reduce the molecular weight, it is preferred to use an endo-type enzyme. As specific examples of enzymes, α-amylase, cyclomaltodextrin glucanotransferase, 4-α-glucanotransferase, 6-α-glucanotransferase, 4,6-α-glucanotransferase, amylomaltase, neopullulanase, amyloplulanase, etc. can be cited. These enzymes can also be used in combination. The pH during enzyme treatment is not particularly limited, preferably pH 5.0 to 7.0. The adjustment of pH can be carried out by adding hydrochloric acid, acetic acid, sodium hydroxide, potassium hydroxide, etc. The enzyme treatment can be carried out while the starch is heated and kneaded at 70°C to 110°C and gelatinized. In addition, the enzyme treatment can be carried out after the gelatinization of the starch, or it can be carried out simultaneously with the gelatinization. As a method for performing enzyme treatment after the gelatinization of the starch, a method of first suspending the starch in water and heating it to gelatinize it, and then adding an enzyme to carry out an enzyme reaction can be cited. Examples of a method for performing enzyme treatment simultaneously with gelatinization of starch include a method in which starch is suspended in water, an enzyme is further added, and the resulting mixed solution is heated within a temperature range in which the enzyme is not completely inactivated.

[0041] When the molecular weight of starch is reduced by acid treatment, the acid used is not particularly limited, and specific examples thereof include hydrochloric acid, sulfuric acid, oxalic acid, acetic acid, formic acid, trifluoroacetic acid, etc. The temperature during the acid treatment is preferably 150°C to 160°C.

[0042] When partial decomposition of starch is performed by physical disruption, specific means include radiation irradiation, shearing, grinding, high pressure treatment, ultrasonic wave, thermal decomposition, photodecomposition, and combinations thereof.

[0043] The weight average molecular weight of the starch partial decomposition product obtained in step (a1) is preferably 7.5 million or less, more preferably 6 million or less. If the weight average molecular weight exceeds 7.5 million, the viscosity becomes high, and there is a tendency for the reaction during the introduction of the acidic group in step (a2) and the operability during purification to decrease. The lower limit of the weight average molecular weight of the starch partial decomposition product is not particularly limited, but is preferably 50,000 or more, more preferably 200,000 or more. When the weight average molecular weight is less than 50,000, there is a tendency for the water retention of the water-absorbing resin to decrease. It should be noted that the method for determining the weight average molecular weight is not particularly limited. For example, in aqueous size exclusion chromatography, it can be obtained based on a calibration curve of molecular weight and elution time prepared by pullulan with a known molecular weight.

[0044] The number average molecular weight of the starch partial degradation product obtained in step (a1) is not particularly limited, but is preferably 1,000,000 or less in consideration of viscosity. In addition, the lower limit of the number average molecular weight of the starch partial degradation product is preferably 10,000 or more, more preferably 50,000 or more. It should be noted that the method for determining the number average molecular weight is not particularly limited, and for example, in aqueous size exclusion chromatography, it can be obtained based on a calibration curve of molecular weight and elution time prepared using pullulan with a known molecular weight.

[0045] The weight average molecular weight or number average molecular weight of the partial decomposition product obtained in step (a1) can be adjusted by mixing two or more partial decomposition products of starch. In this case, the weight average molecular weight or number average molecular weight of the mixture preferably satisfies the above numerical range.

[0046] The degree of dispersion (weight average molecular weight / number average molecular weight) of the partially decomposed starch obtained in step (a1) is preferably 5 or more, more preferably 7 or more. The upper limit of the degree of dispersion is not particularly limited as long as the numerical range of the weight average molecular weight is satisfied, but is usually 70 or less.

[0047] In step (a1), starch that has not been reduced in molecular weight may remain. When starch that has not been reduced in molecular weight remains, the remaining amount is preferably less than 20% by weight relative to the total amount of starch introduced in step (a1).

[0048] <Step (a2) of Obtaining a Water-Soluble Polymer>

[0049] In this step, an acidic group is introduced into the partial decomposition product of starch obtained in step (a1) to obtain a water-soluble polymer. The water-soluble polymer is obtained by introducing an acidic group into the partial decomposition product of starch. The introduced acidic group may be in any state of a free acid state, a salt state, or an ionized state, and these may coexist.

[0050] In addition, in this process, an acidic group can be introduced into a mixture of a partial decomposition product of starch obtained in process (a1) and a starch that has not been reduced in molecular weight. The starch that has not been reduced in molecular weight can be a starch that is provided for the reduction in molecular weight reaction in process (a1) but has not been decomposed to a weight average molecular weight (Mw) of less than 7.5 million, or it can be an untreated starch added after process (a1). The presence of starch that has not been reduced in molecular weight can increase the water absorption when a water-absorbing resin is made. It is believed that this is because the distance between the crosslinking points of the physical gel is increased by the presence of a water-soluble polymer from starch that has not been reduced in molecular weight, thereby making it easy to expand the crosslinking network. In this process, according to the use and the allowable cost, two or more starches and / or partial decomposition products of starch with different weight average molecular weights can also be used in combination.

[0051] Examples of the acidic group include acidic groups having a carboxyl group such as carboxyalkyl and carboxyalkenyl; acidic groups having a sulfonic group such as sulfoalkyl and sulfoalkenyl; and acidic groups having a phosphoryl group such as phosphoalkyl and phosphoalkenyl.

[0052] The carboxyalkyl group is an alkyl group substituted with a carboxyl group. The number of carbon atoms of the alkyl group substituted with a carboxyl group is preferably 1 to 8, more preferably 1 to 5. The alkyl group may be either linear or branched. Specific examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 1-methyl n-butyl, 2-methyl n-butyl, 3-methyl n-butyl, 1,1-dimethyl n-propyl, 1,2-dimethyl n-propyl, 2,2-dimethyl n-propyl, 1-ethyl n-propyl, and the like.

[0053] Specific examples of the carboxyalkyl group include a carboxymethyl group, a carboxyethyl group, a carboxypropyl group, a carboxybutyl group, and a carboxypentyl group.

[0054] The carboxyalkenyl group is an alkenyl group substituted with a carboxyl group. The number of carbon atoms of the alkenyl group substituted with a carboxyl group is preferably 2 to 8, more preferably 2 to 4. The alkenyl group may be either straight chain or branched. Specific examples of alkenyl groups include vinyl, 1-propenyl, 2-propenyl, 1-methyl-1-vinyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylvinyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, etc.

[0055] Specific examples of the carboxyalkenyl group include carboxyvinyl group, carboxypropenyl group, carboxybutenyl group and the like.

[0056] The sulfoalkyl group is an alkyl group substituted with a sulfo group. Examples of the alkyl group substituted with a sulfo group include the alkyl groups described above for the carboxyalkyl group. Specific examples of the sulfoalkyl group include a sulfomethyl group, a sulfoethyl group, a sulfopropyl group, and the like.

[0057] The sulfoalkenyl group is an alkenyl group substituted with a sulfo group. Examples of the alkenyl group substituted with a sulfo group include the alkenyl groups described with respect to the carboxyalkenyl group. Specific examples of the sulfoalkenyl group include sulfovinyl and sulfopropenyl.

[0058] The phosphoalkyl group is an alkyl group substituted with a phosphoryl group. As the alkyl group substituted with a phosphoryl group, the alkyl group described for the carboxylalkyl group can be used. Specific examples of the phosphoalkyl group include a phosphomethyl group, a phosphoethyl group, a phosphopropyl group, and the like.

[0059] The phosphoenyl group is an alkenyl group substituted with a phosphoryl group. As the alkenyl group substituted with a phosphoryl group, the alkenyl group described with respect to the carboxyalkenyl group can be used. Specific examples of the phosphoenyl group include phosphovinyl group, phosphoacryl group, and the like.

[0060] Among the acidic groups, acidic groups having a carboxyl group or a sulfo group are preferred, carboxyalkyl groups, carboxyalkenyl groups, and sulfoalkyl groups are more preferred, and carboxyalkyl groups having 1 to 5 carbon atoms are further preferred.

[0061] In order to introduce the acidic group, the partial decomposition product of starch is reacted with a compound containing an acidic group or a precursor thereof. The compound containing an acidic group is not particularly limited as long as it can introduce the above-mentioned acidic group, and examples thereof include halogenated alkyl compounds having an acidic group, halogenated alkenyl compounds having an acidic group, acid anhydrides, and salts thereof. Examples of the halogen constituting the halogenated alkyl compound and the halogenated alkenyl compound include chlorine and bromine.

[0062] Specific examples of the acidic group-containing compound include monochloroacetic acid, monobromoacetic acid, 3-bromopropionic acid, 6-bromohexanoic acid, succinic anhydride, maleic anhydride, vinylsulfonic acid, phosphorus oxychloride, ethyl monochloroacetate, and sodium salts and potassium salts thereof.

[0063] Precursors of compounds containing acidic groups include acrylonitrile, etc. Examples of methods using acrylonitrile include the following method: first, acrylonitrile is reacted with starch or a partial decomposition product thereof under alkaline conditions to introduce a cyanoethyl group, the cyanoethyl group is derivatized into an amide group (Synthesis; 1989 (12): 949-950), and the resulting amide is subjected to alkaline hydrolysis.

[0064] The outline of the reaction of generating a water-soluble polymer by the reaction of a starch partial degradation product with monochloroacetic acid is shown in formula (I).

[0065] [Chemistry 1]

[0066]

[0067] The outline of the reaction of generating a water-soluble polymer by the reaction of a starch partial degradation product with 3-bromopropionic acid is shown in formula (II).

[0068] [Chemistry 2]

[0069]

[0070] The outline of the reaction of generating a water-soluble polymer by the reaction of a starch partial degradation product with 6-bromohexanoic acid is shown in formula (III).

[0071] [Chemistry 3]

[0072]

[0073] The outline of the reaction of generating a water-soluble polymer by the reaction of a starch partial degradation product and succinic anhydride is shown in formula (IV).

[0074] [Chemistry 4]

[0075]

[0076] The outline of the reaction of generating a water-soluble polymer by the reaction of a starch partial degradation product and maleic anhydride is shown in formula (V).

[0077] [Chemistry 5]

[0078]

[0079] The outline of the reaction of generating a water-soluble polymer by the reaction of a starch partial degradation product with sodium vinyl sulfonate is shown in formula (VI).

[0080] [Chemistry 6]

[0081]

[0082] Formulas (I) to (VI) show water-soluble polymers in which a sodium salt of an acidic group is introduced into all hydroxyl groups at the 6-position of the glucose unit, but hydroxyl groups into which an acidic group is not introduced may remain. In addition, acidic groups that are not neutralized by salt may also exist. The position where the acidic group is introduced is not limited as long as it is a hydroxyl group present in the partial decomposition product of starch, and may be any of the hydroxyl groups at the 1-position, 2-position, 3-position, 4-position, and 6-position.

[0083] The reaction conditions of the partial decomposition product of starch and the compound containing an acidic group are not particularly limited. When a halogenated alkyl compound having a carboxyl group is used as the compound containing an acidic group, it is preferred to use 1 to 1.5 equivalents of an alkali agent relative to the compound containing an acidic group. When a halogenated alkyl compound having a carboxyl group (acidic group) such as monochloroacetic acid and monobromoacetic acid is used as the compound containing an acidic group, it is preferred to use an alkali agent required for neutralization of the carboxyl group, that is, an alkali agent with the same equivalent as the carboxyl group. As the alkali agent, sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, potassium carbonate, etc. can be cited. These alkali agents can be used alone or in combination of two or more. The reaction pH of the partial decomposition product of starch with the compound containing an acidic group or its precursor is preferably 4 or more, more preferably 8 or more.

[0084] The bonding form between the partial decomposition product of starch and the acidic group is preferably a covalent bond. Specifically, an ether bond or an ester bond formed between a hydroxyl group on the partial decomposition product of starch and the alkyl part of the acidic group can be mentioned.

[0085] The acidic group introduced into the partial degradation product of starch preferably forms a salt with sodium, potassium, lithium, ammonia, etc. from an alkali agent, and therefore, the alkali agent preferably uses an amount required for the reaction of the compound containing the acidic group with the partial degradation product of starch and the neutralization of the acidic group of the compound containing the acidic group. For example, when monochloroacetic acid is used as the compound containing the acidic group, the alkali agent is theoretically preferably used in an amount of more than 2 equivalents relative to the monochloroacetic acid. When sodium monochloroacetate is used, the acidic group is neutralized in advance, so the alkali agent is preferably used in an amount of more than 1 equivalent relative to sodium monochloroacetate.

[0086] The amount of the compound containing an acidic group can be arbitrarily set according to the target total acid value (etherification degree) of the water-soluble polymer. Usually, it is preferably set to 0.5 equivalents to 5.0 equivalents, and more preferably to 0.5 equivalents to 2.0 equivalents, relative to 1 mole of hydroxyl groups of the partial decomposition product of starch. In the case of using a halogenated alkyl compound such as monochloroacetic acid to react in the form of an aqueous solution, the introduction reaction of the acidic group competes with the hydrolysis reaction of the halogenated alkyl compound, so the halogenated alkyl compound needs to be in excess than the theory. The amount of the halogenated alkyl compound in the aqueous solution reaction is preferably set to less than 5 equivalents relative to the theoretical value.

[0087] When a halogenated alkyl compound or a salt thereof is used as the acidic group-containing compound, the reaction temperature with the partial decomposition product of starch is preferably 0 to 100°C, and preferably 25 to 90°C to prevent hydrolysis by water in the reaction solution.

[0088] The reaction time is preferably the time until the halogenated alkyl compound as the raw material is consumed, and for the stability of the halogenated alkyl compound and the high efficiency of the process, it is more preferably 1 hour to 12 hours. The reaction can be carried out in water, or in a mixed solvent of water and alcohols such as methanol, ethanol, isopropanol, butanol, glycol ethers such as ethylene glycol dimethyl ether, etc., or the powder of the dried starch partial decomposition product can be dispersed in hydrophilic solvents such as alcohols such as methanol, ethanol, isopropanol, butanol, glycol ethers such as ethylene glycol dimethyl ether. When a mixed solvent is used, the proportion of solvents other than water is preferably less than 50% by volume in the mixed solvent. As a reaction apparatus, a reactor, an extruder, etc. can be used.

[0089] When anhydride is used as the compound containing an acidic group, the reaction can be carried out only by mixing the starch partial decomposition product with the anhydride and heating it, but in order to promote the reaction, tertiary amines such as sodium carbonate, sodium hydroxide, triethylamine, imidazoles such as 2-methylimidazole, quaternary ammonium salts such as tetrabutylammonium bromide, and phosphonium salts such as tetrabutylphosphonium bromide can be used as catalysts. The addition amount of these catalysts is preferably less than 0.1 equivalent relative to the compound containing an acidic group. These catalysts can be used alone or in combination of two or more.

[0090] The reaction time is preferably the time until the anhydride is consumed, and more preferably 1 hour to 12 hours. The end point of the reaction can be determined by acid value determination and IR determination. The reaction can be carried out in water, but in order to prevent hydrolysis and alcoholysis of the anhydride, it is preferred to use aprotic solvents such as dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone as the reaction solvent. In the case of using a mixed solvent, the proportion of solvents other than water is preferably 50% by volume or more in the mixed solvent. In the case of reacting under solvent-free conditions, the anhydride can play the role of a solvent, so the reaction temperature is preferably carried out above the melting point of the anhydride. In the case of using a solvent in the reaction, the reaction temperature is preferably 50°C to 100°C, and more preferably 70°C to 90°C. As a reaction apparatus, a reactor, an extruder, etc. can be used.

[0091] <Physical Properties of Water-Soluble Polymers>

[0092] The molecular weight of the water-soluble polymer produced in step (a2) is not particularly limited, and the weight average molecular weight of pullulan converted based on the aqueous size exclusion chromatography analysis is preferably 500,000 to 40 million, and more preferably 700,000 to 35 million. When the weight average molecular weight is less than 500,000, there is a tendency for the water retention of the water-absorbing resin to decrease, and when it exceeds 40 million, there is a tendency for the water absorption performance of the water-absorbing resin to decrease. It should be noted that the weight average molecular weight of pullulan converted based on the aqueous size exclusion chromatography analysis can be obtained based on a calibration curve of molecular weight and elution time prepared by pullulan with a known molecular weight in the aqueous size exclusion chromatography.

[0093] The total acid value of the water-soluble polymer is preferably 50 mgKOH / g to 350 mgKOH / g, more preferably 70 mgKOH / g to 300 mgKOH / g. The total acid value represents the amount of all acidic groups introduced into the water-soluble polymer. If the total acid value is less than 50 mgKOH / g or exceeds 350 mgKOH / g, the water-absorbing performance of the water-absorbing resin after cross-linking the water-soluble polymer in an aqueous solution containing electrolytes such as physiological saline tends to decrease.

[0094] In the case of introducing an acidic group on a water-soluble polymer by reacting a halogenated alkyl compound having a carboxyl group with a hydroxyl group of starch or a partial decomposition product thereof, the amount of the acidic group (carboxyalkyl group) introduced can also be represented by the degree of etherification. The degree of etherification of the water-soluble polymer is preferably 0.1 to 2.0, more preferably 0.2 to 1.5. The degree of etherification can be determined by ashing titration or the like. In addition, the total acid value is detected by the introduction of carboxyalkyl groups. In the case where the partial decomposition product of starch as a raw material does not contain acidic groups such as carboxyalkyl groups, it is considered that the acidic groups detected by the determination of the total acid value are equal to the acidic groups introduced by the etherification reaction. Therefore, in the case where there are no acidic groups in the starch or the partial decomposition product of the raw material, the degree of etherification can be simply calculated by calculation from the numerical value of the above-mentioned total acid value. For example, in the case where the carboxyalkyl group is a carboxymethyl group and all of them are neutralized as sodium salts, it can be calculated by degree of etherification = (162 × total acid value) ÷ (56100-80 × total acid value). It should be noted that the unit of the total acid value at this time is mgKOH / g.

[0095] The free acid value of the water-soluble polymer is not particularly limited, but is preferably 0 to 70 mgKOH / g, and more preferably 0 to 50 mgKOH / g. The acidic groups on the water-soluble polymer form salts with sodium, potassium, lithium, ammonia, etc., and when no step of partially neutralizing the acidic groups is included, the free acid value is preferably 0 mgKOH / g. When the acidic groups are introduced into the partial decomposition product of starch and the step (ab) of partially neutralizing the acidic groups is included, the free acid value is preferably 5 mgKOH / g to 70 mgKOH / g, and more preferably 7 mgKOH / g to 50 mgKOH / g. The free acid value refers to the acid value obtained by measuring the unneutralized acidic groups. If the free acid value exceeds 70 mgKOH / g, there is a tendency for the water absorption performance to decrease.

[0096] The dispersity (weight average molecular weight / number average molecular weight) of the water-soluble polymer is not particularly limited, but is preferably 5 to 50, more preferably 7 to 45. If it is less than 5 or exceeds 50, the water absorption performance of the water-absorbent resin tends to decrease. The number average molecular weight of the water-soluble polymer is determined by aqueous size exclusion chromatography.

[0097] The biomass degree of the water-soluble polymer is preferably 50% or more, more preferably 60% or more. The biomass degree is the ratio (mass %) of elements derived from natural resources among the elements constituting the water-soluble polymer, and can be measured by the method described in Examples.

[0098] <Desalting Step (aa)>

[0099] After the above step (a2), a step (aa) of desalting the water-soluble polymer may be included. By desalting, the alkali metal halide by-product in step (a2), the salt of the unreacted alkyl halide compound used in step (a2), and the salt produced in the step (ab) of partial neutralization described later can be removed. As a desalting method, a desalting method using a solvent and a desalting method using an ultrafiltration membrane can be mentioned. As a desalting method using a solvent, for example, a method of washing by the following process can be mentioned: a water-soluble polymer is dissolved in water to prepare an aqueous solution, and the aqueous solution is added dropwise to a hydrophilic solvent such as methanol, ethanol, isopropanol, acetone, acetonitrile, etc., so that the water-soluble polymer is reprecipitated, filtered and recovered, and then the filtered and recovered water-soluble polymer is dispersed again in aqueous methanol (water content of 70% to 90%), stirred, and filtered to recover the particles of the water-soluble polymer. As a method using an ultrafiltration membrane, a method of treating an aqueous solution of a hydrophilic polymer using a filter having an ultrafiltration membrane can be mentioned. As the washing liquid during desalination, water or a mixed solution of water and a hydrophilic organic solvent such as methanol, ethanol, propanol, acetone, or acetonitrile can be used. Desalination is preferably performed until the salt concentration in the water-soluble polymer becomes 1% or less.

[0100] <Step (ab) of partially neutralizing the water-soluble polymer>

[0101] In the step (a2), or after the step (a2) and before the drying step (a3), a step (ab) of partially neutralizing the acidic groups of the water-soluble polymer may be included.

[0102] In the water-soluble polymer obtained in step (a2), when the carboxyl, sulfonyl or phosphoryl part of the acidic group introduced into the partial decomposition product of starch forms a salt with sodium, potassium, lithium, ammonia, etc. from the alkaline agent, the salt is neutralized using an acid in step (ab). By neutralization, a part of the carboxyl, sulfonyl or phosphoryl group that forms a salt is converted into a free carboxylic acid, sulfonic acid or phosphoric acid. In addition, in the water-soluble polymer obtained in step (a2), when the carboxyl, sulfonyl or phosphoryl part of the acidic group introduced into the partial decomposition product of starch is a free acid that does not form a salt, the salt is neutralized using an alkali in step (ab). By neutralization, a part of the free carboxylic acid, sulfonic acid or phosphoric acid is converted into a carboxyl, sulfonyl or phosphoric acid that forms a salt.

[0103] Partial neutralization is preferably performed on a portion of the carboxyl groups, sulfonyl groups or phosphoryl groups on the water-soluble polymer that form salts. For example, when monochloroacetic acid is used as the acidic group-containing compound and sodium hydroxide is used as the alkaline agent in step (a2), a water-soluble polymer having a sodium salt of a carboxyl group added to the starch partial decomposition product can be obtained. By adding an acid thereto, a portion of the carboxyl groups are converted into free carboxylic acids.

[0104] In addition, partial neutralization is preferably performed on a portion of the carboxyl groups, sulfonyl groups or phosphoryl groups on the water-soluble polymer that have not formed a salt. For example, when succinic anhydride is used as the acidic group-containing compound in step (a2), a water-soluble polymer having free carboxylic acid added to the starch partial degradation product can be obtained. By adding a base thereto, a portion of the free carboxylic acid is converted into a carboxyl group that has formed a salt.

[0105] In step (ab), the neutralization degree of the acidic groups of the partially neutralized water-soluble polymer is preferably 1% to 50%, more preferably 5% to 25%. By setting the neutralization degree within this range, there is a tendency that the production of the water-absorbent resin becomes easier. The neutralization degree is the ratio of the acidic groups present in the water-soluble polymer that are neutralized, and is calculated by the following formula.

[0106] Neutralization degree (%) = ((free acid value of water-soluble polymer) ÷ (total acid value of water-soluble polymer)) × 100

[0107] The total acid value of the water-soluble polymer and the free acid value of the water-soluble polymer are as described above with respect to the physical properties of the water-soluble polymer.

[0108] An acid is used for neutralization of the carboxyl group that forms a salt. The acid is not particularly limited, and is preferably an acid having a pKa equal to or lower than that of the carboxyl group, and examples thereof include hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, acetic acid, formic acid, trichloroacetic acid, and the like. A strong acid is preferably used for neutralization of the sulfonic group or phosphoryl group that forms a salt, and an inorganic acid such as hydrochloric acid or sulfuric acid or a strongly acidic ion exchange resin is more preferably used. Neutralization can be carried out using a known device such as a reactor or an extruder. After adding the acid, it is preferably stirred at 0 to 50° C. for 0.2 to 1 hour for the neutralization reaction. The neutralization reaction is preferably carried out under the conditions of pH 6.8 to 7.2.

[0109] A base is used for neutralization of free carboxylic acid, sulfonic acid, and phosphoric acid. The base is not particularly limited, and examples thereof include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, ammonia, dimethylamine, tetramethylammonium hydroxide, and the like. Neutralization can be performed using a known apparatus such as a reactor and an extruder. After adding the base, it is preferably stirred at 0 to 50° C. for 0.2 to 1 hour for the neutralization reaction. The neutralization reaction is preferably performed at pH 6.8 to 7.2.

[0110] In the neutralization reaction of the carboxyl group, sulfonyl group or phosphoryl group forming a salt, a salt may be formed between the halogen derived from the acidic group-containing compound and the metal or ammonia derived from the alkali agent. The salt can be removed in the above-mentioned desalting step (aa).

[0111] When the step (ab) is performed in the step (a2), it is preferred that partial neutralization is performed after the reaction of the partial decomposition product of starch with the acidic group-containing compound in the step (a2).

[0112] On the other hand, the above-mentioned step (ab) is not essential. As one embodiment of the present invention, the following method for producing a water-absorbent resin can also be cited, wherein the step of partially neutralizing the acidic groups of the water-soluble polymer is not included after the above-mentioned step (a2) and before the drying step (a3). When the step of partially neutralizing is not included, the cost of partial neutralization can be reduced.

[0113] <Drying step (a3)>

[0114] In this step, the water-soluble polymer is dried in the presence of water at 70° C. to 180° C. until the solid content reaches 90% or more. The water-soluble polymer at the start of step (a3) ​​may be an aqueous solution or a wet powder containing water.

[0115] As the liquid component contained in the water-soluble polymer, water and a mixed solvent of water and a hydrophilic solvent can be cited. As the hydrophilic solvent, lower aliphatic alcohols such as methanol, ethanol, n-propanol, isopropanol, etc.; ketones such as acetone; ethers such as dioxane, tetrahydrofuran, methoxy (poly)ethylene glycol; amides such as ε-caprolactam, N,N-dimethylformamide, etc. can be cited. Two or more of these hydrophilic solvents can be used in combination. The proportion of the hydrophilic solvent in the mixed solvent is preferably adjusted according to the boiling point of the hydrophilic solvent. When the boiling point of the hydrophilic solvent is below 100°C, it is preferably 70% by volume or more, and when it is higher than 100°C, it is preferably 30% by volume or less.

[0116] When the water-soluble polymer is a wet powder at the start of step (a3), the content of the liquid component is preferably 50 to 90 wt %, more preferably 60 to 80 wt %, and even more preferably 65 to 75 wt %.

[0117] The drying is performed until the solid content of the water-soluble polymer reaches 90% or more, preferably 93% or more, more preferably 95% or more, and further preferably 97% or more. The upper limit of the solid content is preferably 99% or less. Here, the solid content refers to the weight ratio of water to the weight of components other than the hydrophilic solvent in the water-soluble polymer. By drying until the solid content of the water-soluble polymer reaches 90% or more, even when the step of partially neutralizing the acidic groups of the water-soluble polymer is not included before step (a3), a water-absorbent resin that forms a physical gel by absorbing water can be obtained.

[0118] The temperature during drying is preferably 70°C to 180°C. Furthermore, the temperature during drying is more preferably selected according to the presence or absence of the step (ab) for partially neutralizing the acidic group. In the case of including the step (ab) for partially neutralizing the acidic group, it is preferably 70°C to 150°C, and more preferably 70°C to 130°C. In the case of not including the step (ab) for partially neutralizing the acidic group, it is preferably 80°C to 150°C, and more preferably 100°C to 130°C. The device used for drying is not particularly limited, and a drum dryer, a spray dryer, a Nauta mixer, etc. can be used.

[0119] In step (a3), a crosslinked structure is formed between water-soluble polymers. The crosslinks formed here are equivalent to internal crosslinks of the water-absorbing resin. The crosslinks are preferably formed by the acidic groups on the water-soluble polymer introduced in step (a2). As crosslinked structures, for example, ionic bonds formed between acidic groups, coordination bonds formed by metal ions, hydrogen bonds based on dimerization of acidic groups, etc. can be cited. In the range that does not hinder the decomposition of the obtained water-absorbing resin, the crosslinks may include crosslinks based on covalent bonds. In the case of crosslinks based on covalent bonds, it is preferably less than 5% of the crosslinked structure, and more preferably less than 2%. As crosslinks based on covalent bonds, ester bonds, ether bonds, carbon-carbon single bonds (CC bonds), carbon-carbon double bonds (C=C bonds), etc. can be cited.

[0120] As described above, the cross-linked structure can be formed without using a cross-linking agent, but a cross-linking agent can also be used. Examples of the cross-linking agent include epoxy compounds, polyol compounds, polyamine compounds, polyisocyanate compounds, alkylene carbonate compounds, halogenated epoxy compounds, halohydrin compounds, polyoxazoline compounds, carbodiimide compounds, silane coupling agents, and polyvalent metal compounds.

[0121] Examples of the epoxy compound include glycidyl succinate, sorbitol polyglycidyl ether, trimethylolpropane polyglycidyl ether, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and glycidol.

[0122] Examples of the polyol compound include ethylene glycol, diethylene glycol, propylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, 1,3-propylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerol, polyglycerol, 2-butene-1,4-diol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,2-cyclohexanediol, trimethylolpropane, diethanolamine, triethanolamine, polyoxypropylene, ethylene oxide-propylene oxide block copolymer, pentaerythritol, and sorbitol.

[0123] Examples of the polyamine compound include ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneimine, inorganic salts or organic salts (azitinium salts, etc.) of these polyamine compounds, and polysaccharides having an amino group such as chitin.

[0124] Examples of the polyisocyanate compound include 2,4-toluene diisocyanate and hexamethylene diisocyanate, and examples of the polyoxazoline compound include 1,2-ethylenebisoxazoline.

[0125] Examples of the alkylene carbonate compounds include 1,3-dioxolane-2-one, 4-methyl-1,3-dioxolane-2-one, 4,5-dimethyl-1,3-dioxolane-2-one, 4,4-dimethyl-1,3-dioxolane-2-one, 4-ethyl-1,3-dioxolane-2-one, 4-hydroxymethyl-1,3-dioxolane-2-one, 1,3-dioxane-2-one, 4-methyl-1,3-dioxane-2-one, and 4,6-dimethyl-1,3-dioxane-2-one.

[0126] Examples of the halogenated epoxy compound include epichlorohydrin, epibromohydrin, α-methylepichlorohydrin, and polyamine adducts thereof (for example, Kymene (registered trademark) manufactured by HERCULES).

[0127] In addition, as other known cross-linking agents, aqueous carbodiimide compounds (for example, CARBODILITE manufactured by Nisshinbo Chemical Co., Ltd.), silane coupling agents such as γ-glycidoxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane, and polyvalent metal compounds such as hydroxides or chlorides of zinc, calcium, magnesium, aluminum, iron, zirconium, etc. can also be used.

[0128] In step (a3), structural units other than water-soluble polymers may be optionally mixed to make them cross-linked. As structural units other than water-soluble polymers, for example, polyacrylic acid (salts) such as partially neutralized cross-linked polyacrylic acid, self-cross-linked partially neutralized polyacrylic acid, and starch-acrylic acid graft polymers may be mentioned. As salts of acrylic acid, sodium salts, potassium salts, and ammonium salts may be mentioned. As structural units other than water-soluble polymers, anionic unsaturated monomers such as methacrylic acid, maleic acid, vinyl sulfonic acid, styrene sulfonic acid, 2-(methyl)acrylamide-2-methylpropanesulfonic acid, 2-(methyl)acryloylethanesulfonic acid, and 2-(methyl)acryloylpropanesulfonic acid and their salts; acrylamide, methacrylamide, N-ethyl (methyl)acrylamide, N-n-propyl (methyl)acrylamide, N-isopropyl (methyl)acrylamide, N,N-dimethyl (methyl)acrylamide, 2-hydroxyethyl (methyl)acrylate, 2-hydroxypropyl (methyl)acrylate Ester, methoxy polyethylene glycol (meth)acrylate, polyethylene glycol mono(meth)acrylate, vinyl pyridine, N-vinyl pyrrolidone, N-acryloyl piperidine, N-acryloyl pyrrolidine and other nonionic hydrophilic group-containing unsaturated monomers; (meth)acrylate N,N-dimethylaminoethyl, (meth)acrylate N,N-diethylaminoethyl, (meth)acrylate, N,N-dimethylaminopropyl, (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, and quaternary ammonium salts thereof, linear cellulose, poly(γ-glutamic acid), etc.

[0129] When the water-absorbent resin contains structural units other than the water-soluble polymer, the content thereof is preferably 90 wt % or less, more preferably 50 wt % or less, and further preferably 20 wt % or less, based on the total amount of the water-soluble polymer used as the main component.

[0130] In order to impart various functions, the water-absorbent resin may contain other additives such as disinfectants, deodorants, antibacterial agents, fragrances, various inorganic powders, foaming agents, pigments, dyes, hydrophilic short fibers, fertilizers, oxidants, reducing agents, water, and salts. The method and amount of these additions may be appropriately selected by those skilled in the art.

[0131] After the drying step (a3), surface crosslinking can be performed. Surface crosslinking can improve the strength of the water-absorbent resin. The crosslinking agent used in the surface crosslinking can be the same as the crosslinking agent described above for the crosslinking of step (a3). Among these, epoxy compounds are preferred, and ethylene glycol diglycidyl ether, sorbitol polyglycidyl ether, and succinic acid glycidyl ester are more preferred.

[0132] The surface crosslinking can be formed by spraying a surface crosslinking agent on the water-absorbent resin, mixing the mixture by a known method using a cylindrical mixer, a V-shaped mixer, a ribbon mixer, a screw mixer, a double-arm mixer, a pulverizing kneading machine, etc. A surfactant can be added as needed during the spraying and mixing.

[0133] In order to remove impurities and by-products, the produced water-absorbing resin may be subjected to treatments such as desalination and washing. Desalination may be performed using a filter having a reverse osmosis membrane, etc. As the washing liquid, water or a mixed liquid of water and a hydrophilic organic solvent such as methanol, ethanol, or propanol may be used.

[0134] <<Method 2 for producing water-absorbent resin>>

[0135] The production method of the present invention is characterized in that it includes: a step (b1) of introducing an acidic group into starch; a step (b2) of reducing the molecular weight of the starch having the acidic group to obtain a water-soluble polymer; and a step (b3) of drying the water-soluble polymer at 70°C to 180°C in the presence of water until the solid content reaches 90% or more.

[0136] <Step (b1) of introducing acidic groups into starch>

[0137] In this step, starch is reacted with an acidic group-containing compound. The starch, acidic group, and acidic group-containing compound used are the same as those described above in the step (a2) of introducing an acidic group into a partial degradation product of starch.

[0138] The conditions for the reaction of starch with the acidic group-containing compound are not particularly limited. When a halogenated alkyl compound having a carboxyl group is used as the acidic group-containing compound, it is preferred to use 1 to 1.5 equivalents of an alkali agent relative to the acidic group-containing compound. In order to stabilize the starch, the pH is preferably 10.5 to 12.5, and more preferably pH 11 to 12. As the alkali agent for adjusting the pH, sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, and potassium carbonate can be cited.

[0139] The acidic group of starch is preferably formed into salt with sodium, potassium, lithium, ammonia etc. from alkaline agent, therefore, alkaline agent preferably uses the amount required for the neutralization of the acidic group of the compound containing acidic group and starch and the acidic group of the compound containing acidic group. For example, when using monochloroacetic acid as the compound containing acidic group, alkaline agent theoretically preferably uses more than 2 equivalents relative to monochloroacetic acid. When using sodium monochloroacetate, acidic group is neutralized in advance, therefore alkaline agent preferably uses more than 1 equivalent relative to sodium chloroacetate.

[0140] The amount of the compound containing an acidic group can be arbitrarily set according to the target total acid value (etherification degree) of the water-soluble polymer. Usually, relative to 1 mol of hydroxyl groups of starch, it is preferably set to 0.5 equivalent to 5.0 equivalents, and more preferably set to 0.5 equivalent to 2.0 equivalents. When a haloalkyl compound such as monochloroacetic acid is used to react in the form of an aqueous solution, the introduction reaction of the acidic group competes with the hydrolysis reaction of the haloalkyl compound, so the haloalkyl compound needs to be in excess than theory. The amount of the haloalkyl compound in the aqueous solution reaction is preferably set to less than 5 equivalents relative to the theoretical value.

[0141] The reaction temperature of starch and the compound containing an acidic group is not particularly limited, and is preferably 0 to 120° C., more preferably 0 to 100° C. The reaction time is not particularly limited, and is preferably 1 to 24 hours. The reaction can be carried out in water, or in a mixed solvent of water and alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, diethylene glycol, propylene glycol, ethylene glycol monoethyl ether, glycol ethers such as ethylene glycol dimethyl ether, etc. When a mixed solvent is used, the proportion of solvents other than water in the mixed solvent is preferably 50% by volume or less. As a reaction apparatus, a reactor, an extruder, etc. can be used.

[0142] In particular, when chloroacetic acid or its salt is used as a haloalkyl compound, in order to prevent hydrolysis caused by water in the reaction solution, it is preferably carried out at 25°C to 60°C. The reaction time is preferably the time until the haloalkyl compound as a raw material is consumed, and for the stability of the haloalkyl compound and the efficiency of the process, it is more preferably 1 hour to 6 hours. The reaction can be carried out in water, or in a mixed solvent of water and alcohols such as methanol, ethanol, isopropanol, butanol, glycol ethers such as ethylene glycol dimethyl ether, etc., or the powder of the dried starch can be dispersed in a hydrophilic solvent such as alcohols such as methanol, ethanol, isopropanol, butanol, glycol ethers such as ethylene glycol dimethyl ether. When a mixed solvent is used, the proportion of solvents other than water is preferably less than 50% by volume in the mixed solvent. As a reaction apparatus, a reactor, an extruder, etc. can be used.

[0143] In addition, when using anhydride as the compound containing acidic group, only by mixing starch with anhydride and heating, reaction can be carried out, but in order to promote the reaction, quaternary ammonium salts such as imidazoles such as sodium carbonate, sodium hydroxide, triethylamine, tetrabutylammonium bromide, tetrabutylphosphonium bromide, etc. can be used as catalysts. Relative to the compound containing acidic group, the addition amount of these catalysts is preferably below 0.1 equivalent. These catalysts can be used alone, or two or more can be used in combination.

[0144] The reaction time is preferably the time until the acid anhydride as a raw material is consumed, and more preferably 1 hour to 12 hours. The end point of the reaction can be determined by acid value determination and IR determination. The reaction can be carried out in water, but in order to prevent the hydrolysis and alcoholysis of the acid anhydride, a non-protonic solvent such as dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone is preferably used as a reaction solvent. In the case of using a mixed solvent, the proportion of solvents other than water is preferably 50% by volume or more in the mixed solvent. In the case of reacting under solvent-free conditions, the acid anhydride can play the role of a solvent, so the reaction temperature is preferably carried out above the melting point of the acid anhydride. In the case of using a solvent in the reaction, the reaction temperature is preferably 50°C to 100°C, and more preferably 70°C to 90°C. As a reaction apparatus, a reactor, an extruder, etc. can be used.

[0145] <Step (b2) of Obtaining a Water-Soluble Polymer>

[0146] In this step, the starch having an acidic group obtained in step (b1) is reduced in molecular weight to reduce viscosity. The method of reducing the molecular weight is not particularly limited, and examples thereof include methods such as enzyme treatment, acid treatment, and physical crushing of the starch. These methods are as described above for step (a1) of reducing the molecular weight of the starch to obtain a partial decomposition product of the starch.

[0147] After step (a2), the water-soluble polymer may be desalted in the same manner as in step (aa) above. Alternatively, the acidic groups of the water-soluble polymer may be partially neutralized in the same manner as in step (ab) above.

[0148] <Drying step (b3)>

[0149] In this step, the water-soluble polymer is dried at 70°C to 180°C in the presence of water until the solid content reaches 90% or more. The water-soluble polymer at the start of step (b3) may be an aqueous solution or a wet powder containing water. The liquid component contained in the water-soluble polymer used and its content, drying conditions, solid content ratio, and cross-linked structure formed between the water-soluble polymers are as described above for the drying step (a3).

[0150] <<Crosslinking structure of water-absorbent resin>>

[0151] Generally, a water-absorbent resin having polyacrylic acid as a main structural unit has a network structure based on covalent bonds and forms a chemical gel by absorbing water. In contrast, the water-absorbent resin obtained in the production method 1 and the production method 2 of the water-absorbent resin of the present invention is characterized in that it forms a physical gel by absorbing water. The physical gel can be converted into a sol having fluidity because the crosslinking points are relatively easy to disappear due to the thermal motion of the molecular chain, changes in pH and ionic strength, etc., and is therefore easily decomposed by the addition of alkali or acid, heating, shaking, etc., thereby reducing the environmental burden when discarded.

[0152] The formation of a physical gel can be confirmed by confirming the sol-gel transition caused by the disappearance of the above-mentioned crosslinking points. For example, in the case of crosslinking by ionic bonds and / or hydrogen bonds, it can be confirmed by fluidization after alkali or acid treatment. Specifically, when a water-absorbent resin is suspended in a 1% sodium hydroxide aqueous solution so as to have a final concentration of 5% by weight and stirred for 60 minutes, and then sieved with a sieve with a mesh of 500 μm, the dry weight of the water-absorbent resin remaining on the sieve is less than 2% by weight of the dry weight of the water-absorbent resin contained in the above-mentioned aqueous solution. In this case, it can be determined that the water-absorbent resin forms a physical gel by absorbing water.

[0153] More specifically, 0.5 g of the water-absorbent resin was suspended in 9.5 g of a 1% NaOH aqueous solution and stirred for 60 minutes, and then naturally filtered using a 30-mesh metal mesh (mesh size 500 μm) of about 50 mm × 50 mm square, and the mesh was cleaned with ion exchange water. After cleaning, the metal mesh was dried in a 120°C blower dryer for 2 hours. When the weight of the metal mesh before filtration is Wm1 and the weight of the metal mesh after filtration and drying is Wm2, when the 30-mesh sieve residue obtained by the following formula is less than 2% by weight, it can be determined that a physical gel is formed by absorbing water. It should be noted that the sieve with a mesh size of 500 μm is a 30-mesh sieve specified in JIS.

[0154] 30 mesh sieve residue (%) = (Wm2-Wm1) / 0.5×100

[0155] The 30-mesh sieve residue is preferably less than 2% by weight, more preferably less than 1.5% by weight, further preferably less than 1.0% by weight, and still further preferably less than 0.5% by weight.

[0156] In addition, the formation of a physical gel due to water absorption can also be confirmed by observing the properties of the water-absorbent resin after adding water. Specifically, 0.2 g of the water-absorbent resin is placed in a nylon mesh tea bag, which is immersed in 1 L of water and left to stand for 3 hours. The solubility in water and the gel strength are evaluated according to the criteria described in the Examples. When the evaluation is 2 to 6, it can be determined that a physical gel has been formed.

[0157] <<Water Absorption Performance of Water-Absorbent Resin>>

[0158] The water absorption rate without pressure of the water-absorbent resin obtained in the production method 1 and the production method 2 of the water-absorbent resin of the present invention is determined by measuring the absorbency of the water-absorbent resin to saline or ion-exchanged water when no load is applied to the water-absorbent resin by the method described in the Examples. The water absorption rate without pressure of the water-absorbent resin to ion-exchanged water in the state of a solid substance is preferably 100 g / g to 500 g / g, more preferably 120 g / g to 460 g / g. In addition, the water absorption rate without pressure to saline is preferably 10 g / g to 70 g / g, more preferably 20 g / g to 70 g / g, and further preferably 30 g / g to 65 g / g.

[0159] The ratio (A / B) of the water-absorbent resin's absorption capacity (A) for ion-exchanged water to its absorption capacity (B) for physiological saline is preferably 7 or less, more preferably 5 or less.

[0160] The water retention rate of the water-absorbent resin is determined by measuring the absorbency of the water-absorbent resin for saline or ion-exchanged water when a load of 150 G is applied to the water-absorbent resin by the method described in the Examples. The water retention rate of the water-absorbent resin for ion-exchanged water in the state of a solid substance is preferably 80 g / g to 300 g / g, more preferably 100 g / g to 300 g / g. In addition, the water retention rate for saline is preferably 5 g / g to 65 g / g, more preferably 10 g / g to 60 g / g, and further preferably 20 g / g to 60 g / g.

[0161] The biomass degree of the water-absorbent resin is preferably 50% or more, more preferably 60% or more. The biomass degree is the ratio (mass %) of elements derived from natural resources in the elements constituting the water-absorbent resin, and can be calculated, for example, from the biomass degree of the water-soluble polymer measured by the method described in the Examples, taking into account changes in molecular weight due to partial neutralization and crosslinking.

[0162] <<Method for decomposing water-absorbent resin>>

[0163] The water-absorbent resin obtained in the production method 1 and the production method 2 of the water-absorbent resin of the present invention can be decomposed by alkali treatment. When the alkali treatment is performed, the water-absorbent resin is preferably placed under conditions of pH 9 or higher, more preferably pH 10 or higher. By the alkali treatment, the cross-linked structure and glucosidic bonds of the water-absorbent resin are cleaved and decomposed into water-soluble polymers, which can reduce the environmental burden when discarded.

[0164] The alkali agent used in the alkali treatment is not particularly limited, and examples thereof include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, potassium carbonate, etc. The temperature during the alkali treatment is not particularly limited, and the treatment can be performed at, for example, 5°C to 50°C.

[0165] <<Articles containing water-absorbent resin>>

[0166] Various articles can be manufactured by the water-absorbent resin obtained by the production method 1 and the production method 2 of the water-absorbent resin of the present invention. Examples of the articles include: disposable diapers, sanitary products, incontinence pads, portable toilets, waste disposal bags, urine and feces treatment agents for animals, medical treatment materials, surgical cloths, dental waste liquid treatment agents, medical waste blood coagulants, wound dressing materials, moisturizers and other sanitary products, medical products, soil water-retaining agents, seedling cloths, seed coatings, fertilizer slow-release agents, pesticide and fertilizer disintegration aids, desert greening materials, agricultural films, preservatives and other agricultural and gardening products, soil modifiers, sludge solidifying agents, waterproof materials and other civil engineering materials, as well as cooling agents, thickeners, deodorants, food drip absorbents, pet mats, disposable body warmers, battery gelling agents, anti-condensation sheets, fillers, artificial snow and other articles. Examples of sanitary products include laminates in which a back sheet, an absorbent and a top sheet are laminated in this order. The absorbent body contains the water-absorbent resin of the present invention and may further contain absorbent paper or pulp as required. The specific method for producing the article is not particularly limited, and each article can be produced by a known method.

[0167] These articles contain the water-absorbent resin and are therefore easily decomposed. The water-absorbent resin can be decomposed by alkaline treatment conditions, which can reduce the environmental burden when it is discarded.

[0168] Example

[0169] Hereinafter, the present invention will be described with reference to Examples, but the present invention is not limited to the following Examples. Hereinafter, "parts" or "%" means "parts by weight" or "% by weight", respectively, unless otherwise specified.

[0170] (1) Materials used

[0171] (1-1) Starch raw materials

[0172] Corn starch

[0173] Tapioca starch

[0174] Tapioca starch acetate

[0175] Oxidized acetylated tapioca starch

[0176] Acetylated tapioca starch

[0177] Hydroxypropylated starch

[0178] Hydroxypropylated cross-linked starch phosphate

[0179] (1-2) Hydrolase

[0180] α-Amylase (Spitase (registered trademark) HK / R manufactured by Nagase ChemteX Corporation), 12,200 units / g

[0181] Amylomaltase: Thermus thermophilus was aerobically cultured, the recovered bacterial cell extract was centrifuged, and the supernatant was used as a crude enzyme solution. The crude enzyme solution was subjected to column chromatography according to a conventional method, and the sample purified to a single substance by electrophoresis was used as a purified enzyme solution.

[0182] It should be noted that the activity of amylomaltase is measured by the following method. A reaction solution 1 containing 10 w / v% maltotriose, 50 mM sodium acetate buffer (pH 6.0) and an enzyme is incubated at 60°C for 20 minutes. Then, the reaction is stopped by heating at 100°C for 10 minutes. The amount of glucose in the reaction solution is determined by the glucose oxidase method. Regarding the unit amount of amylomaltase, the amylomaltase activity that generates 1 μmol of glucose in 1 minute is set to 1 unit.

[0183] (2) Production of Partially Degraded Starch Products (Production Examples 1 to 7)

[0184] The starch partial degradation product was prepared by the following method. It should be noted that the weight average molecular weight of the obtained starch partial degradation product was obtained based on a calibration curve of molecular weight and elution time prepared by pullulan with a known molecular weight in aqueous size exclusion chromatography. The weight average molecular weight and dispersity of the starch partial degradation product are shown in Table 1.

[0185] (Production Example 1) Partially Degraded Starch from Corn Starch

[0186] Corn starch was suspended in tap water at a concentration of 15% (w / w), and 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. A crude amylomaltase enzyme solution was added to the starch milk at a rate of 0.4 units per 1 gram of starch solid matter, and the mixture was stirred at room temperature for 30 minutes and then reacted at 80°C for 6 hours under stirring to prepare liquefied starch. The weight average molecular weight of the obtained starch partial decomposition product was 1.93 million, and the degree of dispersion was 9.6.

[0187] (Production Example 2)

[0188] Corn starch was suspended in tap water at a concentration of 30% (w / w), and 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To the starch milk, 0.15 units of a crude amylomaltase solution and 0.04 units of α-amylase were added to each gram of starch solid matter, and after stirring at room temperature for 30 minutes, the mixture was reacted at 80°C for 6 hours under stirring to prepare liquefied starch. The weight average molecular weight of the obtained starch partial decomposition product was 1.34 million, and the degree of dispersion was 10.6.

[0189] (Production Example 3)

[0190] Liquefied starch was prepared by the same operation as in Production Example 1 except that the concentration of corn starch was 30% (w / w) and the amount of crude amylomaltase solution was 0.2 units per 1 gram of starch solid matter. The weight average molecular weight of the obtained starch partial degradation product was 1.97 million and the degree of dispersion was 10.5.

[0191] (Production Example 4)

[0192] Liquefied starch was prepared by the same operation as in Production Example 3 except that corn starch from a different batch was used. The weight average molecular weight of the obtained starch partial degradation product was 1,910,000, and the degree of dispersion was 10.1.

[0193] (Production Example 5)

[0194] Liquefied starch was prepared by the same operation except that the concentrations of corn starch and enzyme in Manufacturing Example 3 were maintained and the scale was expanded to 14 times. The weight average molecular weight of the obtained starch partial degradation product was 5.16 million and the dispersity was 26.3. It is speculated that the reaction efficiency changed due to the expansion of the scale, and the molecular weight and dispersity increased compared with Manufacturing Example 3.

[0195] (Production Example 6)

[0196] The aqueous solution of the starch partial decomposition product obtained in Preparation Example 2 was vacuum dried at 80°C, and the obtained dried product was pulverized to recover a dry powder product passing 1 mm. The moisture content of the dry powder product was 2.7%. It should be noted that the molecular weight and dispersity of the obtained starch partial decomposition product were based on Preparation Example 2.

[0197] (Production Example 7)

[0198] After corn starch was suspended in tap water at a concentration of 15% (w / w), 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. In the starch milk, 0.5 units of α-amylase were added per 1 gram of starch solid matter, and after stirring at room temperature for 30 minutes, the mixture was reacted at 100°C for 20 minutes under stirring to prepare liquefied starch. The weight average molecular weight of the obtained starch partial decomposition product was 1.37 million, and the dispersity was 65.6. The concentration of corn starch was the same as that in Manufacturing Example 1, but it is presumed that the reaction efficiency changed due to the expansion of the scale and the difference in the enzyme used, and the dispersity increased compared with Manufacturing Example 1.

[0199] [Table 1]

[0200] Production Example 1 Manufacturing Examples 2, 6 Production Example 3 Production Example 4 Production Example 5 Production Example 7 Mw(million) 193 134 197 191 516 137 Dispersion 9.6 10.6 10.5 10.1 26.3 65.6

[0201] (3) Production of water-soluble polymers

[0202] (Production Example 8)

[0203] 200 g of a 15 wt% aqueous solution of the starch partial decomposition product prepared in Preparation Example 1 (0.56 mol of hydroxyl groups of the starch partial decomposition product) was placed in a 500 ml separable flask equipped with a stirrer, a thermometer, and a cooling tube. Next, 76.5 g of a 48.8% sodium hydroxide aqueous solution (0.93 mol, 1.68 equivalents to the hydroxyl groups of the starch partial decomposition product) was added, and the mixture was stirred at 60°C or below until the solution was completely uniform. After confirming that the solution was uniform, an aqueous solution prepared by dissolving 42.0 g of monochloroacetic acid (0.44 mol, 0.8 equivalents to the hydroxyl groups of the starch partial decomposition product) in 10.5 g of ion exchange water was added dropwise at 50°C to 60°C for 30 minutes. After the monochloroacetic acid aqueous solution was added, the temperature was adjusted to 45°C to 50°C, and the mixture was stirred for 10 hours. Regarding the end point of the reaction, the reaction solution was sampled and the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01N silver nitrate solution, with the condition that the chloride ion content reached 98% or more of the calculated value of 4.8% when the monochloroacetic acid was completely reacted. In this production example, the chloride content was 4.8%.

[0204] After the reaction was completed, the reaction solution was diluted with 200 g of ion exchange water. The diluted reaction solution was cooled to room temperature and added to 1.7 L of methanol over a period of about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by vacuum filtration.

[0205] Next, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 0.9 L of aqueous methanol with a methanol / water ratio of 80 / 20 (volume ratio), stirred at room temperature for 30 minutes for washing, and then filtered under reduced pressure for solid-liquid separation to recover the water-soluble polymer again. The chlorine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01N silver nitrate solution, and the washing process was repeated until the chlorine content was less than 1%. The total acid value of the obtained water-soluble polymer was 166 mgKOH / g, and the degree of etherification calculated from the total acid value was 0.63.

[0206] (Production Examples 9 to 14)

[0207] A water-soluble polymer was obtained by carrying out a reaction in the same manner as in Production Example 8 except that the raw materials, the charge amounts and the reaction temperature were changed to those shown in Table 2.

[0208] (Production Example 15)

[0209] 200 g of a 30 wt% aqueous solution of the starch partial decomposition product prepared in Preparation Example 4 (1.11 mol of hydroxyl groups of the starch partial decomposition product) is placed in a 500 ml removable flask equipped with a stirrer, a thermometer, and a cooling tube. Next, 79.4 g of a 48.8% sodium hydroxide aqueous solution (0.96 mol, 0.86 equivalents relative to the hydroxyl groups of the starch partial decomposition product) is added, and the mixture is stirred at a temperature below 60°C until the solution is completely uniform. After confirming that the solution has reached uniformity, 89.9 g of 6-bromohexanoic acid (0.46 mol, 0.4 equivalents relative to the hydroxyl groups of the starch partial decomposition product) is added little by little at 50°C to 60°C over a period of 30 minutes. After adding 6-bromohexanoic acid, the temperature is adjusted to 45°C to 50°C and stirred for 10 hours. At the end point of the reaction, the reaction solution was sampled and the bromide ion content in the reaction solution was measured by potentiometric titration using a 0.01N silver nitrate solution, with the condition that the bromide ion content reached 98% or more of the calculated value of 9.8% when 6-bromohexanoic acid was fully reacted. In this production example, the bromine content was 10.1%.

[0210] After the reaction was completed, the reaction solution was diluted with 250 g of ion exchange water. The diluted reaction solution was cooled to room temperature and added to 1.6 L of ethanol over a period of about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the ethanol was subjected to solid-liquid separation by vacuum filtration.

[0211] Next, in order to remove the sodium bromide contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 0.5 L of aqueous ethanol with an ethanol / water ratio of 90 / 10 (volume ratio), stirred at room temperature for 30 minutes for washing, and then filtered under reduced pressure for solid-liquid separation to recover the water-soluble polymer again. The bromine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01N silver nitrate solution, and the washing process was repeated until the bromide ion content was less than 1%. The total acid value of the obtained water-soluble polymer was 145 mgKOH / g, and the degree of etherification calculated from the total acid value was 0.64.

[0212]

[0213] (Production Example 16)

[0214] 27.2 g of the powder of the starch partial hydrolyzate produced in Production Example 7 (0.47 mol of hydroxyl groups of the starch partial hydrolyzate) and 58.1 g of dimethyl sulfoxide (DMSO) were added to a 300 ml separable flask equipped with a stirrer, a thermometer, and a cooling tube to dissolve them. Then, 14.2 g of succinic anhydride (0.14 mol, 0.30 equivalents to the hydroxyl groups of the starch partial hydrolyzate) was added, and the mixture was stirred at 70°C to 75°C for 1 hour to react. The reaction solution after stirring was sampled and neutralized and titrated with 0.1 N NaOH. As a result, the acid value of the reaction solution was 85 mgKOH / g (theoretical end point acid value 80.1 mgKOH / g).

[0215] After the reaction is completed, 125 g of ion exchange water is added to the reaction solution for dilution. Furthermore, 10.8 g (0.13 mol) of a 48% NaOH aqueous solution is added to neutralize 93% of the theoretical amount of carboxylic acid introduced by the reaction with succinic anhydride to prepare a sodium salt. Next, the resulting solution is added to 750 ml of methanol over a period of about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution is added, stirring is performed for 30 minutes, and the water-soluble polymer dispersed in the methanol is subjected to solid-liquid separation and recovery by vacuum filtration.

[0216] Next, in order to remove the unreacted succinic anhydride contained in the water-soluble polymer and the succinic acid generated by hydrolysis, the recovered water-soluble polymer was redispersed in 500 mL of methanol, stirred at room temperature for 30 minutes for washing, and then filtered under reduced pressure for solid-liquid separation to recover the water-soluble polymer again. The total acid value and free acid value of the obtained water-soluble polymer were measured, and the results confirmed that it was a partially neutralized product with a total acid value of 138 mgKOH / g and a free acid value of 37 mgKOH / g. The weight average molecular weight of the obtained water-soluble polymer was 3.7×10 6 , the dispersion is 13.8.

[0217] (Production Example 17)

[0218] 20.0 g of the powder of the starch partial hydrolyzate produced in Production Example 6 (0.36 mol of hydroxyl groups of the starch partial hydrolyzate) and 110 g of dimethyl sulfoxide (DMSO) were placed in a 300 ml detachable flask equipped with a stirrer, a thermometer, and a cooling tube to dissolve them. Then, 10.6 g of maleic anhydride (0.11 mol, 0.30 equivalents relative to the hydroxyl groups of the starch partial hydrolyzate) was added, and the mixture was stirred at 90°C to 95°C for 3 hours to react. The reaction solution after stirring was sampled and neutralized and titrated with 0.1 N NaOH. The acid value of the reaction solution was 70 mgKOH / g (theoretical end point acid value 43 mgKOH / g).

[0219] After the reaction was completed, the reaction solution was added to 2.5 L of acetone over about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, stirring was performed for 30 minutes, and the water-soluble polymer dispersed in acetone was separated into solid and liquid by vacuum filtration and recovered.

[0220] Next, in order to remove the unreacted maleic anhydride contained in the water-soluble polymer and the maleic acid generated by hydrolysis, the recovered water-soluble polymer was redispersed in 500 mL of acetone, stirred at room temperature for 30 minutes for washing, and then filtered under reduced pressure for solid-liquid separation to recover the water-soluble polymer again. The total acid value of the obtained water-soluble polymer was 90 mgKOH / g. The weight average molecular weight of the obtained water-soluble polymer was 3.1×10 6 , the dispersion is 39.6.

[0221] [Table 3]

[0222]

[0223] (4) Production of water-absorbent resin

[0224] (4-1) Method without partial neutralization

[0225] (Example 1)

[0226] 25 g (wet crystals) of the water-soluble polymer (wet product containing methanol with water, moisture content 67%) obtained in Preparation Example 9 was transferred to a petri dish and placed in a blower dryer set at 100° C. and dried for 20 hours to perform a crosslinking treatment. After the treatment, the obtained solid was pulverized in a mortar and sieved using sieves with mesh sizes of 150 μm and 850 μm to recover particles with a particle size of 150 μm to 850 μm.

[0227] (Examples 2 to 9, 13 and Comparative Examples 2 to 3)

[0228] The same operation as in Example 1 was carried out except that the raw materials and the charge amounts described in Table 4 were changed to obtain a water-absorbent resin.

[0229] (4-2) Partial Neutralization Method

[0230] (Example 10)

[0231] 25 g of the water-soluble polymer obtained in Preparation Example 12 (wet product containing methanol, wet ratio 71%) is put into a 300 ml beaker, and 100 ml of methanol containing methanol at a volume ratio of 80 / 20 (volume ratio) is further added to disperse the water-soluble polymer. While stirring with a magnetic stirrer, 1.1 ml of 1N hydrochloric acid is slowly added thereto with a graduated pipette. After adding the hydrochloric acid, stir for 15 minutes, perform vacuum filtration, and recover the water-soluble polymer partially neutralized by the free acid. The recovered water-soluble polymer is a wet crystal containing alcohol. The wet crystal is transferred to a plate, put into a blast dryer set at 70°C, dried for 20 hours, and cross-linked. The solid obtained after the mortar pulverization treatment is sieved using a sieve with a mesh size of 150 μm and 850 μm, and particles with a particle size of 150 μm to 850 μm are recovered.

[0232] (Examples 11 to 12 and Comparative Example 1)

[0233] The same operation as in Example 10 was carried out except that the raw materials and the charge amounts described in Table 4 were changed to obtain a water-absorbent resin.

[0234] (Example 14)

[0235] 25 g of the water-soluble polymer obtained in Preparation Example 15 (wet product of aqueous ethanol, wet ratio 61%) is put into a 300 ml beaker, and 80 ml of aqueous ethanol with ethanol / water = 90 / 10 (volume ratio) is further added to disperse the water-soluble polymer. While stirring with a magnetic stirrer, 12.1 ml of 1N hydrochloric acid is slowly added thereto with a graduated pipette. After adding hydrochloric acid, stir for 15 minutes, perform vacuum filtration, and recover the water-soluble polymer partially neutralized by the free acid. The recovered water-soluble polymer is wet crystals containing aqueous alcohol. The wet crystals are transferred to a plate, put into a blast dryer set at 150°C, dried for 1 hour, and cross-linked. The solid obtained after the mortar pulverization treatment is sieved using sieves with mesh sizes of 150 μm and 850 μm, and particles with a particle size of 150 μm to 850 μm are recovered.

[0236] (Example 16)

[0237] 20 g of the water-soluble polymer obtained in Preparation Example 17 (wet product containing aqueous acetone, wet ratio 61%) was put into a 300 ml beaker, and 60 ml of aqueous acetone with acetone / water = 90 / 10 (volume ratio) was further added to disperse the water-soluble polymer. While stirring with a magnetic stirrer, 19.3 ml of 1N NaOH was slowly added thereto with a graduated pipette. After adding the NaOH aqueous solution, the mixture was stirred for 15 minutes, and vacuum filtration was performed to recover the water-soluble polymer in which a part of the carboxylic acid introduced by maleic anhydride was neutralized as a sodium salt. The recovered water-soluble polymer is a wet crystal containing aqueous acetone. The wet crystal was transferred to a plate, put into a blast dryer set at 70°C, dried for 12 hours, and cross-linked. The solid obtained after the mortar pulverization treatment was sieved using a sieve with a mesh size of 150 μm and 850 μm, and particles with a particle size of 150 μm to 850 μm were recovered.

[0238] (4-3) Method for partial neutralization during synthesis of water-soluble polymer

[0239] (Example 15)

[0240] 25 g (wet crystals) of the water-soluble polymer (wet product containing methanol, moisture content 63%) obtained in Preparation Example 16 were transferred to a petri dish and placed in a blower dryer set at 70°C and dried for 12 hours to perform a crosslinking treatment. The solid obtained after the pulverization treatment was sieved using sieves with mesh sizes of 150 μm and 850 μm to recover particles with a particle size of 150 μm to 850 μm.

[0241] (5) Evaluation method of water-soluble polymers

[0242] (5-1) Total acid value of water-soluble polymer

[0243] Accurately weigh about 0.3g of a water-soluble polymer in a 100ml beaker and dissolve it in 40ml of ion exchange water. The aqueous solution is placed in a potentiometric titration apparatus (AT-610 manufactured by Kyoto Electronics Co., Ltd.) equipped with a glass electrode (C-171 manufactured by Kyoto Electronics Co., Ltd.). In the case where the sample is all sodium salt, at this stage, the potential is roughly displayed as less than 30mV, so 1N hydrochloric acid is added until the potential reaches more than 320mV, so that all the carboxylic acid groups in the water-soluble polymer become free acid states (become a state of excess hydrochloric acid). Confirm that the potential has reached more than 320mV, and neutralization titration is performed with a 0.1N NaOH aqueous solution. In this titration, two inflection points are detected, the first inflection point is detected near 220mV, and the second inflection point is detected near 0 to -30mV. The former is the neutralization point of the excess hydrochloric acid in the sample, and the latter is the neutralization point of the carboxylic acid in the water-soluble polymer. Therefore, the total acid value is calculated by the following formula 1.

[0244] Total acid value (mgKOH / g) = [{(Vb-Va)×0.1×fa×56.11}÷Sa] / (1-wr) (Formula 1)

[0245] Here, Va is the volume (ml) of 0.1N NaOH consumed until the first inflection point, Vb is the volume (ml) of 0.1N NaOH consumed until the second inflection point, fa is the titer of 0.1N NaOH, Sa is the sampling amount, and wr is the moisture content of the water-soluble polymer measured by the method described below.

[0246] (5-2) Free Acid Value of Water-Soluble Polymers When Cross-Linked Polymers Are Prepared After Acid Treatment or Alkali Treatment (Examples 10 to 12, Example 14, Example 16, Comparative Example 1)

[0247] Since a cross-linked polymer is produced subsequently after the acid treatment or the alkali treatment, it is difficult to directly quantify the amount by titration, and therefore the value calculated by the following calculation is defined as the free acid value.

[0248] In the case of acid treatment using an acid having a lower pKa than the carboxylic acid of the water-soluble polymer, the amount of acid added during the acid treatment is substantially equal to the free acid value. Therefore, the free acid value is calculated by the following formula 2.

[0249] Free acid value (mgKOH / g) = (Vc×N×fb×56.11)÷(Sb-Vc×N×fb×22) (Formula 2)

[0250] Here, Vc is the volume (ml) of the acid aqueous solution used in the acid treatment, N is the normality of the acid aqueous solution, fb is the titer of the acid aqueous solution, and Sb is the weight (pure content) of the water-soluble polymer introduced in the acid treatment.

[0251] When the alkali treatment is performed with sodium hydroxide, the free acid is in a form neutralized by the alkali, and therefore, it is calculated by the following formula 3.

[0252] Free acid value (mgKOH / g) = {(Tav÷56.11)×Sc-Vd×N×fc)÷(Sc+Vd×N×fc×22)}×56.11 (Formula 3)

[0253] Here, Tav is the total acid value of the water-soluble polymer (mgKOH / g), Vd is the volume (ml) of the sodium hydroxide aqueous solution used in the alkali treatment, N is the equivalent concentration of the sodium hydroxide aqueous solution, fc is the titer of the sodium hydroxide aqueous solution, and Sc is the weight (pure component) of the water-soluble polymer added in the alkali treatment.

[0254] (5-3) Free Acid Value of Water-Soluble Polymer When Partially Neutralized During Synthesis of Water-Soluble Polymer (Example 15)

[0255] In the method described in the above (5-1) Total Acid Value of Water-Soluble Polymer, neutralization titration is performed without adding 1N hydrochloric acid before titration. In this case, one inflection point is detected and calculated by the following formula 4.

[0256] Free acid value (mgKOH / g) = [Va×0.1×fa×56.11÷Sa] / (1-wr) (Formula 4)

[0257] Here, Va is the volume (ml) of 0.1N NaOH consumed until the inflection point, fa is the titer of 0.1N NaOH, Sa is the sampling amount, and Wr is the moisture content of the water-soluble polymer.

[0258] (5-4) Moisture content of water-soluble polymer

[0259] The moisture ratio refers to the ratio (%) of the weight reduction of the sample when it is dried at a drying temperature of 130°C using a halogen moisture meter relative to the initial weight of the sample. In this embodiment, 0.5 g to 1.0 g of a water-soluble polymer is placed in a halogen moisture meter HC103 manufactured by Mettler Toledo Co., Ltd., and the measurement is performed at a drying temperature of 130°C, a shutdown standard of 1 mg / 50 seconds, and a %MC mode (a mode in which the displayed MC value = (initial weight of the sample - drying weight) ÷ initial weight of the sample × 100). The displayed MC value is taken as the moisture ratio.

[0260] (5-5) Degree of etherification of water-absorbent polymer

[0261] Degree of etherification = (162×TAV) ÷ (56100-80×TAV)

[0262] Here, TAV is the total acid value (unit: mgKOH / g) of the water-soluble polymer.

[0263] (5-6) Biomass of water-soluble polymers

[0264] The biomass degree is the ratio (mass %) of elements derived from natural resources in the elements constituting the water-soluble polymer. The biomass degree is calculated using the following formula using the degree of etherification. It should be noted that in the water-absorbent resin obtained by partially neutralizing the water-soluble polymer and then drying it, the sodium salt is separated from the acidic group by partial neutralization, so the biomass degree is slightly increased.

[0265] ((molecular weight of glucose unit) - degree of etherification × 1) / ((molecular weight of glucose unit) + (degree of etherification × (molecular weight of acidic group - 1))) × 100

[0266] In the molecule of the above formula, the molecular weight of the starch monomer (glucose unit) is 162. Since hydrogen atoms are removed when the acidic group is introduced, the degree of etherification × 1 is subtracted.

[0267] In the denominator of the above formula, when the acidic group is carboxymethyl (sodium salt), the molecular weight is 81. When the acidic group is carboxyhexyl, the molecular weight is 137. Since hydrogen atoms are removed when the acidic group is introduced, the value obtained by subtracting 1 from the molecular weight is used.

[0268] (6) Evaluation method of water-absorbent resin

[0269] (6-1) Water absorption rate without pressure (normal saline)

[0270] 1.0 g of the test sample was added to a tea bag (20 cm long, 10 cm wide) made of a nylon net with a mesh size of 63 μm (JIS Z8801-1: 2006), immersed in 1,000 ml of saline (salt concentration 0.9 wt%) without stirring for 3 hours, and then hung for 10 minutes to remove water. The weight (h1) including the tea bag was measured, and the water retention was calculated by the following formula. It should be noted that the temperature of the saline solution and the measurement atmosphere used was 25°C ± 2°C.

[0271] FSC(g / g)=(h1)-(h2)

[0272] It should be noted that (h2) is the weight of the tea bag measured by the same operation as above without measuring the sample. Here, FSC is the abbreviation of Free Swell Capacity, which means free swelling ratio and water absorption ratio under no pressure.

[0273] (6-2) Water absorption rate without pressure (ion exchange water)

[0274] The weight (h1') including the tea bag after immersion was measured in the same manner as the water absorption ratio under no pressure (physiological saline) except that 0.2 g of the measurement sample was added to the tea bag and ion exchange water was used instead of the physiological saline, and the water retention was calculated from the following formula. It should be noted that (h2') is the weight of the tea bag measured by the same operation as above without the measurement sample.

[0275] FSC(g / g)={(h1')-(h2')} / 0.2

[0276] (6-3) Water retention rate (normal saline)

[0277] After the above-mentioned measurement of water absorption rate under no pressure, the tea bag is placed in a centrifuge and dehydrated at 150G for 90 seconds to remove the remaining liquid components. The weight (h3) including the tea bag is measured and the water retention is calculated by the following formula.

[0278] CRC(g / g)=(h3)-(h4)

[0279] It should be noted that (h4) is the weight of the tea bag measured by the same operation as above without measuring the sample. Here, CRC is the abbreviation of Centrifuge Retention Capacity, which means centrifuge retention capacity and water retention rate.

[0280] (6-4) Water retention rate (ion exchange water)

[0281] After the above-mentioned water absorption rate under no pressure is measured, the tea bag is placed in a centrifuge and dehydrated at 150G for 90 seconds to remove the remaining liquid components. The weight (h3') including the tea bag is measured and the water retention is calculated by the following formula.

[0282] CRC(g / g)={(h3')-(h4')} / 0.2

[0283] In addition, (h4') is the weight of the tea bag measured by the same operation as above without measuring the sample.

[0284] (6-5) Gel properties of water-absorbent resin

[0285] After the water retention test for physiological saline described in (6-3) was performed, the gel was taken out from the tea bag and the appearance of the gel was visually evaluated according to the following 6 stages. Figure 1 .

[0286] 1: Soluble in water

[0287] 2: Semi-soluble in water

[0288] 3: Insoluble in water and high in water content

[0289] 4: Insoluble in water and slightly more water

[0290] 5: Insoluble in water and soft

[0291] 6: Insoluble in water and strong

[0292] (6-6) Alkali decomposition

[0293] 0.5 g of water-absorbent resin and 9.5 g of 1% NaOH aqueous solution were weighed into a screw-capped tube bottle with a capacity of 13.5 ml, and stirred for 60 minutes using a mixing rotor to dissolve. Next, a 30-mesh metal mesh (mesh size 500 μm) of about 50 mm × 50 mm square was prepared, and the weight of the metal mesh (Wm1) was measured. The mixed solution was naturally filtered using the metal mesh whose weight was measured, and after filtration, the mesh was washed with about 5 ml of ion exchange water. After washing, the metal mesh was dried in a 120°C air dryer for 2 hours, and the weight of the metal mesh after drying (Wm2) was measured, and the 30-mesh sieve residue was calculated by the following formula. When the water-absorbent resin is completely dissolved, the 30-mesh sieve residue is 0%, and when it is not dissolved and gel remains, the 30-mesh sieve residue exceeds 0%.

[0294] 30 mesh sieve residue (%) = (Wm2 - Wm1) / 0.5 × 100

[0295] (7) Evaluation of water-absorbent resin

[0296] The water absorption performance and gel properties of each of the water-absorbent resins obtained in Examples 1 to 16 and Comparative Examples 1 to 3 were evaluated.

[0297]

[0298] In Comparative Examples 1 to 3, the solid content of the water-soluble polymer when dried was less than 90%, so no gelation was observed and no water absorption performance was observed. In Examples 1 to 16, by making the solid content of the water-soluble polymer when dried 90% or more, a water-insoluble water-absorbent resin was obtained and sufficient water absorption performance was achieved.

[0299] (8) Production of Partially Degraded Products of Processed Starch (Production Examples 18 to 22)

[0300] The partially decomposed product of the processed starch was produced by the following method. Table 5 shows the weight average molecular weight and the degree of dispersion of the partially decomposed product.

[0301] (Production Example 18) Partially Decomposed Starch from Acetic Acid Tapioca Starch

[0302] After suspending acetic cassava starch in tap water at a concentration of 45% (w / w), 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To the starch milk, 3 units of amylomaltase crude enzyme solution were added per 1 gram of starch solid matter, and after stirring at room temperature for 30 minutes, the mixture was reacted at 90°C for 5 hours under stirring.

[0303] (Production Example 19) Partially Decomposed Starch from Oxidized Acetylated Tapioca Starch

[0304] Oxidized acetylated tapioca starch was suspended in tap water at a concentration of 45% (w / w), and 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. A crude amylomaltase enzyme solution was added to the starch milk at a rate of 3 units per 1 gram of starch solid matter, and the mixture was stirred at room temperature for 30 minutes and then reacted at 90°C for 5 hours under stirring.

[0305] (Production Example 20) Partially Decomposed Starch from Acetylated Tapioca Starch

[0306] Oxidized acetylated cassava starch was suspended in tap water at a concentration of 45% (w / w), and 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To the starch milk, 5 units of amylomaltase crude enzyme solution were added per 1 gram of starch solid matter, and after stirring at room temperature for 30 minutes, the mixture was reacted at 90°C for 5 hours with stirring.

[0307] (Production Example 21) Partially Degraded Starch from Hydroxypropylated Starch

[0308] Hydroxypropyl starch was suspended in tap water at a concentration of 45% (w / w), and 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To the starch milk, 3 units of amylomaltase crude enzyme solution were added per 1 gram of starch solid matter, and after stirring at room temperature for 30 minutes, the mixture was reacted at 90°C for 5 hours with stirring.

[0309] (Production Example 22) Partially Degraded Starch from Hydroxypropylated Phosphate-Crosslinked Starch

[0310] Hydroxypropylated phosphate cross-linked starch was suspended in tap water at a concentration of 30% (w / w), and 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. A crude amylomaltase enzyme solution was added to the starch milk at a rate of 3 units per 1 gram of starch solid matter, and the mixture was stirred at room temperature for 30 minutes and then reacted at 90°C for 5 hours under stirring.

[0311] [Table 5]

[0312] Production Example 18 Production Example 19 Production Example 20 Production Example 21 Production Example 22 Mw(million) 465 62 456 256 204 Dispersion 19.1 7.4 8.9 8.1 8.4

[0313] (9) Production of water-soluble polymers

[0314] (Production Example 23)

[0315] 100 g of a 45 wt% aqueous solution of the starch partial hydrolyzate produced in Production Example 18 (0.83 mol of hydroxyl groups of the starch partial hydrolyzate) was placed in a 500 ml removable flask equipped with a stirrer, a thermometer, and a cooling tube. Next, 34.4 g of a 48.8% sodium hydroxide aqueous solution (0.42 mol, 0.5 equivalents relative to the hydroxyl groups of the starch partial hydrolyzate) was added, and the mixture was stirred at 60°C or below until the solution was completely uniform. After confirming that the solution was uniform, an aqueous solution prepared by dissolving 18.9 g of monochloroacetic acid (0.2 mol, 0.2 equivalents relative to the hydroxyl groups of the starch partial hydrolyzate) in 25 g of ion exchange water was added dropwise at 50°C to 60°C for 30 minutes. After the monochloroacetic acid aqueous solution was added, the temperature was adjusted to 45°C to 50°C, and the mixture was stirred for 10 hours. Regarding the end point of the reaction, the reaction solution was sampled and the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01N silver nitrate solution, with the condition that the chloride ion content reached 98% or more of the calculated value of 4.0% when the monochloroacetic acid was completely reacted. In this production example, the chloride content was 4.0%.

[0316] After the reaction was completed, the reaction solution was diluted with 400 g of ion exchange water. The diluted reaction solution was cooled to room temperature and added to 5 L of methanol over a period of about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by vacuum filtration.

[0317] Next, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 1L of aqueous methanol with a methanol / water ratio of 80 / 20 (volume ratio), stirred at room temperature for 30 minutes for washing, and then the solid-liquid separation was performed by vacuum filtration to recover the water-soluble polymer again. The chlorine content of the recovered water-soluble polymer was determined by potentiometric titration using a 0.01N silver nitrate solution, and the washing process was repeated until the chlorine content was less than 1%. The total acid value of the obtained water-soluble polymer was 146 mgKOH / g, and the degree of etherification calculated from the total acid value was 0.53. In addition, the weight-average molecular weight was 18.6×10 6 , the dispersion is 19.7.

[0318] (Production Examples 24 to 27)

[0319] A water-soluble polymer was produced in the same manner as in Production Example 23 except that the raw materials, input amounts and reaction conditions were changed to those shown in Table 6. Table 6 shows the total acid value, degree of etherification, weight average molecular weight and dispersion of the obtained water-soluble polymer.

[0320] [Table 6]

[0321]

[0322] (10) Production of water-absorbent resin

[0323] (Example 17)

[0324] 25 g of the water-soluble polymer obtained in Preparation Example 23 (wet product containing methanol, wet ratio 65%) is placed in a 300 ml beaker, and 120 ml of methanol containing methanol / water = 80 / 20 (volume ratio) is further added to disperse the water-soluble polymer. While stirring with a magnetic stirrer, 0.8 ml of 1N hydrochloric acid is slowly added thereto with a graduated pipette. After adding hydrochloric acid, stir for 15 minutes, perform vacuum filtration, and recover the water-soluble polymer partially neutralized by the free acid. The recovered water-soluble polymer is wet crystals containing alcohol. The wet crystals are transferred to a plate, placed in a blast dryer set at 70°C, dried for 12 hours, and cross-linked. The solid obtained after the mortar pulverization treatment is sieved using sieves with mesh sizes of 150 μm and 850 μm, and particles with a particle size of 150 μm to 850 μm are recovered.

[0325] (Examples 18 to 25)

[0326] A water-absorbent resin was obtained by the same operation as in Example 17 except that the raw materials, input amounts and reaction conditions were changed to those shown in Table 7. Table 7 shows the free acid value, water absorption performance, gel properties and alkali decomposition properties of each water-absorbent resin.

[0327]

[0328] In Examples 17 to 25 using modified starch as a raw material, by setting the solid content of the water-soluble polymer at the time of drying to 90% or more, a water-insoluble water-absorbent resin can be obtained, and sufficient water-absorbing performance can be achieved.

[0329] (Production Example 28) Partially decomposed starch from cassava starch (1)

[0330] After suspending cassava starch in tap water at a concentration of 45% (w / w), 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To the starch milk, 8.0 units of amylomaltase crude enzyme solution were added per 1 gram of starch solid matter, and after stirring at room temperature for 30 minutes, the mixture was reacted at 95°C for 6 hours under stirring to prepare liquefied starch. The weight average molecular weight of the obtained starch partial decomposition product was 2.61 million, and the dispersion degree was 7.9.

[0331] (Production Example 29) Production of Water-Soluble Polymer from Tapioca Starch (1)

[0332] 100 g of a 45 wt% aqueous solution of the starch partial decomposition product from cassava starch obtained in Preparation Example 28 (0.83 mol of hydroxyl groups of the starch partial decomposition product) was placed in a 500 ml separable flask equipped with a stirrer, a thermometer, and a cooling tube. Next, 34.0 g of a 48.8% sodium hydroxide aqueous solution (0.42 mol, 0.50 molar equivalent to 1 mol of hydroxyl groups of the starch partial decomposition product) was added, and the mixture was stirred at 60°C or below until the solution was completely uniform. After confirming that the solution was uniform, an aqueous solution prepared by dissolving 19.8 g of monochloroacetic acid (0.21 mol, 0.3 molar equivalent to 1 mol of hydroxyl groups of the starch partial decomposition product) in 50 g of ion exchange water was added dropwise at 50°C to 60°C for 30 minutes. After the monochloroacetic acid aqueous solution was added, the temperature was adjusted to 45°C to 50°C, and the mixture was stirred for 12 hours. Regarding the end point of the reaction, the reaction solution was sampled and the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01N silver nitrate aqueous solution, with the condition that the chloride ion content reached 98% or more of the calculated value of 3.7% when the monochloroacetic acid was completely reacted. In this production example, the chloride content was 3.7%.

[0333] After the reaction was completed, the reaction solution was diluted with 900 g of ion exchange water. The diluted reaction solution was cooled to room temperature and added to 6000 ml of methanol over a period of about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by filtration under reduced pressure.

[0334] Next, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer is redispersed in 1000 ml of aqueous methanol with a methanol / water ratio of 80 / 20 (volume ratio), stirred at room temperature for 30 minutes for washing, and then filtered under reduced pressure for solid-liquid separation to recover the water-soluble polymer again. The chlorine content of the recovered water-soluble polymer is determined by potentiometric titration using a 0.01N silver nitrate aqueous solution, and the washing process is repeated until the chlorine content is less than 1%. The total acid value of the obtained water-soluble polymer is 130 mgKOH / g, the degree of etherification calculated from the total acid value is 0.46, the weight-average molecular weight is 8.12 million, the dispersion is 13.7, and the biomass degree is 81%.

[0335] (Production Example 30) Production of Water-Soluble Polymer from Tapioca Starch (2)

[0336] 95 g of a 45 wt% aqueous solution of the starch partial decomposition product from cassava starch obtained in Preparation Example 28 (0.79 mol of hydroxyl groups of the starch partial decomposition product) and 2.5 g of cassava starch (2.2 g of pure components of cassava starch, 0.04 mol of hydroxyl groups of cassava starch) were placed in a 500 ml separable flask equipped with a stirrer, a thermometer, and a cooling tube. Next, 34.0 g of a 48.8% sodium hydroxide aqueous solution (0.42 mol, 0.50 molar equivalent to 1 mol of hydroxyl groups of the starch partial decomposition product) was added, and the mixture was stirred at 60°C or below until the solution was completely uniform. After confirming that the solution was uniform, an aqueous solution prepared by dissolving 19.8 g of monochloroacetic acid (0.21 mol, 0.3 molar equivalent to 1 mol of hydroxyl groups of the starch partial decomposition product) in 50 g of ion exchange water was added dropwise at 50°C to 60°C for 30 minutes. After the monochloroacetic acid aqueous solution was added, the temperature was adjusted to 45°C to 50°C, and the mixture was stirred for 12 hours. Regarding the end point of the reaction, the reaction solution was sampled and the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01N silver nitrate aqueous solution, with the condition that the chloride ion content reached 98% or more of the calculated value of 3.7% when the monochloroacetic acid was completely reacted. In this production example, the chloride content was 3.7%.

[0337] After the reaction was completed, the reaction solution was diluted with 900 g of ion exchange water. The diluted reaction solution was cooled to room temperature and added to 6000 ml of methanol over a period of about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by filtration under reduced pressure.

[0338] Next, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer is redispersed in 1000 ml of aqueous methanol with a methanol / water ratio of 80 / 20 (volume ratio), stirred at room temperature for 30 minutes for washing, and then filtered under reduced pressure for solid-liquid separation to recover the water-soluble polymer again. The chlorine content of the recovered water-soluble polymer is determined by potentiometric titration using a 0.01N silver nitrate aqueous solution, and the washing process is repeated until the chlorine content is less than 1%. The total acid value of the obtained water-soluble polymer is 132 mgKOH / g, the degree of etherification calculated from the total acid value is 0.47, the weight-average molecular weight is 8.05 million, the dispersion is 14.7, and the biomass degree is 81%.

[0339] (Production Example 31) Partially decomposed starch from cassava starch (2)

[0340] After suspending cassava starch in tap water at a concentration of 45% (w / w), 1N sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To the starch milk, 4.0 units of amylomaltase crude enzyme solution were added per 1 gram of starch solid matter, and after stirring at room temperature for 30 minutes, the mixture was reacted at 85°C for 5 hours under stirring to prepare liquefied starch. The weight average molecular weight of the obtained starch partial decomposition product was 4.01 million, and the dispersity was 14.1.

[0341] (Production Example 32) Production of Water-Soluble Polymer from Tapioca Starch (3)

[0342] 100 g of a 45 wt% aqueous solution of the starch partial decomposition product from cassava starch obtained in Preparation Example 31 (0.83 mol of hydroxyl groups of the starch partial decomposition product) was placed in a 500 ml separable flask equipped with a stirrer, a thermometer, and a cooling tube. Next, 59.5 g of a 48.8% sodium hydroxide aqueous solution (0.73 mol, 0.87 molar equivalent to 1 mol of hydroxyl groups of the starch partial decomposition product) was added, and the mixture was stirred at 60°C or below until the solution was completely uniform. After confirming that the solution was uniform, an aqueous solution prepared by dissolving 32.7 g of monochloroacetic acid (0.35 mol, 0.4 molar equivalent to 1 mol of hydroxyl groups of the starch partial decomposition product) in 80 g of ion exchange water was added dropwise at 50°C to 60°C for 30 minutes. After the monochloroacetic acid aqueous solution was added, the temperature was adjusted to 45°C to 50°C, and the mixture was stirred for 12 hours. Regarding the end point of the reaction, the reaction solution was sampled and the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01N silver nitrate aqueous solution, with the condition that the chloride ion content reached 98% or more of the calculated value of 4.6% when the monochloroacetic acid was completely reacted. In this production example, the chloride content was 4.6%.

[0343] After the reaction was completed, the reaction solution was diluted with 1000 g of ion exchange water. The diluted reaction solution was cooled to room temperature and added to 7000 ml of methanol over a period of about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by filtration under reduced pressure.

[0344] Next, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer is redispersed in 1000 ml of aqueous methanol with a methanol / water ratio of 80 / 20 (volume ratio), stirred at room temperature for 30 minutes for washing, and then filtered under reduced pressure for solid-liquid separation to recover the water-soluble polymer again. The chlorine content of the recovered water-soluble polymer is determined by potentiometric titration using a 0.01N silver nitrate aqueous solution, and the washing process is repeated until the chlorine content is less than 1%. The total acid value of the obtained water-soluble polymer is 179 mgKOH / g, the degree of etherification calculated from the total acid value is 0.69, the weight-average molecular weight is 9.6 million, the dispersion is 36.7, and the biomass degree is 74%.

[0345] (Example 26) Production of liquid-absorbing resin

[0346] 25 g of the water-soluble polymer obtained in Preparation Example 29 (wet product containing methanol, moisture content 65%) was placed in a 500 ml beaker, and 200 ml of methanol containing methanol in a volume ratio of 80 / 20 (volume ratio) was further added to disperse the water-soluble polymer. While stirring with a magnetic stirrer, 1.7 ml of a 1N hydrochloric acid aqueous solution was slowly added thereto using a graduated pipette. After adding hydrochloric acid, the mixture was stirred for 1 hour, and vacuum filtered to recover the water-soluble polymer partially neutralized by the free acid. The recovered water-soluble polymer was wet crystals containing alcohol. The wet crystals were transferred to a plate, placed in a blast dryer set at 70°C, and dried for 20 hours to perform a crosslinking treatment. The solid obtained after the pulverization treatment was sieved using a sieve with a mesh size of 150 μm and 850 μm to recover particles of a liquid-absorbing resin with a particle size of 150 μm to 850 μm.

[0347] (Example 27) Production of liquid-absorbing resin

[0348] The same operation as in Example 26 was carried out except that the 1N hydrochloric acid aqueous solution was changed to 0.23 g of DL-malic acid, and the water-absorbent resin particles were recovered.

[0349] (Example 28) Production of liquid-absorbing resin

[0350] The same operation as in Example 26 was carried out except that the water-soluble polymer was changed to 25 g of the water-soluble polymer obtained in Production Example 30 (a wet product containing methanol containing water, moisture ratio 66%) to recover water-absorbent resin particles.

[0351] (Example 29) Production of liquid-absorbing resin

[0352] The water-soluble polymer was changed to 20 g of the water-soluble polymer obtained in Preparation Example 32 (wet product containing methanol with a moisture content of 69%), and the 1N hydrochloric acid aqueous solution was changed to 0.7 ml. The mixture was placed in a blower dryer set at 85° C. and dried for 10 hours to perform a cross-linking treatment. The same operations as in Example 26 were carried out to recover the water-absorbent resin particles.

[0353] [Table 8]

[0354]

[0355] In Examples 26 to 27 and 29 using cassava starch as a raw material, by making the solid content of the water-soluble polymer at the time of drying 90% or more, a water-insoluble water-absorbent resin can be obtained, and sufficient water absorption performance can be achieved. In Example 28, a starch partial decomposition product from cassava starch (Production Example 28) is mixed with undecomposed cassava starch, and then an acidic group is introduced to prepare a water-soluble polymer (Production Example 30). As a result, the water-absorbent resin shows a high water absorption capacity (FSC) for ion-exchanged water without pressure.

Claims

1. A method for producing a water-absorbent resin that forms a physical gel by absorbing water, comprising: A step (a1) of reducing the molecular weight of starch to obtain a partially decomposed product of starch; a step (a2) of introducing an acidic group into the partial decomposition product of starch obtained in the step (a1) to obtain a water-soluble polymer; and A step (a3) ​​of drying the water-soluble polymer at 70°C to 180°C in the presence of water until the solid content reaches 90% or more.

2. The method for producing a water-absorbent resin according to claim 1, wherein The method further includes a step (aa) of desalting the water-soluble polymer after the step (a2).

3. The method for producing a water-absorbent resin according to claim 1 or 2, wherein: In the step (a2), or after the step (a2) and before the step (a3), The process comprises the steps (ab) of partially neutralizing the acidic groups of the water-soluble polymer.

4. The method for producing a water-absorbent resin according to claim 1 or 2, wherein: After the step (a2) and before the step (a3), The process of partially neutralizing the acidic groups of the water-soluble polymer is not included.

5. The method for producing a water-absorbent resin according to any one of claims 1 to 4, wherein In the step (a3), drying is performed until the solid content reaches 90% or more and 99% or less.

6. The method for producing a water-absorbent resin according to any one of claims 1 to 5, wherein The acidic group is a carboxyalkyl group, a carboxyalkenyl group or a sulfoalkyl group.

7. The method for producing a water-absorbent resin according to any one of claims 1 to 6, wherein In the step (a1), a partial decomposition product of starch having a weight average molecular weight Mw of 7.5 million or less and / or a dispersion degree of 5 or more is obtained, wherein the dispersion degree is the weight average molecular weight Mw / the number average molecular weight Mn.

8. The method for producing a water-absorbent resin according to any one of claims 1 to 7, wherein In the step (a1), the molecular weight of starch is reduced by enzyme treatment.

9. The method for producing a water-absorbent resin according to any one of claims 1 to 8, wherein In the step (a2), an acidic group is introduced into a mixture of the partial decomposition product of starch obtained in the step (a1) and the starch whose molecular weight has not been reduced.

10. The method for producing a water-absorbent resin according to any one of claims 1 to 9, wherein The water-soluble polymer obtained in the step (a2) has a pullulan-equivalent weight average molecular weight Mw of 500,000 to 40,000,000 as measured by aqueous size exclusion chromatography.

11. The method for producing a water-absorbent resin according to any one of claims 1 to 10, wherein The obtained water-absorbent resin has the following characteristics: (a) the water absorption capacity of ion exchange water without pressure is 100 g / g to 500 g / g; (b) The water retention rate of ion exchange water is 80g / g to 300g / g; (c) a water absorption capacity of 10 g / g to 70 g / g for physiological saline without pressure; and / or (d) The water retention rate of physiological saline is 5g / g to 65g / g.