Polyvinyl alcohol film and method for producing same
By using PVA films with a specific range of swelling and water absorption speed and performing heat treatment, the problems of PVA film fracture and optical performance degradation under high-speed stretching conditions are solved, and efficient and excellent polarizing film manufacturing is achieved.
Patent Information
- Application Number
- CN202380029176.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-22
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, when manufacturing polarizing films, the PVA film is prone to fracture under high-speed stretching conditions, wrinkles and optical performance deteriorates, resulting in poor manufacturing efficiency and optical performance.
The PVA film with a swelling degree of 195-205% and an average water absorption rate of 1.35%/second was used, and the swelling ratio and water absorption performance of the film were adjusted to reduce fractures and wrinkles by heat treatment on a drum of 50-120°C. , improve optical performance.
Under high-speed stretching conditions, the breakage of the PVA film is reduced, the optical performance of the polarizing film is improved, and efficient manufacturing is achieved.
Smart Images

Figure BDA0005052420430000181 
Figure BDA0005052420430000182 
Figure BDA0005052420430000183
Abstract
Description
Technical Field
[0001] The present invention relates to a polyvinyl alcohol film and a method for producing the same. Background Art
[0002] Polarizing plates that transmit and block light are the basic components of liquid crystal displays (LCDs) along with liquid crystals that change the polarization state of light. LCDs are used in a wide range of applications, including small devices such as calculators and watches, notebook computers, LCD monitors, LCD color projectors, LCD TVs, car navigation systems, mobile phones, and indoor and outdoor measuring equipment.
[0003] Polarizers are generally manufactured by dyeing a polyvinyl alcohol film (hereinafter, "polyvinyl alcohol" is sometimes abbreviated as "PVA"), uniaxially stretching it, and, if necessary, further performing a fixing treatment using a boron compound to manufacture a polarizing film, and then laminating a protective film such as a triacetyl cellulose (TAC) film to the surface of the polarizing film. Optical properties such as contrast of LCDs depend to a large extent on polarization properties such as the polarization degree of the polarizing film, so in order to improve the polarization performance, a PVA film with high stretchability has been proposed.
[0004] For example, Patent Document 1 describes a PVA film having a swelling degree of 190 to 230% and a thickness of less than 40 μm as a PVA film that can reduce the generation of wrinkles during stretching, has low tensile stress, reduces breakage during stretching, and can produce a thin polarizing film with a high yield. The swelling degree of the PVA film after being stretched to a stretching ratio of 3 times in water at 30°C is greater than 260%.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2014 / 050697 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In recent years, due to the increase in demand for LCDs, it is required to efficiently manufacture polarizing films as one of the components. In order to improve the manufacturing efficiency of polarizing films, it is considered to use wide PVA films to manufacture polarizing films or to adopt high-speed stretching conditions when manufacturing polarizing films. However, in the former method, a huge equipment investment is required for the construction or transformation of manufacturing equipment for PVA films and polarizing films, which is not economically preferred. On the other hand, in the latter method, even if the stretching ratio is the same as before, the breakage of the PVA film during stretching often occurs, which is prone to reduce the manufacturing efficiency of the polarizing film. It is speculated that this is because the PVA film cannot meet the rapid increase in strain rate accompanied by the high-speed stretching conditions when manufacturing polarizing films. As a countermeasure, by lowering the softening point temperature of the PVA film or increasing the stretching temperature when manufacturing the polarizing film, the breakage of the PVA film can be reduced even under high-speed stretching conditions. However, in these methods, abnormalities such as wrinkles on the PVA film during stretching and folds on the ends of the polarizing film are prone to occur, and the optical performance of the manufactured polarizing film is also prone to decrease.
[0010] The inventors of the present invention have conducted research and found that even for the PVA film described in Patent Document 1, when a high-speed stretching condition is used in the manufacture of a polarizing film, it is sometimes difficult to sufficiently reduce the breakage of the PVA film during stretching. In addition, it is sometimes difficult to sufficiently reduce the wrinkles of the PVA film during stretching, the folds at the ends, and the reduction in the optical performance of the polarizing film.
[0011] The present invention is made to solve the above-mentioned problems, and its purpose is to provide a PVA film and a method for manufacturing the same, wherein the PVA film can reduce breakage even under high-speed stretching conditions when manufacturing a polarizing film and can obtain a polarizing film with excellent optical properties.
[0012] Solutions to Solve Problems
[0013] The present inventors have conducted diligent research and found that the above-mentioned problems can be solved by using a PVA film having a swelling ratio and an average water absorption rate within a specific range measured under specified conditions. Based on this finding, the present invention was completed after further repeated research.
[0014] That is, the present invention relates to the following [1] to [7].
[0015] [1] A PVA film having a swelling degree (A) of 195 to 205% by mass, wherein a value obtained by dividing a swelling degree (B) after stretching 2.5 times in water at 30°C at a stretching rate of 240% / min by the swelling degree (A) is 1.27 to 1.40, wherein the average water absorption rate when immersed in water at 30°C for 30 seconds is 1.35% by mass / second or more;
[0016] [2] The PVA film according to [1], wherein the dimensional change rate in the width direction when immersed in water at 30° C. for 30 seconds is 14.6 to 16.2%;
[0017] [3] The PVA film according to [1] or [2], wherein the film has a thickness of 45 to 80 μm;
[0018] [4] The PVA film according to any one of [1] to [3], which is an optical film;
[0019] [5] The method for producing a PVA film according to any one of [1] to [3], wherein a film-forming stock solution containing PVA is cast onto a roller or a belt heated to 50 to 99° C. and dried, wherein after the PVA film is dried until the content of the plasticizer component is 20 to 23% by mass, the PVA film is heat-treated on a roller or a belt heated to 100 to 120° C.;
[0020] [6] The method for producing a PVA film according to [5], wherein the heat treatment is performed on a drum heated to 100 to 120° C.;
[0021] [7] The method for producing a PVA film according to [5] or [6], wherein the plasticizing component consists of water and a plasticizer, and the plasticizer is at least one selected from glycerol, diglycerol and propylene glycol.
[0022] Effects of the Invention
[0023] According to the present invention, a PVA film and a method for producing the same can be provided, wherein the PVA film can reduce breakage even under high-speed stretching conditions when producing a polarizing film and can obtain a polarizing film having excellent optical properties. DETAILED DESCRIPTION
[0024] <PVA film>
[0025] For the PVA film of the present invention, the swelling degree (A) is 195 to 205% by mass, and the value obtained by dividing the swelling degree (B) after stretching to 2.5 times at a stretching speed of 240% / min in water at 30°C by the above swelling degree (A) (hereinafter sometimes abbreviated as swelling degree ratio (B / A)) is 1.27 to 1.40, and the average water absorption rate of the PVA film when immersed in water at 30°C for 30 seconds is more than 1.35% by mass / second.
[0026] In the PVA film of the present invention, the swelling degree (A) is 195 to 205% by mass. The swelling degree (A) is an index indicating the water retention capacity of the PVA film when immersed in water at 30°C, and is an index that can be obtained as a percentage by dividing the mass of the PVA film directly (without stretching) immersed in water at 30°C for 30 minutes by the mass after drying at 105°C for 16 hours after immersion. Specifically, it can be measured by the method described in the following examples.
[0027] If the swelling degree (A) is less than 195% by mass, when the polarizing film is manufactured under high-speed stretching conditions, the stress applied to the PVA film during stretching becomes high, and the PVA film is prone to breakage. On the other hand, if the swelling degree (A) exceeds 205% by mass, when the polarizing film is manufactured under high-speed stretching conditions, there is a tendency for wrinkles to form on the PVA film during stretching and the optical properties of the resulting polarizing film to decrease. The swelling degree (A) is preferably 198% by mass or more, more preferably 199% by mass or more, and preferably 203% by mass or less, more preferably 201% by mass or less.
[0028] In the PVA film of the present invention, the value obtained by dividing the swelling degree (B) after stretching to a stretch ratio of 2.5 times at a stretching speed of 240% / min in water at 30°C by the aforementioned swelling degree (A), that is, the swelling ratio (B / A) is 1.27 to 1.40. Here, the swelling degree (B) is an index representing the water retention capacity of the PVA film after the PVA film is stretched to a stretch ratio of 2.5 times in water at 30°C, and can be obtained as a percentage by dividing the mass of the film after the PVA film is stretched to a stretch ratio of 2.5 times at a stretching speed of 240% / min in water at 30°C by the mass of the film after drying at 105°C for 16 hours after stretching. Specifically, it can be measured by the method described in the following examples. It should be noted that the stretch ratio (2.5 times) when measuring the swelling degree (B) is equivalent to the stretch ratio at the initial stage of stretching when manufacturing the polarizing film. Therefore, it is believed that by making the swelling degree (B) measured under such conditions larger than the swelling degree (A), that is, the swelling degree ratio (B / A) is 1.27 to 1.40, the PVA film can easily absorb water and stretch from the initial stage of stretching when manufacturing the polarizing film, and the breakage of the PVA film can be reduced even under high-speed stretching conditions.
[0029] If the swelling ratio (B / A) is less than 1.27, when the polarizing film is manufactured under high-speed stretching conditions, the stress applied to the PVA film during stretching becomes high, and the PVA film is prone to breakage. On the other hand, if the swelling ratio (B / A) exceeds 1.40, when the polarizing film is manufactured under high-speed stretching conditions, there is a tendency that wrinkles are easily generated on the PVA film during stretching, and the optical properties of the resulting polarizing film are reduced. The swelling ratio (B / A) is preferably 1.29 or more, more preferably 1.30 or more, and preferably 1.35 or less, more preferably 1.33 or less.
[0030] In the PVA film of the present invention, the average water absorption rate when immersed in water at 30°C for 30 seconds is 1.35 mass% / second or more. The average water absorption rate is an index of the water absorption rate at the initial stage of immersion in water, and can be obtained by subtracting the moisture content before immersion from the moisture content after immersion of the PVA film in water at 30°C for 30 seconds, and dividing by the immersion time. Specifically, it can be measured by the method described in the following examples.
[0031] Since the PVA film of the present invention has an average water absorption rate of 1.35 mass% / second or more and is large enough, if it is stretched in various water baths in the manufacturing process of the polarizing film, part of the lamellar crystals of PVA in the PVA film are easily untied and amorphized. As a result, since the swelling degree of the PVA film becomes easier to increase than before stretching, it is believed that the breakage of the PVA film is reduced even under high-speed stretching conditions when manufacturing the polarizing film. In addition, since the PVA film of the present invention has an average water absorption rate of 1.35 mass% / second or more and is large enough, it is easy to absorb boric acid contained in the stretching bath, etc. in the manufacturing process of the polarizing film. As a result, it is easy to form a foothold for the iodine complex that shows polarization performance, so it is believed that the optical properties of the resulting polarizing film are maintained. The average water absorption rate is preferably 1.36 mass% / second or more, more preferably 1.38 mass% / second or more, and preferably 1.44 mass% / second or less, more preferably 1.42 mass% / second or less. By setting the average water absorption rate to be below the upper limit, wrinkles generated in the PVA film during stretching can be further reduced even under high-speed stretching conditions when producing a polarizing film, and deterioration in the optical performance of the resulting polarizing film can be easily prevented.
[0032] The dimensional change rate in the width direction (a direction perpendicular to the mechanical flow direction; hereinafter abbreviated as TD) of the PVA film of the present invention when immersed in water at 30°C for 30 seconds is preferably in the range of 14.6 to 16.2%. The dimensional change rate in water can be obtained by calculating the ratio [100×(BA) / A], which is the ratio of the value obtained by subtracting the distance between the markings A in the width direction of the film before immersion from the distance between the markings B in the width direction of the film after the PVA film is immersed in water at 30°C for 30 seconds to the distance between the markings A in the width direction of the film before immersion. Specifically, it can be measured by the method described in the following embodiments. From the viewpoint of process passability, the dimensional change rate in water is more preferably 14.8% or more, more preferably 15.0% or more, and more preferably 15.8% or less, and more preferably 15.6% or less. It should be noted that, in general, when the PVA film is continuously formed into a film, periodic or continuous thickness and delay unevenness will occur in the mechanical flow direction and the width direction. By observing this unevenness, the mechanical flow direction / width direction of the PVA film can be identified even if the film sample is not a long one.
[0033] The PVA film of the present invention is preferably immersed in pure water at 30° C. for 8 seconds and then uniaxially stretched in the longitudinal direction at a stretching rate of 480% / min to have a tensile stress of 14.5 to 17.0 N / mm 2 Specifically, the tensile stress can be measured by the method described in the examples described later. By making the tensile stress 14.5N / mm 2 The above can improve the optical performance of the obtained polarizing film. From this point of view, the tensile stress is more preferably 14.7 N / mm 2 More preferably, 14.9 N / mm 2 Above, particularly preferably 15.1 N / mm 2 On the other hand, by setting the tensile stress to 17.0 N / mm 2 Next, when the polarizing film is manufactured under high-speed stretching conditions, the occurrence of PVA film breakage during stretching can be reduced. From this point of view, the tensile stress is more preferably 16.8 N / mm 2 Below, more preferably 16.7 N / mm 2 Below, particularly preferably 16.6 N / mm 2 the following.
[0034] [PVA]
[0035] As the PVA constituting the PVA film of the present invention, for example, PVA obtained by the following method can be cited, that is, one or more of vinyl esters such as vinyl acetate, vinyl formate, vinyl propionate, vinyl butyrate, vinyl pivalate, vinyl neodecanoate (versatic acid) vinyl ester, vinyl laurate, vinyl stearate, vinyl benzoate, isopropenyl acetate, etc. are polymerized to obtain polyvinyl ester, and the obtained polyvinyl ester is saponified to obtain PVA. Among these vinyl esters, vinyl acetate is preferably used from the viewpoints of ease of manufacture, ease of acquisition, cost, etc. of PVA.
[0036] The polyvinyl ester is preferably a substance obtained by using only one or two or more vinyl esters as a monomer, more preferably a substance obtained by using only one vinyl ester as a monomer, and may also be a copolymer of one or two or more vinyl esters and other monomers copolymerizable therewith within a range not impairing the effects of the present invention.
[0037] Examples of other monomers copolymerizable with vinyl esters include α-olefins having 2 to 30 carbon atoms, such as ethylene, propylene, 1-butene, and isobutylene; (meth)acrylic acid or its salts; (meth)acrylic acid esters, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate; (meth)acrylamide, N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, (Meth)acrylamide derivatives such as N,N-dimethyl(meth)acrylamide, diacetone(meth)acrylamide, (meth)acrylamidepropanesulfonic acid or its salts, (meth)acrylamidepropyldimethylamine or its salts, N-hydroxymethyl(meth)acrylamide or its derivatives; N-vinylamides such as N-vinylformamide, N-vinylacetamide, N-vinylpyrrolidone; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether; acrylonitrile such as (meth)acrylonitrile; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; maleic acid or its salts, esters or anhydrides; itaconic acid or its salts, esters or anhydrides; vinylsilyl compounds such as vinyltrimethoxysilane; unsaturated sulfonic acids, etc. The polyvinyl ester may have a structural unit derived from one or two or more of these other monomers.
[0038] Based on the molar number of all structural units constituting polyvinyl ester, the proportion of structural units derived from other monomers in polyvinyl ester is preferably 15 mol% or less, more preferably 10 mol% or less, and further preferably 5 mol% or less. In particular, when other monomers are monomers that may promote the water solubility of the obtained PVA, such as (meth) acrylic acid and unsaturated sulfonic acid, in order to prevent the PVA from dissolving when the obtained PVA film is used as a raw material film for the manufacture of polarizing films, the proportion of structural units derived from these monomers in polyvinyl ester is preferably 5 mol% or less, and more preferably 3 mol% or less, based on the molar number of all structural units constituting polyvinyl ester.
[0039] As long as the effect of the present invention is not impaired, PVA may be a material modified by one or more graft copolymerizable monomers. Examples of graft copolymerizable monomers include unsaturated carboxylic acids or their derivatives; unsaturated sulfonic acids or their derivatives; α-olefins having 2 to 30 carbon atoms, etc. Based on the molar number of all structural units constituting PVA, the proportion of structural units derived from graft copolymerizable monomers in PVA is preferably 5 mol% or less.
[0040] For PVA, a part of its hydroxyl groups may be cross-linked or not. In addition, for PVA, a part of its hydroxyl groups may react with aldehyde compounds such as acetaldehyde and butyraldehyde to form an acetal structure or may not react with these compounds to form an acetal structure.
[0041] The degree of polymerization of PVA is preferably in the range of 1,500 to 6,000, more preferably in the range of 1,800 to 5,000, and further preferably in the range of 2,000 to 4,000. If the degree of polymerization is less than 1,500, there is a tendency for the durability of the polarizing film manufactured using the obtained PVA film to deteriorate. On the other hand, if the degree of polymerization exceeds 6,000, there is a tendency involving increased manufacturing costs, poor process passability during film making, and increased shrinkage stress of the obtained polarizing film. It should be noted that the so-called PVA degree of polymerization in this specification refers to the average degree of polymerization measured in accordance with the description of JIS K6726-1994.
[0042] From the viewpoint of water resistance of a polarizing film manufactured using the obtained PVA film, the saponification degree of PVA is preferably 98.0 mol% or more, more preferably 98.5 mol% or more, and further preferably 99.0 mol% or more. If the saponification degree is less than 98.0 mol%, the water resistance of the polarizing film tends to deteriorate. It should be noted that the saponification degree of PVA in this specification refers to the ratio (mol%) of the molar number of the vinyl alcohol unit relative to the total molar number of the structural unit (typically a vinyl ester unit) and the vinyl alcohol unit that can be converted into the vinyl alcohol unit by saponification of the PVA. The saponification degree can be measured in accordance with the description of JIS K6726-1994.
[0043] [Surfactant]
[0044] The PVA film of the present invention preferably contains a surfactant. By containing a surfactant, the generation of uneven thickness of the PVA film is suppressed, and the peeling from the roller or belt when manufacturing the PVA film becomes easy. The type of surfactant is not particularly limited, but from the viewpoint of peelability from the roller or belt when manufacturing the PVA film, an anionic surfactant or a nonionic surfactant is preferred.
[0045] Preferred anionic surfactants include, for example, carboxylic acid type surfactants such as potassium laurate; sulfate ester type surfactants such as polyoxyethylene lauryl ether sulfate and octyl sulfate; and sulfonic acid type surfactants such as dodecylbenzenesulfonate.
[0046] As the nonionic surfactant, preferred are, for example, alkyl ether types such as polyoxyethylene oleyl ether; alkyl phenyl ether types such as polyoxyethylene octylphenyl ether; alkyl ester types such as polyoxyethylene laurate; alkyl amine types such as polyoxyethylene lauryl amino ether; alkyl amide types such as polyoxyethylene lauric acid amide; polypropylene glycol ether types such as polyoxyethylene polyoxypropylene ether; alkanolamide types such as lauric acid diethanolamide and oleic acid diethanolamide; allyl phenyl ether types such as polyoxyalkylene allyl phenyl ether, etc.
[0047] These surfactants may be used alone or in combination of two or more.
[0048] The content of the surfactant in the PVA film of the present invention is preferably in the range of 0.01 to 0.5 parts by mass relative to 100 parts by mass of PVA, more preferably in the range of 0.02 to 0.3 parts by mass, and further preferably in the range of 0.05 to 0.1 parts by mass. By making the content of the surfactant within the above range, the film forming property and peeling property of the PVA film can be maintained, and the surfactant can be prevented from oozing out on the surface of the PVA film and clogging and reducing the operability.
[0049] [Plasticizer]
[0050] The PVA film of the present invention preferably contains a plasticizer. Examples of the plasticizer include polyols such as ethylene glycol, glycerol, propylene glycol, diethylene glycol, diglycerol, triethylene glycol, tetraethylene glycol, and trimethylolpropane, and the PVA film of the present invention may contain at least one of these plasticizers. Among these, as described in the manufacturing method of the PVA film below, the plasticizer is preferably at least one selected from glycerol, diglycerol, and propylene glycol, and the plasticizer more preferably contains at least glycerol.
[0051] The content of the plasticizer in the PVA film of the present invention is preferably in the range of 1 to 20 parts by mass, more preferably in the range of 3 to 17 parts by mass, and further preferably in the range of 5 to 15 parts by mass relative to 100 parts by mass of PVA. By making the content of the plasticizer within the above range, the stretchability of the PVA film can be further improved, and the PVA film can be prevented from becoming too soft and reducing the handleability.
[0052] [Other additives]
[0053] The PVA film of the present invention may further contain components such as an antioxidant, an antifreeze agent, a pH adjuster, a concealing agent, an anti-coloring agent, and an oil agent as required.
[0054] [Shape, etc.]
[0055] The shape of the PVA film of the present invention is not particularly limited, but preferably a long film can be used to continuously and smoothly manufacture a more uniform PVA film and to continuously use it when used to manufacture a polarizing film, etc. The length of the long film (the length in the mechanical flow direction) is not particularly limited and can be appropriately set according to the purpose, for example, it can be set within the range of 5 to 30,000 m.
[0056] The width of the PVA film of the present invention is not particularly limited and can be appropriately set according to the use of the PVA film or the polarizing film manufactured therefrom, but from the viewpoint that the large screen of liquid crystal televisions or liquid crystal displays is developing in recent years, if the width of the PVA film is set to be 3m or more, more preferably 4m or more, it is suitable for these uses. On the other hand, if the width of the PVA film is too large, it is easy to make it difficult to uniformly perform uniaxial stretching itself when the polarizing film is manufactured using a practical device, so the width of the PVA film is preferably 7m or less.
[0057] In the present invention, the thickness of the PVA film is preferably in the range of 45 to 80 μm, more preferably in the range of 45 to 60 μm. By making the thickness of the PVA film below the upper limit, it becomes easy and quick to dry the polarizing film. On the other hand, by making the thickness of the PVA film above the lower limit, the breakage of the PVA film during uniaxial stretching for the manufacture of the polarizing film can be more effectively suppressed.
[0058] The PVA film of the present invention is preferably an optical film. That is, the PVA film of the present invention is preferably used as a raw material film used in the manufacture of optical films such as polarizing films and phase difference films. Among these, the PVA film according to the present invention is preferably used as a raw material film used in the manufacture of polarizing films from the perspective of reducing breakage even under high-speed stretching conditions and obtaining a polarizing film with excellent optical properties.
[0059] There is no particular limitation on the manufacture of the PVA film of the present invention, and conventionally known methods such as wet film-making, gel film-making, cast film-making, and extrusion film-making can be used. However, by adopting the PVA film manufacturing method described later, the PVA film of the present invention can be efficiently manufactured.
[0060] <Method for producing PVA film>
[0061] The manufacturing method of the PVA film of the present invention is a method for manufacturing the PVA film by casting a film-forming stock solution containing PVA on a roller or a belt heated to 50 to 99° C. and drying the PVA film, wherein after the PVA film is dried until the content of the plasticizer component becomes 20 to 23% by weight, the PVA film is heat-treated on a roller or a belt heated to 100 to 120° C.
[0062] In the above-mentioned method for producing a PVA film, as a film-forming stock solution containing PVA (hereinafter, sometimes abbreviated as film-forming stock solution), a substance obtained by dissolving PVA in a liquid medium, or a substance obtained by melting PVA and a liquid medium can be used. The specific form and suitable form of the PVA contained in the film-forming stock solution are the same as those of the PVA contained in the above-mentioned PVA film.
[0063] Examples of the liquid medium contained in the membrane-forming stock solution include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, glycerol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, trimethylolpropane, ethylenediamine, and diethylenetriamine. One or more of these can be used. Among them, water is preferably used from the viewpoint of environmental load or recyclability.
[0064] The volatile content of the film-forming stock solution (the proportion of volatile components such as the liquid medium removed by volatilization or evaporation during film formation) varies depending on the film-forming method, film-forming conditions, etc., but is preferably in the range of 50 to 95% by mass, more preferably in the range of 55 to 90% by mass, and further preferably in the range of 60 to 85% by mass. If the volatile content of the film-forming stock solution is too low, the viscosity of the film-forming stock solution becomes too high, and filtering or degassing during the preparation of the film-forming stock solution becomes difficult, and the production of a PVA film with few impurities or defects tends to become difficult. On the other hand, if the volatile content of the film-forming stock solution is too high, the concentration of the film-forming stock solution becomes too low, and the production of industrial PVA films tends to become difficult.
[0065] Here, the volatile content of the membrane-forming stock solution in this specification refers to a value obtained by the following formula.
[0066] Volatile content of film-forming stock solution (mass %) = {(Wa-Wb) / Wa}×100
[0067] In the above formula, Wa represents the mass (g) of the film-forming stock solution, and Wb represents the mass (g) of the film-forming stock solution of Wa (g) after drying in an electric heating dryer at 105° C. for 16 hours.
[0068] The film-forming stock solution preferably contains a surfactant. The specific form and suitable form of the surfactant contained in the film-forming stock solution are the same as those of the surfactant contained in the above-mentioned PVA film.
[0069] The film-forming stock solution preferably contains a plasticizer. The specific form and suitable form of the plasticizer contained in the film-forming stock solution are the same as those of the plasticizer contained in the above-mentioned PVA film.
[0070] In the above-mentioned method for producing a PVA film, a film-forming stock solution containing PVA is cast on a roller or a belt heated to 50 to 99° C. and dried. From the viewpoint of the production efficiency of the PVA film, the surface temperature of the heated roller or belt is more preferably in the range of 60 to 98° C., and further preferably in the range of 70 to 97° C.
[0071] In the above-mentioned method for manufacturing the PVA film, the PVA film is dried until the amount of the plasticizer reaches 20 to 23% by mass. By making the amount of the plasticizer within the above-mentioned range, the PVA film of the present invention can be effectively manufactured. Here, the amount of the plasticizer refers to the mass fraction of the plasticizer contained in the PVA film when the film-making stock solution containing PVA is cast on a roller or belt heated to 50 to 99° C. and the dried PVA film is brought into contact with the initial heat treatment roller. The plasticizer consists of a liquid medium and a plasticizer contained in the film-making stock solution of the PVA film.
[0072] As mentioned above, the plasticizing component is composed of a liquid medium and a plasticizer. As the liquid medium, water is preferred, and as the plasticizer, at least one selected from glycerol, diglycerol and propylene glycol is preferred. That is, the plasticizing component is composed of water and a plasticizer, and the plasticizer is preferably at least one selected from glycerol, diglycerol and propylene glycol. By using such a plasticizer with a high plasticizing effect, the tensile properties of the resulting PVA film become easy to improve. In addition, among these plasticizers, glycerol has a lower volatility and a higher plasticizing effect, so it is more preferred that the plasticizer contains at least glycerol.
[0073] In the above-mentioned method for producing a PVA film, after the PVA film is dried until the amount of the plasticizer component becomes 20 to 23% by mass, the PVA film is heat-treated on a roller or a belt heated to 100 to 120° C. By making the temperature of the heat treatment within the above-mentioned range, the swelling degree (A), swelling degree ratio (B / A) and average water absorption rate of the PVA film can be adjusted to the desired range. In addition, the mechanical strength and other properties of the PVA film can also be adjusted.
[0074] The heat treatment is preferably performed on a drum heated to 100 to 120° C. In order to more efficiently produce the PVA film of the present invention, the heat treatment temperature is preferably 102° C. or higher, preferably 115° C. or lower, and more preferably 108° C. or lower. The heat treatment time is usually 10 to 30 seconds.
[0075] <Method for producing polarizing film>
[0076] The PVA film according to the present invention is preferably used as a raw material film used in the manufacture of a polarizing film from the perspective of reducing breakage even under high-speed stretching conditions and obtaining a polarizing film with excellent optical properties. The method for manufacturing a polarizing film using the PVA film of the present invention as a raw material film is not particularly limited, and any method that has been used so far can be used. As such a method, for example, a method of dyeing and uniaxially stretching the PVA film can be cited. Specifically, a method of swelling, dyeing, uniaxially stretching the PVA film, and further performing a fixing treatment, drying, heat treatment, etc. as required can be cited. In this case, the order of each treatment such as swelling, dyeing, uniaxial stretching, and fixing treatment is not particularly limited, and one or more treatments may be performed simultaneously. In addition, one or more of each treatment may be performed twice or more.
[0077] Swelling can be performed by immersing the PVA film in water. The temperature of the water when immersed in water is preferably in the range of 20 to 40°C, more preferably in the range of 22 to 38°C, and further preferably in the range of 25 to 35°C. In addition, the time of immersion in water is, for example, preferably in the range of 0.1 to 5 minutes, and more preferably in the range of 0.5 to 3 minutes. It should be noted that the water when immersed in water is not limited to pure water, and can be an aqueous solution obtained by dissolving various components, or a mixture of water and an aqueous medium.
[0078] Dyeing is preferably performed using iodine, and the dyeing period may be any stage before uniaxial stretching, during uniaxial stretching, or after uniaxial stretching. Dyeing is generally performed by immersing the PVA film in a solution (especially an aqueous solution) containing iodine-potassium iodide as a dyeing bath, and such a dyeing method is also suitable for the present invention. The iodine concentration in the dyeing bath is preferably in the range of 0.01 to 0.5% by mass, and the potassium iodide concentration is preferably in the range of 0.01 to 10% by mass. In addition, the temperature of the dyeing bath is preferably in the range of 20 to 50° C., and more preferably in the range of 25 to 40° C.
[0079] The uniaxial stretching can be performed by any method of wet stretching or dry stretching. In the case of the wet stretching method, it can be performed in an aqueous solution containing boric acid, in the dyeing bath described above, or in the fixing treatment bath described later. In addition, in the case of the dry stretching method, the PVA film after absorbing water can be used and performed in the air. Among these, the wet stretching method is preferred, and the uniaxial stretching in an aqueous solution containing boric acid is more preferred. The concentration of boric acid in the boric acid aqueous solution is preferably in the range of 0.5 to 6.0 mass%, more preferably in the range of 1.0 to 5.0 mass%, and particularly preferably in the range of 1.5 to 4.0 mass%. In addition, the boric acid aqueous solution may contain potassium iodide, and its concentration is preferably in the range of 0.01 to 10 mass%. The stretching temperature of the uniaxial stretching is preferably in the range of 30 to 90°C, more preferably in the range of 40 to 80°C, and particularly preferably in the range of 50 to 70°C. In addition, from the viewpoint of the polarization performance of the obtained polarizing film, the stretching ratio of the uniaxial stretching is preferably 5 times or more, more preferably 5.5 times or more, and particularly preferably 6 times or more. The upper limit of the stretching ratio is not particularly limited, but the stretching ratio is preferably 8 times or less.
[0080] When manufacturing a polarizing film, in order to make the dye (iodine, etc.) firmly adsorbed to the PVA film, it is preferably fixed. As a fixing treatment bath used in the fixing treatment, an aqueous solution containing one or more boron compounds such as boric acid and borax can be used. In addition, as needed, an iodine compound or a metal compound can also be added to the fixing treatment bath. The concentration of the boron compound in the fixing treatment bath is preferably in the range of 2 to 15 mass%, more preferably in the range of 3 to 10 mass%. The temperature of the fixing treatment bath is preferably in the range of 15 to 60°C, more preferably in the range of 25 to 40°C.
[0081] Drying is preferably performed at a temperature in the range of 30 to 150° C., more preferably in the range of 50 to 130° C. When the polarizing film has a moisture content of 10% or less by drying, tension is applied to the polarizing film and heat treatment is performed at about 80 to 120° C. for about 1 to 5 minutes, a polarizing film having better dimensional stability, durability, etc. can be obtained.
[0082] The polarizing film obtained as above is usually used as a polarizer by laminating protective films on both sides or one side thereof. As the protective film, optically transparent and mechanically strong protective films can be cited, and specifically, for example, triacetyl cellulose (TAC) film, cellulose acetate / butyrate (CAB) film, acrylic film, polyester film, etc. can be used. In addition, as the adhesive for lamination, PVA adhesives or urethane adhesives can be cited, among which PVA adhesives are suitable.
[0083] The polarizing plate obtained as described above can be applied with an acrylic adhesive and then bonded to a glass substrate to be used as a component of an LCD. It can also be bonded to a retardation film, a viewing angle improvement film, a brightness improvement film, etc.
[0084] The thickness of the polarizing film is not particularly limited, and can be set to 30 μm or less, and further can be set to 25 μm or less. From the viewpoint of reducing the shrinkage stress of the polarizing film and the polarizer using the polarizing film, and preventing the warping of the laminated thin glass, the thickness of the polarizing film is preferably 20 μm or less, and more preferably 15 μm or less. On the other hand, from the viewpoint that an excessively thin polarizing film tends to be difficult to manufacture or handle, the thickness of the polarizing film is preferably 3 μm or more.
[0085] Example
[0086] The present invention will be specifically described below by way of examples, but the present invention is not limited to these examples. Evaluation methods and the like were performed according to the methods shown below.
[0087] [Swelling degree of PVA film (A)]
[0088] From the PVA film obtained in the following examples and comparative examples, a rectangular sample with a width direction (TD) of 100 mm and a length direction (mechanical flow direction) of 200 mm is cut, and the sample is further cut into a long strip with a width of 2 to 3 mm and a length of 200 mm. Then, all these long strip samples are directly immersed in 1000 g of pure water at 30°C. After immersion for 30 minutes, the long strip sample is taken out, centrifuged and dehydrated at 3000 rpm for 5 minutes, and the mass Wa (g) after dehydration (the total of all long strip samples) is measured. Then, after the long strip sample is dried in a dryer at 105°C for 16 hours, the mass Wb (g) (the total of all long strip samples) is measured, and the swelling degree (A) is calculated by the following formula. It should be noted that the same measurement was performed 3 times, and the average value was adopted.
[0089] Swelling degree (A) (%) = 100 × Wa / Wb
[0090] [Swelling degree of PVA film (B)]
[0091] A rectangular sample with a width direction (TD) of 40 mm and a length direction (mechanical flow direction) of 110 mm was cut from the PVA film obtained in the following examples and comparative examples. Two marking lines (thickness of about 0.5 mm) in the width direction of the sample were drawn in the center of the length direction of the sample with an oil pen so that the distance between the marking lines (between the centers of the thickness direction of the marking lines) was 50 mm. The sample was set on a stretching fixture (the distance between the chucks was 50 mm) in such a way that each marking line was located at the end of the stretching fixture, immersed in pure water at 30°C, and after 10 seconds, uniaxially stretched at a stretching speed of 0.12 m / min (240% / min) in such a way that the actual stretching ratio became 2.5 times. The so-called actual stretching ratio here is the value obtained by dividing the distance between the centers of the marking lines after stretching (the centers of the thickness direction of the marking lines at the position where the length of the marking lines is equally divided) by the distance between the marking lines before stretching (50 mm). After stretching, within 1 minute, wipe the moisture on the surface of the stretched sample with filter paper, cut the sample along the marking line at the center of the thickness direction of the marking line, and cut out the film between the marking lines, and measure the mass Wc (g) of the film between the marking lines. Then, after drying the film in a dryer at 105°C for 16 hours, measure the mass Wd (g), and calculate the swelling degree (B) after stretching in 30°C water at a stretching ratio of 2.5 times by the following formula. It should be noted that the same measurement was performed 5 times, and the average value of 3 times excluding the maximum and minimum values was adopted.
[0092] Swelling degree (B) (%) = 100 × Wc / Wd
[0093] [Dimensional change rate of PVA film in the width direction]
[0094] From the central part in the width direction of the PVA film obtained in the following examples and comparative examples, a rectangular sample with a length direction (mechanical flow direction) of 40 mm x width direction (TD) of 270 mm is cut out. A 10 mm length direction marking line is drawn inward from both ends of the sample with a length of 270 mm. The outer part is clamped from the marking lines at both ends with a clamp (clamp width 40 mm, mass 7.8 g (weight in water 7.3 g)), and one of the clamps is fixed with a rod-shaped clamp. After confirming that the distance between the marking lines is 250 mm, the entire sample is quickly immersed in pure water stored in a water tank and adjusted to 30°C in a manner such that the long side of the sample becomes vertical (vertical). At this time, immediately after the immersion, the rod-shaped clamp is hung on the upper part of the water tank and fixed in a manner such that the long side of the sample becomes vertical (vertical). The distance W between the marking lines of the sample is measured 30 seconds after the immersion. TD Then, the dimensional change rate was calculated by the following formula.
[0095] Dimensional change rate (%) = 100 × {(W TD -250) / 250}
[0096] [Average water absorption rate of PVA film]
[0097] The moisture content M of the PVA films obtained in the following examples and comparative examples was determined by the following methods (1) and (2). 30 The average water absorption rate (mass % / second) of the PVA film was calculated by the following formula: M0 and M0. When measuring a PVA film having a water content of less than 2.5 mass % or more than 4.0 mass %, the water content M0 of the PVA film before water absorption was adjusted to 2.5 to 4.0 mass %, and then the film was allowed to absorb water by the following method (1) and the water content M0 after water absorption was measured. 30 , thus the average water absorption rate is obtained.
[0098] Average water absorption rate (mass % / sec) = {(M 30 -M0) / 30}
[0099] (1) A rectangular sample with a width of 50 mm and a length of 100 mm was cut from the PVA film obtained in the following examples and comparative examples, and immersed in 1000 g of pure water at 30°C for 30 seconds. The immersed sample was taken out, the surface water was absorbed with filter paper, and its mass We (g) was measured. Then, the sample was dried in a dryer at 105°C for 16 hours, and its mass Wf (g) was measured. From the obtained masses We and Wf, the moisture content M of the PVA film was calculated by the following formula: 30 (mass %) The same measurement was performed three times, and the average value was adopted.
[0100] M 30(mass %) = {(We - Wf) / We} × 100
[0101] (2) Cut out a sample of about 5 g from the PVA film obtained in the following examples and comparative examples. Place the sample in a heat-resistant container made of glass and seal it, and measure the mass Wg (g) of the sample after removing the tare to 4 decimal places. Next, place the sample in a vacuum dryer at a temperature of 50°C and a pressure of less than 0.1 kPa in each heat-resistant container, and after drying for 4 hours with the lid of the heat-resistant container open, measure the mass Wh (g) of the sample after removing the tare to 4 decimal places. From the obtained masses Wg and Wh, the moisture content M0 (mass %) of the PVA film is calculated by the following formula.
[0102] M0 (mass %) = {(Wg-Wh) / Wg} × 100
[0103] [Content of plasticizer in PVA film before heat treatment]
[0104] In the following examples and comparative examples, a sample of about 5 g was cut out from the center of the width direction of a PVA film dried on a heated metal drum (heated roller). The moisture content M (mass %) and the plasticizer content G (mass %) of the sample were determined by the following methods (1) and (2), and their total value was set as the content (mass %) of the plasticizer component in the PVA film before heat treatment.
[0105] (1) The sample is placed in a heat-resistant container made of glass and sealed, and the mass Wi (g) of the sample after removing the tare is measured to 4 decimal places. Next, the sample is placed in a vacuum dryer at a temperature of 50°C and a pressure of 0.1 kPa or less in each heat-resistant container, and after drying for 4 hours with the lid of the heat-resistant container open, the mass Wj (g) of the sample after removing the tare is measured to 4 decimal places. From the obtained masses Wi and Wj, the moisture content M (mass %) of the PVA film is calculated by the following formula.
[0106] M (mass %) = {(Wi - Wj) / Wi} × 100
[0107] (2) Take out 0.3g of the film from the sample and immerse it in 9g of pure water at room temperature for 3 minutes. After measuring the mass Wk (g) of the obtained extract, pass it through a solid phase extraction column and collect the separated liquid, and measure the glycerol concentration CG (mass %) using a refractometer ("ABBEMAT550" manufactured by Anton-paar). On the other hand, the immersed film from which the extract has been removed is dried at 105°C for 2 hours, and the mass Wl (g) of the dried film is measured. From the obtained mass Wk, Wl and concentration CG, the plasticizer rate G (mass %) of the PVA film is calculated by the following formula.
[0108] G (mass %) = CG × Wk / Wl
[0109] [Tensile stress of PVA film (480% / min)]
[0110] From the central part of the width direction of the PVA film obtained in the following examples and comparative examples, a sample with a width direction of 30 mm and a length direction of 100 mm was cut out. In order to perform uniaxial stretching in the length direction, it was clamped in a stretching fixture in a manner that the gap between the chucks was 30 mm, and immersed in pure water at 30°C for 8 seconds. Then, while uniaxial stretching was performed in the length direction at a stretching speed of 144 mm / min (480% / min), the stress relative to the stretching ratio was continuously measured. At this time, the stress when the strain of the PVA film was 400% was set as the tensile stress. It should be noted that the stress was measured using an automatic plotter (Autograph) ("AG-I" manufactured by Shimadzu Corporation), and the stress was obtained by dividing the measured tension by the cross-sectional area before stretching (sample thickness × sample width (30 mm)). The same measurement was performed 3 times, and the average value was taken as the tensile stress (480% / min) of the PVA film.
[0111] [Tensile stress of PVA film (240% / min)]
[0112] The tensile stress (240% / min) of the PVA film was determined in the same manner as in the above-mentioned “tensile stress (480% / min) of the PVA film” except that the tensile speed was 72 mm / min (240% / min).
[0113] [Polarization degree when the transmittance of the polarizing film is 43.0%]
[0114] In the following examples and comparative examples, the iodine concentration in the iodine / potassium iodide aqueous solution during the second stretching when manufacturing a polarizing film from a PVA film was changed to manufacture five polarizing films with different dyeing concentrations. For each of the five polarizing films, the single transmittance Y (%) and the polarization degree V (%) were calculated using the following methods (1) and (2), and the data of the five polarizing films were plotted with the single transmittance Y as the horizontal axis and the polarization degree V as the vertical axis to create an approximate curve. The value of the polarization degree V when the single transmittance Y was 43.0% was calculated from the approximate curve, and this value was set as "Polarization degree (%) when the transmittance was 43.0%".
[0115] (1) Collect two square samples of 30 mm in length and 30 mm in width from one of the five polarizing films. For one of the samples, use a spectrophotometer with an integrating sphere ("V7100" manufactured by JASCO Corporation) to perform visual sensitivity correction in the visible light region of 2° field of view with C light source and according to JIS Z8722:2009 (Method for measuring object color). Measure the transmittance of light when inclined at 45° relative to the length direction and the transmittance of light when inclined at -45°, and calculate their average value TY1(%). Similarly, measure the transmittance of light when inclined at 45° and the transmittance of light when inclined at -45° for the other sample, and calculate their average value TY2(%). TY1(%) and TY2(%) are averaged by the following formula to calculate the single transmittance Y(%) of the polarizing film. Perform this operation for each of the five polarizing films.
[0116] Y(%)=(TY1+TY2) / 2
[0117] (2) Overlap the two polarizing film samples collected in the measurement of the single transmittance Y in (1) above so that their length directions are parallel, measure the transmittance of light when inclined at 45° and when inclined at -45° relative to the length direction, and find their average value T∥(%). Next, overlap them so that their length directions are orthogonal, measure the transmittance of light when inclined at 45° and when inclined at -45° relative to the length direction, and find their average value T⊥(%). The polarization degree V(%) is calculated using the following formula. This operation is performed for each of the five polarizing films.
[0118] V(%)={(T∥-T⊥) / (T∥+T⊥)}1 / 2×100
[0119] [Example 1]
[0120] A film-making stock solution having a volatile content of 66% by mass was prepared, which consisted of 100 parts by mass of PVA (a saponified homopolymer of vinyl acetate, with a polymerization degree of 2,400 and a saponification degree of 99.95 mol%), 13 parts by mass of glycerol as a plasticizer, 0.1 parts by mass of lauric acid diethanolamide as a surfactant, and water. The film-making stock solution was cast onto a metal drum having a surface temperature of 80°C, dried until the content of the plasticizer component became 20.1% by mass (water content 7% by mass, plasticizer content 13.1% by mass), and then heat-treated at 105°C for 15 seconds to obtain a PVA film having a width of 65 cm and a thickness of 60 μm. The swelling degree (A), swelling degree (B), average water absorption rate, dimensional change rate in water in the width direction, tensile stress (240% / min), and tensile stress (480% / min) were measured by the above-mentioned method for the obtained PVA film. The swelling ratio (B / A) was calculated by dividing the swelling ratio (B) by the swelling ratio (A).
[0121] After the PVA film was immersed in water at a temperature of 30°C and uniaxially stretched (first stretching) to twice the original length in the longitudinal direction, it was then immersed in an iodine / potassium iodide aqueous solution containing 0.05% by mass of iodine and 1.2% by mass of potassium iodide at 32°C and uniaxially stretched (second stretching) to 2.5 times the original length in the longitudinal direction. Next, it was immersed in a boric acid aqueous solution containing 2.6% by mass of boric acid at 30°C and uniaxially stretched (third stretching) to three times the original length in the longitudinal direction, and further immersed in a boric acid / potassium iodide aqueous solution containing 2.8% by mass of boric acid and 5% by mass of potassium iodide at 55°C and uniaxially stretched (fourth stretching) to 5.8 times the original length in the longitudinal direction. Next, the film was washed by immersing in a 22°C potassium iodide aqueous solution containing 1.5% by mass of boric acid and 3.3% by mass of potassium iodide, and dried in a dryer at 80°C for 110 seconds to produce a polarizing film with a thickness of 24 μm. The polarization degree of the obtained polarizing film was measured by the above method at a transmittance of 43.0%. The results are shown in Table 1.
[0122] [Examples 2 to 5, Comparative Examples 1 to 3]
[0123] The PVA film and polarizing film were obtained in the same manner as in Example 1, except that the amount of glycerol added or the drying time of the PVA film was adjusted, the content of the plasticizer component of the PVA film before heat treatment was changed as shown in Table 3, and the conditions of the heat treatment temperature were changed as shown in Table 3. For the obtained PVA film, the swelling degree (A), swelling degree (B), average water absorption rate, dimensional change rate in water in the width direction, tensile stress (240% / min) and tensile stress (480% / min) were measured by the above-mentioned method. In addition, the swelling degree (B) was divided by the swelling degree (A) to obtain the swelling degree ratio (B / A). Furthermore, for the obtained polarizing film, the polarization degree at a transmittance of 43.0% was measured by the above-mentioned method. These results are shown in Tables 1 and 2.
[0124] [Table 1]
[0125]
[0126] [Table 2]
[0127]
[0128] [Table 3]
[0129]
[0130] As shown in Table 1, the PVA films of Examples 1 to 5 have sufficiently low tensile stress under the stretching condition of 480% / min, so the breakage of the PVA films is reduced even under high-speed stretching conditions when manufacturing polarizing films. In addition, the polarizing films obtained from the PVA films of Examples 1 to 5 have a sufficiently high degree of polarization at a transmittance of 43.0%. That is, according to the PVA films of Examples 1 to 5, the breakage of the PVA films is reduced even under high-speed stretching conditions when manufacturing polarizing films, and polarizing films with excellent optical properties can be manufactured.
[0131] On the other hand, as shown in Table 1, for the PVA films of Comparative Examples 1 to 2, the optical properties of the obtained polarizing films are excellent, but the tensile stress under the stretching condition of 480% / min is large, so the PVA film is easily broken under the high-speed stretching condition when manufacturing the polarizing film. In addition, since the tensile stress of the PVA film of Comparative Example 3 is sufficiently small under the stretching condition of 480% / min, the breakage of the polarizing film is reduced even under the high-speed stretching condition when manufacturing the polarizing film, but the polarization degree of the obtained polarizing film at a transmittance of 43.0% is insufficient. It should be noted that even the PVA films of Comparative Examples 1 to 2 have sufficiently small tensile stress under relatively low-speed stretching conditions such as 240% / min. That is, in the PVA films of Comparative Examples 1 to 2, the breakage of the PVA film can be reduced under the conventional relatively low-speed stretching conditions and a polarizing film with excellent optical properties can be manufactured, but the PVA film is easily broken under high-speed stretching conditions such as 480% / min, and the manufacturing efficiency of the polarizing film is reduced.
[0132] As shown in the above-mentioned embodiment, according to the present invention, when manufacturing a polarizing film, the breakage of the PVA film is reduced even under high-speed stretching conditions, and a polarizing film with excellent optical properties can be manufactured. Therefore, a polarizing film can be efficiently manufactured without compromising the optical properties.
Claims
1. A polyvinyl alcohol film having a swelling degree (A) of 195 to 205% by mass, wherein the swelling degree (B) after stretching 2.5 times in water at 30° C. at a stretching speed of 240% / min divided by the swelling degree (A) is 1.27 to 1.40, wherein: The average water absorption rate when immersed in water at 30° C. for 30 seconds was 1.35 mass % / second or more. 2 . The polyvinyl alcohol film according to claim 1 , wherein the dimensional change rate in the width direction when immersed in water at 30° C. for 30 seconds is 14.6 to 16.2%.
3. The polyvinyl alcohol film according to claim 1 or 2, wherein the thickness of the film is 45 to 80 μm. The polyvinyl alcohol film according to claim 1 or 2, which is an optical film.
5. The method for producing a polyvinyl alcohol film according to claim 1 or 2, which is a method for producing a polyvinyl alcohol film by casting a film-forming stock solution containing polyvinyl alcohol onto a drum or a belt heated to 50 to 99°C and drying the drum or belt, wherein: After the polyvinyl alcohol film is dried until the content of the plasticizer becomes 20 to 23% by mass, the polyvinyl alcohol film is heat-treated on a drum or a belt heated to 100 to 120°C.
6. The method for producing a polyvinyl alcohol film according to claim 5, wherein: The heat treatment is performed on a drum heated to 100 to 120°C.
7. The method for producing a polyvinyl alcohol film according to claim 5, wherein: The plasticizing component consists of water and a plasticizer, and the plasticizer is at least one selected from glycerol, diglycerol and propylene glycol.
Citation Information
Patent Citations
Polyvinyl alcohol film and polarizing film
WO2014050697A1