Steel sheet for hot stamping and hot-stamped molded article
By uniformly dispersing austenite grains in the steel plate and controlling the pearlite dispersion indicators, the hydrogen embrittlement cracking problem in the hot stamping molded body is solved, and the high strength and hydrogen embrittlement resistance characteristics are achieved, which is suitable for the automotive industry's lightweight need.
Patent Information
- Application Number
- CN202380027993.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-02
- Publication Date
- 2024-11-05
AI Technical Summary
Existing high-strength steels are prone to hydrogen embrittlement cracking during hot stamping, and it is difficult to take into account the requirements for high-strength and lightweight steels in the automotive industry that pursues lightweight.
By dispersing the austenite grains evenly in the steel plate before hot stamping, the uneven hardness of the original austenite grains is reduced, and high-pressure finishing and rapid cooling processes are adopted to control the dispersion index of pearlite and the original austenite. The hardness distribution of the grains is standard deviation, forming a steel plate with high tensile strength and hydrogen embrittlement resistance.
It significantly improves the hydrogen embrittlement resistance of the hot stamped molded body, ensures high strength and good forming properties, and is suitable for structural components such as automobiles.
Smart Images

Figure BDA0005044549880000291 
Figure BDA0005044549880000301 
Figure BDA0005044549880000311
Abstract
Description
Technical Field
[0001] The present invention relates to a steel sheet for hot stamping and a hot stamped body produced using the steel sheet. Background Art
[0002] In recent years, the automobile industry has been demanding lightweight vehicles from the perspective of improving fuel efficiency. In order to achieve both lightweight vehicles and collision safety, increasing the strength of the steel sheets used is one of the effective methods, and the development of high-strength steel sheets has been promoted from this background. On the other hand, if the strength of the steel sheet is increased, the formability decreases, so it is generally difficult to achieve a balance between strength and formability in steel sheets.
[0003] In connection therewith, Patent Document 1 describes a cold-rolled steel sheet having a predetermined chemical composition, wherein the metal structure contains, by area ratio, 40.0% or more and less than 60.0% of polygonal ferrite, 30.0% or more of bainitic ferrite, 10.0% or more and less than 25.0% of retained austenite, and 15.0% or less of martensite, wherein the proportion of retained austenite having an aspect ratio of 2.0 or less, a major axis length of 1.0 μm or less, and a minor axis length of 1.0 μm or less in the retained austenite is 80.0% or more, the proportion of bainitic ferrite having an aspect ratio of 1.7 or less, and an average value of a crystal orientation difference of a region surrounded by grain boundaries having a crystal orientation difference of 15° or more is 0.5° or more and less than 3.0° is 80.0% or more, and the connectivity D value of the martensite, the bainitic ferrite, and the retained austenite is 0.70 or less. Patent Document 1 states that the above-described structure can provide a high-strength cold-rolled steel sheet having a tensile strength of 980 MPa or more, a 0.2% yield strength of 600 MPa or more, excellent punching fatigue properties, elongation, and hole expandability, which is suitable as a structural member for automobiles, etc.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2016 / 136810 Summary of the invention
[0007] Problems to be solved by the invention
[0008] As a technology for press-forming difficult-to-form materials such as high-strength steel plates, hot stamping (hot pressing) is known. Hot stamping is a hot forming technology that heats the material to be formed and then forms it. In this technology, since the material is heated and then formed, the steel is soft and has good formability during forming. Therefore, even high-strength steel can be formed into complex shapes with good precision. In addition, it is known that the steel has sufficient strength after forming because it is quenched simultaneously with the forming by the pressing die.
[0009] In hot stamped parts with such high strength, hydrogen embrittlement cracking (also called delayed fracture, etc.) sometimes becomes a problem. So-called hydrogen embrittlement cracking is a phenomenon in which a steel component subjected to high stress under use conditions suddenly breaks due to hydrogen invading the steel from the environment. In general, it is known that the higher the strength of the steel becomes, the easier it is to produce hydrogen embrittlement cracking. On the other hand, in the automotive industry and the like, there is a demand for further lightweighting of steel, and in order to achieve such lightweighting, it is necessary to increase the strength of steel to a level higher than before. Therefore, there is a high demand for steel, more specifically hot stamped parts, that can solve the problem of hydrogen embrittlement even when the strength is increased to the same level or higher than before.
[0010] Therefore, an object of the present invention is to provide a hot stamped product having high strength and capable of suppressing hydrogen embrittlement, and a hot stamping steel sheet for producing such a hot stamped product, by a novel structure.
[0011] Means for solving problems
[0012] In order to achieve the above-mentioned purpose, the present inventors conducted research focusing on the metal structure of the steel sheet before hot stamping and the hot stamped body after hot stamping. As a result, the present inventors found that in the steel sheet before hot stamping, the pearlite that becomes the starting point of the austenite grains is uniformly dispersed during the heating of hot stamping, so that the original austenite grains are homogenized in the final hot stamped body, thereby reducing the unevenness of the hardness of the original austenite grains in the metal structure of the hot stamped body. Furthermore, the present inventors found that by reducing the unevenness of the hardness of the original austenite grains in the metal structure of the hot stamped body, the increase in local hardness can be suppressed, resulting in that despite having high tensile strength, the hydrogen embrittlement resistance can be significantly improved, thereby completing the present invention.
[0013] The present invention which can achieve the above-mentioned object is as follows.
[0014] (1) A steel sheet for hot stamping, having the following chemical composition in mass %:
[0015] C: 0.40~0.70%,
[0016] Si: 0.010~1.300%,
[0017] Mn: 0.60~3.00%,
[0018] P: 0.100% or less,
[0019] S: 0.0100% or less,
[0020] N: 0.0200% or less,
[0021] O: 0.0200% or less,
[0022] Al: 0.0010~0.5000%,
[0023] Nb: 0.0010~0.100%,
[0024] Ti: 0.010~0.200%,
[0025] B: 0.0005~0.0200%,
[0026] Cr: 0.010~0.80%,
[0027] Mo: 0.0010~1.000%,
[0028] Co: 0-2.00%,
[0029] Ni: 0-3.00%,
[0030] Cu: 0-1.00%,
[0031] V: 0~1.00%,
[0032] W: 0~1.000%、
[0033] Ca: 0~0.010%
[0034] Mg: 0~1.000%,
[0035] REM: 0~1.000%、
[0036] Sb: 0~1.000%,
[0037] Zr: 0~1.000%,
[0038] Sn: 0~1.000%,
[0039] As: 0 to 0.100%, and
[0040] The rest: Fe and impurities.
[0041] The hot stamping steel sheet has the following metal structure:
[0042] The area ratio includes:
[0043] Ferrite: 10% or more
[0044] Pearlite: more than 10%,
[0045] The total of ferrite and pearlite is more than 80%,
[0046] The dispersion index of pearlite is 0.50 or more.
[0047] (2) The hot stamping steel sheet according to (1) above, wherein the chemical composition contains, in mass %, one or more selected from the group consisting of the following elements:
[0048] Co: 0.001~2.00%
[0049] Ni: 0.001~3.00%,
[0050] Cu: 0.001~1.00%,
[0051] V: 0.001~1.00%,
[0052] W: 0.001~1.000%,
[0053] Ca: 0.0001~0.010%,
[0054] Mg: 0.0001~1.000%,
[0055] REM: 0.0001~1.000%,
[0056] Sb: 0.001~1.000%,
[0057] Zr: 0.001~1.000%,
[0058] Sn: 0.001~1.000% and
[0059] As: 0.001~0.100%.
[0060] (3) A hot stamped body having the following chemical composition in mass %:
[0061] C: 0.40~0.70%,
[0062] Si: 0.010~1.300%,
[0063] Mn: 0.60~3.00%,
[0064] P: 0.100% or less,
[0065] S: 0.0100% or less,
[0066] N: 0.0200% or less,
[0067] O: 0.0200% or less,
[0068] Al: 0.0010~0.5000%,
[0069] Nb: 0.0010~0.100%,
[0070] Ti: 0.010~0.200%,
[0071] B: 0.0005~0.0200%,
[0072] Cr: 0.010~0.80%,
[0073] Mo: 0.0010~1.000%,
[0074] Co: 0-2.00%,
[0075] Ni: 0-3.00%,
[0076] Cu: 0-1.00%,
[0077] V: 0~1.00%,
[0078] W: 0~1.000%、
[0079] Ca: 0~0.010%
[0080] Mg: 0~1.000%,
[0081] REM: 0~1.000%、
[0082] Sb: 0~1.000%,
[0083] Zr: 0~1.000%,
[0084] Sn: 0~1.000%,
[0085] As: 0 to 0.100%, and
[0086] The rest: Fe and impurities.
[0087] The hot stamping formed body has the following metal structure:
[0088] Contains at least one of martensite, bainite and tempered martensite in an area ratio of 90% or more in total,
[0089] The standard deviation of the hardness distribution of prior austenite grains at the position of 1 / 4 of the plate thickness is 150 Hv or less.
[0090] (4) The hot stamped body according to (3) above, wherein the chemical composition contains, in mass %, one or more selected from the group consisting of the following elements:
[0091] Co: 0.001~2.00%
[0092] Ni: 0.001~3.00%,
[0093] Cu: 0.001~1.00%,
[0094] V: 0.001~1.00%,
[0095] W: 0.001~1.000%,
[0096] Ca: 0.0001~0.010%,
[0097] Mg: 0.0001~1.000%,
[0098] REM: 0.0001~1.000%,
[0099] Sb: 0.001~1.000%,
[0100] Zr: 0.001~1.000%,
[0101] Sn: 0.001~1.000% and
[0102] As: 0.001~0.100%.
[0103] Effects of the Invention
[0104] According to the present invention, it is possible to provide a hot stamped product having high strength and capable of suppressing hydrogen embrittlement, and a hot stamping steel sheet for producing such a hot stamped product. DETAILED DESCRIPTION
[0105] <Steel Sheet for Hot Stamping>
[0106] The steel sheet for hot stamping according to the embodiment of the present invention is characterized in that it has the following chemical composition in mass %:
[0107] C: 0.40~0.70%,
[0108] Si: 0.010~1.300%,
[0109] Mn: 0.60~3.00%,
[0110] P: 0.100% or less,
[0111] S: 0.0100% or less,
[0112] N: 0.0200% or less,
[0113] O: 0.0200% or less,
[0114] Al: 0.0010~0.5000%,
[0115] Nb: 0.0010~0.100%,
[0116] Ti: 0.010~0.200%,
[0117] B: 0.0005~0.0200%,
[0118] Cr: 0.010~0.80%,
[0119] Mo: 0.0010~1.000%,
[0120] Co: 0-2.00%,
[0121] Ni: 0-3.00%,
[0122] Cu: 0-1.00%,
[0123] V: 0~1.00%,
[0124] W: 0~1.000%、
[0125] Ca: 0~0.010%
[0126] Mg: 0~1.000%,
[0127] REM: 0~1.000%、
[0128] Sb: 0~1.000%,
[0129] Zr: 0~1.000%,
[0130] Sn: 0~1.000%,
[0131] As: 0 to 0.100%, and
[0132] The rest: Fe and impurities.
[0133] The hot stamping steel sheet has the following metal structure:
[0134] The area ratio includes:
[0135] Ferrite: 10% or more
[0136] Pearlite: more than 10%,
[0137] The total of ferrite and pearlite is more than 80%,
[0138] The dispersion index of pearlite is 0.50 or more.
[0139] As described above, it is known that the higher the strength of the steel becomes, the easier it is to cause hydrogen embrittlement cracking. Therefore, the present inventors have conducted research from the perspective of reducing or suppressing the area that can become the starting point of hydrogen embrittlement cracking in such high-strength steel, focusing on the metal structure of the steel plate before hot stamping and the hot stamping body after hot stamping. More specifically, the present inventors first discovered that if the unevenness of the original austenite grain size in the metal structure of the hot stamping body is large, the hardness becomes higher in the area with a smaller original austenite grain size, and such a local high hardness area can become the starting point of hydrogen embrittlement cracking. In contrast, the present inventors found that by reducing the unevenness of the original austenite grain size, the unevenness of the hardness in the original austenite grains is reduced. More specifically, by controlling the standard deviation of the hardness distribution of the original austenite grains to less than 150Hv, such a local increase in hardness can be reliably suppressed.
[0140] Although it is not intended to be bound by any particular theory, it is believed that during hot stamping, the starting temperature of the martensitic transformation changes according to the grain size of the austenite grains. If described in more detail, it is believed that the starting temperature of the martensitic transformation is high compared to the austenite grains with a smaller grain size, so the hardness decreases. The austenite grains with a smaller grain size undergo martensitic transformation at a lower temperature than the large grains, so the hardness increases. Therefore, in order to suppress or reduce such a local increase in hardness, it becomes important to reduce the unevenness in the austenite grain size before the martensitic transformation. In other words, it is believed that by reducing the unevenness in the austenite grain size before the martensitic transformation, the unevenness in the original austenite grain size after the martensitic transformation can be reduced, and as a result, the unevenness in the hardness of the original austenite grains can be reduced in the metal structure of the hot stamping body. For such reasons, it is believed that by controlling the standard deviation of the hardness distribution of the original austenite grains in the metal structure of the hot stamping body to 150Hv or less and reducing the hardness unevenness of the original austenite grains, it is possible to significantly suppress the local hardness increase based on the different timing of the martensitic transformation. It is believed that if there is a high hardness area locally, there is a high possibility of causing hydrogen embrittlement cracking, especially at the interface of the original austenite grains with hardness difference, so reducing the hardness unevenness of the original austenite grains in the metal structure of the hot stamping body is very effective in improving the hydrogen embrittlement resistance.
[0141] In connection with this, as described in detail below with respect to the manufacturing method of the steel sheet for hot stamping, the present inventors focused on the metal structure of the steel sheet before hot stamping, such as the hot rolled steel sheet, and found that: by uniformly dispersing pearlite in the metal structure, the non-uniformity of the original austenite grain size can be reduced in the final metal structure of the hot stamped body, and in connection with this, the standard deviation of the hardness distribution of the original austenite grains can be controlled to be less than 150 Hv. With the high strength of steel materials, a relatively large amount of Mn is sometimes added to improve the hardenability of the steel materials, but this time, through the research of the present inventors, it is known that: at such a high Mn content (for example, 0.60 mass % or more), pearlite is relatively easy to generate, so it becomes very difficult to uniformly disperse the pearlite generated more in the metal structure of the hot rolled steel sheet compared with the case of low Mn content, and as a result, the non-uniformity of the original austenite grain size in the metal structure after hot stamping becomes larger. However, in response to such a problem, the inventors have discovered that by implementing a relatively high reduction in the final stage of finish rolling and then appropriately controlling the subsequent cooling, a uniform dispersion of pearlite can be achieved in the metal structure of the hot-rolled steel plate. As a result, the unevenness of the original austenite grain size can be reduced in the final metal structure of the hot stamped body, thereby significantly reducing the unevenness of the hardness distribution of the original austenite grains. More specifically, the present inventors have found that: in an electron microscope image of the metal structure of a hot stamping steel sheet mainly composed of ferrite and pearlite, it is important to control the dispersion index of pearlite, which is obtained by dividing the number of A / B boundaries (boundaries between ferrite phase and pearlite phase) by the total number of A / A boundaries (boundaries between ferrite phase and ferrite phase), the number of B / B boundaries (boundaries between pearlite phase and pearlite phase), and the number of A / B boundaries (boundaries between ferrite phase and pearlite phase), to be 0.5 or more, and by controlling the dispersion index of pearlite to be 0.5 or more, the standard deviation of the hardness distribution of prior austenite grains of 150 Hv or less can be achieved in the final metal structure of the hot stamped formed body due to the uniform dispersion of pearlite.
[0142] The present inventors have found out for the first time that the uneven distribution of hardness of the original austenite grains in the metal structure of the obtained hot stamped body can be controlled within a specified range by hot stamping a hot stamped steel sheet in which pearlite is uniformly dispersed within a specified range. In addition, the hot stamped body according to the embodiment of the present invention can significantly suppress the increase in local hardness by controlling the uneven distribution of hardness of the original austenite grains within a specified range, so that despite having a high tensile strength, such as a high tensile strength of more than 2200 MPa, the hydrogen embrittlement resistance can be significantly improved.
[0143] Hereinafter, the hot stamping steel sheet according to the embodiment of the present invention will be described in more detail. In the following description, the unit of the content of each element, i.e., "%", means "mass %" unless otherwise specified. In addition, in this specification, "-" indicating a numerical range is used to include the numerical values recorded before and after it as the lower limit and upper limit unless otherwise specified.
[0144] [C: 0.40~0.70%]
[0145] C is an element that improves the strength of hot stamped parts. When the C content is less than 0.40%, the desired strength cannot be obtained in the hot stamped parts. Therefore, the C content is set to 0.40% or more. The C content is preferably more than 0.40%, more than 0.42%, more than 0.43%, more than 0.44%, more than 0.45% or more than 0.46%.
[0146] On the other hand, when the C content exceeds 0.70%, the strength becomes too high and sometimes it is not possible to obtain excellent hydrogen embrittlement resistance. Therefore, the C content is set to 0.70% or less. Preferably, the C content is 0.68% or less, 0.67% or less, 0.65% or less, or 0.60% or less.
[0147] [Si: 0.010~1.300%]
[0148] Si is an element that improves the strength of hot stamping parts by solid solution strengthening. When the Si content is less than 0.010%, the desired strength cannot be obtained. Therefore, the Si content is set to 0.010% or more. The Si content is preferably 0.050% or more, 0.100% or more, 0.200% or more, more than 0.250%, 0.255% or more, 0.260% or more, 0.270% or more, 0.280% or more, 0.300% or more, or 0.400% or more.
[0149] On the other hand, when the Si content exceeds 1.300%, the amount of ferrite in the hot stamping steel sheet increases, and the desired metal structure may not be obtained. Therefore, the Si content is set to 1.300% or less. The Si content is preferably 1.200% or less, 1.000% or less, 0.800% or less, 0.600% or less, or 0.500% or less.
[0150] [Mn: 0.60~3.00%]
[0151] Mn is an element that promotes the phase transformation from austenite to pearlite in the hot-rolled steel sheet during the manufacturing process of the hot stamping formed body, contributes to the dispersion index of pearlite in the hot stamping steel sheet, and further controls the hardness distribution of the original austenite grains in the hot stamping formed body. In order to set the standard deviation of the dispersion index of pearlite and the hardness distribution of the original austenite grains to the desired range, the Mn content is set to 0.60% or more. The Mn content is preferably more than 0.60%, more than 0.70%, more than 0.80%, more than 1.00% or more than 1.30%.
[0152] On the other hand, if the Mn content exceeds 3.00%, the phase transformation from austenite to pearlite in the hot-rolled steel sheet is excessively promoted, and the dispersion index of pearlite and the standard deviation of the hardness distribution of the original austenite grains cannot be set to the desired range. Therefore, the Mn content is set to 3.00% or less. Preferably, the Mn content is 2.90% or less, 2.70% or less, 2.50% or less, 2.30% or less, or 2.00% or less.
[0153] [P: 0.100% or less]
[0154] P is an impurity element and segregates at grain boundaries to deteriorate hydrogen embrittlement resistance. Therefore, the P content is set to 0.100% or less. The P content is preferably 0.070% or less, 0.050% or less, or 0.010% or less.
[0155] The lower limit of the P content is not particularly limited, but if it is reduced to less than 0.0001%, the P removal cost will increase significantly, which is not economically preferable. Therefore, the P content may be set to 0.0001% or more.
[0156] [S: 0.0100% or less]
[0157] S is an impurity element and forms inclusions in steel. This inclusion deteriorates the hydrogen embrittlement resistance, so the S content is set to 0.0100% or less. The S content is preferably 0.0080% or less, 0.0050% or less, 0.0030% or less, or 0.0020% or less.
[0158] The lower limit of the S content is not particularly limited, but if it is reduced to less than 0.0001%, the S removal cost will increase significantly, which is not economically preferable. Therefore, the S content may be set to 0.0001% or more.
[0159] [N: 0.0200% or less]
[0160] N is an impurity element and forms nitrides in steel. The nitrides deteriorate the hydrogen embrittlement resistance, so the N content is set to 0.0200% or less. The N content is preferably 0.0180% or less, 0.0150% or less, 0.0100% or less, 0.0060% or less, or 0.0040% or less.
[0161] The lower limit of the N content is not particularly limited, but if it is reduced to less than 0.0001%, the cost of removing N increases significantly, which is not economically preferable. Therefore, the N content may be set to 0.0001% or more.
[0162] [O: 0.0200% or less]
[0163] If a large amount of O is contained in steel, it forms coarse oxides and deteriorates the hydrogen embrittlement resistance. Therefore, the O content is set to 0.0200% or less. The O content is preferably set to 0.0150% or less, 0.0100% or less, 0.0070% or less, or 0.0040% or less.
[0164] From the viewpoint of reducing refining cost, the O content may be set to 0.0001% or more. In order to disperse a large amount of fine oxides during deoxidation of molten steel, the O content may be set to 0.0005% or more.
[0165] [Al: 0.0010~0.5000%]
[0166] Al is an element that has the function of deoxidizing molten steel and improving steel. When the Al content is less than 0.0010%, deoxidation is not fully performed, and coarse oxides are generated, which deteriorates the hydrogen embrittlement resistance. Therefore, the Al content is set to 0.0010% or more. The Al content is preferably 0.0030% or more, 0.0050% or more, 0.0100% or more, or 0.0300% or more.
[0167] On the other hand, if the Al content exceeds 0.5000%, coarse oxides are generated in the steel, and the hydrogen embrittlement resistance of the hot stamping body is reduced. Therefore, the Al content is set to 0.5000% or less. The Al content is preferably 0.4000% or less, 0.3000% or less, 0.2000% or less, 0.1500% or less, or 0.1000% or less.
[0168] [Nb: 0.0010~0.100%]
[0169] Nb is an element that forms carbonitrides in steel and improves the strength of hot stamping parts by precipitation strengthening. If the Nb content is less than 0.0010%, the desired strength cannot be obtained. Therefore, the Nb content is set to 0.0010% or more. The Nb content is preferably 0.005% or more, 0.009% or more, or 0.015% or more.
[0170] On the other hand, if the Nb content exceeds 0.100%, a large amount of carbonitrides are generated in the steel, and the hydrogen embrittlement resistance of the hot stamped body is reduced. Therefore, the Nb content is set to 0.100% or less. The Nb content is preferably 0.080% or less, 0.060% or less, or 0.050% or less.
[0171] [Ti: 0.010~0.200%]
[0172] Ti is an element that forms carbonitrides in steel and improves the strength of hot stamping parts by precipitation strengthening. If the Ti content is less than 0.010%, the desired strength cannot be obtained. Therefore, the Ti content is set to 0.010% or more. The Ti content is preferably 0.015% or more, 0.020% or more, or 0.025% or more.
[0173] On the other hand, if the Ti content exceeds 0.200%, a large amount of carbonitrides are generated in the steel and the hydrogen embrittlement resistance of the hot stamping body is reduced. Therefore, the Ti content is set to 0.200% or less. The Ti content is preferably 0.180% or less, 0.150% or less, 0.100% or less, 0.080% or less, 0.060% or less, or 0.050% or less.
[0174] [B: 0.0005~0.0200%]
[0175] B is an element that improves the hardenability of steel. If the B content is less than 0.0005%, the desired strength cannot be obtained. Therefore, the B content is set to 0.0005% or more. The B content is preferably 0.0010% or more, 0.0015% or more, or 0.0020% or more.
[0176] On the other hand, if the B content exceeds 0.0200%, coarse intermetallic compounds are formed in the hot stamping body, and the hydrogen embrittlement resistance of the hot stamping body is reduced. Therefore, the B content is set to 0.0200% or less. The B content is preferably 0.0150% or less, 0.0100% or less, 0.0080% or less, 0.0060% or less, or 0.0040% or less.
[0177] [Cr: 0.010~0.80%]
[0178] Cr is an element that improves the strength of the hot stamped body by being dissolved in the original austenite grains during heating before hot stamping. If the Cr content is less than 0.010%, the desired strength cannot be obtained. Therefore, the Cr content is set to 0.010% or more. The Cr content is preferably 0.05% or more, 0.10% or more, 0.15% or more, or 0.20% or more.
[0179] On the other hand, if the Cr content exceeds 0.80%, coarse intermetallic compounds are formed in the hot stamping body, and the hydrogen embrittlement resistance of the hot stamping body is deteriorated. Therefore, the Cr content is set to 0.80% or less. The Cr content is preferably 0.70% or less, 0.60% or less, 0.50% or less, or 0.40% or less.
[0180] [Mo: 0.0010~1.000%]
[0181] Mo is an element that improves the hardenability of steel. If the Mo content is less than 0.0010%, the desired strength cannot be obtained. Therefore, the Mo content is set to 0.0010% or more. The Mo content is preferably 0.005% or more, 0.010% or more, 0.050% or more, or 0.100% or more.
[0182] On the other hand, if the Mo content exceeds 1.000%, coarse intermetallic compounds are formed in the hot stamping body, and the hydrogen embrittlement resistance of the hot stamping body is deteriorated. Therefore, the Mo content is set to 1.000% or less. The Mo content is preferably 0.800% or less, 0.600% or less, 0.500% or less, or 0.300% or less.
[0183] The basic chemical composition of the hot stamping steel sheet according to the embodiment of the present invention is as described above. Furthermore, the hot stamping steel sheet may contain at least one of the following optional elements as needed to replace part of the remaining Fe. For example, the hot stamping steel sheet may contain at least one selected from the group consisting of Co: 0 to 2.00%, Ni: 0 to 3.00%, Cu: 0 to 1.00%, V: 0 to 1.00% and W: 0 to 1.000%. In addition, the hot stamping steel sheet may contain at least one selected from the group consisting of Ca: 0 to 0.010%, Mg: 0 to 1.000% and REM: 0 to 1.000%. In addition, the hot stamping steel sheet may contain at least one selected from the group consisting of Sb: 0 to 1.000%, Zr: 0 to 1.000% and Sn: 0 to 1.000%. In addition, the hot stamping steel sheet may contain As: 0 to 0.100%. These optional elements are described in detail below.
[0184] [Co: 0~2.00%]
[0185] Co is an element that improves the strength of a hot stamped body by solid solution strengthening. The Co content may be 0.001% or more, but in order to reliably obtain this effect, the Co content is preferably set to 0.01% or more or 0.05% or more.
[0186] On the other hand, even if a large amount is contained, the above effect is saturated, so the Co content is preferably set to 2.00% or less. The Co content may be 1.80% or less, 1.50% or less, 1.00% or less, 0.80% or less, or 0.60% or less.
[0187] [Ni: 0~3.00%]
[0188] Ni has the effect of improving the strength of the hot stamped body by dissolving in austenite grains during heating in the hot stamping process. The Ni content may be 0.001% or more, but in order to reliably obtain this effect, the Ni content is preferably set to 0.01% or more.
[0189] On the other hand, even if a large amount is contained, the above effect is saturated, so the Ni content is preferably set to 3.00% or less. The Ni content may be less than 3.00%, 2.80% or less, 2.50% or less, 2.00% or less, 1.50% or less, 1.00% or less, or 0.80% or less.
[0190] [Cu: 0-1.00%]
[0191] Cu has the effect of improving the strength of the hot stamped body by dissolving in austenite grains during heating in the hot stamping process. The Cu content may be 0.001% or more, but in order to reliably obtain this effect, the Cu content is preferably set to 0.01% or more or 0.05% or more.
[0192] On the other hand, even if a large amount is contained, the above-mentioned effect is saturated, so the Cu content is preferably set to 1.00% or less. The Cu content may be 0.80% or less, 0.60% or less, 0.50% or less, or 0.30% or less.
[0193] [V: 0~1.00%]
[0194] V has the effect of forming carbonitrides in steel and improving the strength of the hot stamped body by precipitation strengthening. The V content may be 0.001% or more, but in order to reliably obtain this effect, the V content is preferably set to 0.01% or more or 0.05% or more.
[0195] On the other hand, even if V is contained in a large amount, the above-mentioned effect is saturated, so the V content is preferably set to 1.00% or less. The V content may be 0.80% or less, 0.60% or less, 0.50% or less, or 0.30% or less.
[0196] [W: 0~1.000%]
[0197] W is an element that improves the hardenability of steel. The W content may be 0.001% or more, but in order to reliably obtain this effect, the W content is preferably set to 0.005% or more or 0.010% or more.
[0198] On the other hand, even if a large amount is contained, the above-mentioned effect is saturated, so the W content is preferably set to 1.000% or less. The W content may be 0.800% or less, 0.600% or less, 0.500% or less, or 0.300% or less.
[0199] [Ca: 0~0.010%]
[0200] Ca is an element that suppresses the formation of oxides. The Ca content may be 0.0001% or more, but in order to reliably obtain this effect, the Ca content is preferably set to 0.0005% or more or 0.001% or more.
[0201] On the other hand, even if a large amount is contained, the above effect is saturated, so the Ca content is preferably set to 0.010% or less. The Ca content may be 0.008% or less, 0.006% or less, 0.004% or less, 0.003% or less, or 0.002% or less.
[0202] [Mg: 0~1.000%]
[0203] Mg forms oxides or sulfides in the molten steel, inhibits the formation of coarse MnS, disperses fine oxides in large quantities, and contributes to the refinement of the metal structure. The Mg content may be 0.0001% or more, but in order to reliably obtain these effects, the Mg content is preferably set to 0.0005% or more or 0.001% or more.
[0204] On the other hand, even if a large amount is contained, the above effect is saturated, so the Mg content is preferably set to 1.000% or less. The Mg content may be 0.500% or less, 0.100% or less, 0.050% or less, 0.010% or less, 0.005% or less, or 0.002% or less.
[0205] [REM: 0~1.000%]
[0206] REM is an element that suppresses the generation of oxides. The REM content may be 0.0001% or more, but in order to reliably obtain this effect, the REM content is preferably set to 0.0005% or more or 0.001% or more.
[0207] On the other hand, even if a large amount is contained, the above effect is saturated, so the REM content is preferably set to 1.000% or less. The REM content may be 0.500% or less, 0.100% or less, 0.050% or less, 0.010% or less, 0.005% or less, or 0.002% or less.
[0208] It should be noted that in this embodiment, REM is a general term for 17 elements including scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71, which are lanthanide elements, and the REM content is the total content of these elements.
[0209] [Sb: 0~1.000%]
[0210] Sb is an element that suppresses the generation of oxides. In order to reliably obtain this effect, the Sb content is preferably set to 0.001% or more.
[0211] On the other hand, even if a large amount is contained, the above-mentioned effect is saturated, so the Sb content is preferably set to 1.000% or less. The Sb content may be 0.800% or less, 0.500% or less, 0.200% or less, or 0.100% or less.
[0212] [Zr: 0~1.000%]
[0213] Zr is an element that suppresses the generation of oxides. In order to reliably obtain this effect, the Zr content is preferably set to 0.001% or more.
[0214] On the other hand, even if a large amount is contained, the above effect is saturated, so the Zr content is preferably set to 1.000% or less. The Zr content may be 0.800% or less, 0.500% or less, 0.200% or less, or 0.100% or less.
[0215] [Sn: 0~1.000%]
[0216] Sn is an element that suppresses the generation of oxides. In order to reliably obtain this effect, the Sn content is preferably set to 0.001% or more.
[0217] On the other hand, even if a large amount of Sn is contained, the above-mentioned effect is saturated, so the Sn content is preferably set to 1.000% or less. The Sn content may be 0.800% or less, 0.500% or less, 0.200% or less, or 0.100% or less.
[0218] [As: 0~0.100%]
[0219] As contributes to the refinement of prior austenite grains by lowering the austenite single-phase transformation temperature. In order to reliably obtain this effect, the As content is preferably set to 0.001% or more.
[0220] On the other hand, even if a large amount is contained, the above-mentioned effect is saturated, so the As content is preferably set to 0.100% or less. The As content may be 0.080% or less, 0.050% or less, 0.020% or less, or 0.010% or less.
[0221] In the hot stamping steel sheet of the embodiment of the present invention, the remainder other than the above elements is composed of Fe and impurities. Impurities are components mixed into raw materials such as ore and scrap iron due to various factors in the manufacturing process when the hot stamping steel sheet is industrially manufactured.
[0222] The chemical composition of the hot stamping steel sheet can be measured by general analytical methods. For example, ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry) can be used for measurement. It should be noted that C and S are measured using the combustion-infrared absorption method, N using the inert gas melting-thermal conductivity method, and O using the inert gas melting-non-dispersive infrared absorption method.
[0223] When the surface of the steel sheet for hot stamping has a plating layer, the chemical composition analysis may be performed after the plating layer is removed by mechanical grinding.
[0224] [Ferrite: 10% or more, pearlite: 10% or more, total of ferrite and pearlite: 80% or more]
[0225] The metal structure of the hot stamping steel sheet according to the embodiment of the present invention includes ferrite: 10% or more and pearlite: 10% or more in terms of area ratio, and the total of ferrite and pearlite is 80% or more. Pearlite becomes the starting point of austenite grains during heating for hot stamping, so it must be present in the metal structure at an area ratio of 10% or more. In addition, in the present embodiment, by including pearlite in combination with ferrite, uniform dispersion of pearlite can be achieved. The area ratios of ferrite and pearlite can be any value of 10% or more within the range in which their total is 80% or more, for example, they can also be independently 20% or more, 30% or more, 40%, 50% or more, or 60% or more. The upper limit is not particularly limited, but the area ratios of ferrite and pearlite can also be, for example, 85% or less, 80% or less, or 70% or less, respectively and independently. The total area ratio of ferrite and pearlite can also be 85% or more, 90% or more, or 95% or more. The upper limit is not particularly limited, but the total area ratio of ferrite and pearlite can also be 100%, for example, it can be 99% or less or 98% or less. The remaining structure is not particularly limited, but it can also contain at least one of bainite, martensite, residual austenite and carbide. Carbides are, for example, Fe carbides, which are sometimes generated in trace amounts at the interface between ferrite phase and ferrite phase. The area ratio of the remaining structure is 20% or less, for example, it can be 17% or less, 15% or less, 12% or less, 10% or less, 8% or less, 5% or less or 3% or less.
[0226] [Pearlite dispersion index: 0.50 or more]
[0227] In the metal structure of the hot stamping steel sheet according to the embodiment of the present invention, pearlite must be uniformly dispersed. In the present embodiment, such uniform dispersion of pearlite is achieved by controlling the dispersion index of pearlite to be 0.50 or more. The dispersion index of pearlite is obtained by dividing the number of A / B boundaries (boundaries between ferrite phase and pearlite phase) by the total number of A / A boundaries (boundaries between ferrite phase and ferrite phase), the number of B / B boundaries (boundaries between pearlite phase and pearlite phase), and the number of A / B boundaries (boundaries between ferrite phase and pearlite phase) in the electron microscope image of the metal structure of the hot stamping steel sheet mainly composed of ferrite and pearlite. A high dispersion index of pearlite means that the ratio of A / B boundaries is high in the metal structure mainly composed of ferrite and pearlite, that is, the number of boundaries between ferrite phase and pearlite phase is large. Therefore, by controlling the dispersion index of pearlite to a higher value, the portion where pearlite is connected can be reduced, and a more uniform dispersion of pearlite can be achieved. According to the present embodiment, by controlling the dispersion index of pearlite to be above 0.50, the standard deviation of the hardness distribution of the original austenite grains below 150Hv can be achieved in the final metal structure of the hot stamping body due to the uniform dispersion of such pearlite. As a result, the unevenness of the hardness of the original austenite grains in the metal structure of the hot stamping body can be reduced, and the increase in local hardness can be significantly suppressed. Therefore, despite having a high tensile strength, such as a high tensile strength of more than 2200MPa, the hydrogen embrittlement resistance can be significantly improved. The higher the dispersion index of pearlite, the more preferred, for example, it can also be above 0.52, above 0.55, above 0.58, above 0.60, above 0.62 or above 0.65. The upper limit is not particularly limited, but the dispersion index of pearlite can also be, for example, below 0.80, below 0.75 or below 0.70.
[0228] The dispersion index of pearlite is determined as follows. First, using a scanning electron microscope, an electron channel contrast image with a range of 35 μm in a direction perpendicular to the plate thickness direction and 10 μm in the plate thickness direction is obtained in a cross section perpendicular to the surface with a 1 / 4 position of the plate thickness as the center. For this measurement, specifically, an EBSD analysis device consisting of a thermal field emission scanning electron microscope and an EBSD detector can be used, for example, an EBSD analysis device consisting of a JSM-7001F made by JEOL and a DVC5 detector made by TSL can be used. Then, 10 straight lines perpendicular to the plate thickness direction are drawn at intervals of 1 μm in the obtained electron channel contrast image. Then, the phase boundaries intersecting these straight lines are classified into A / A boundaries (boundaries between ferrite phase and ferrite phase), B / B boundaries (boundaries between pearlite phase and pearlite phase) and A / B boundaries (boundaries between ferrite phase and pearlite phase) and the intersection of each boundary is calculated. Next, the ratio of the A / B boundaries in the field of view is obtained by dividing the number of intersections of the A / B boundaries by the total number of intersections, i.e., the number of intersections of the A / A boundaries, the number of intersections of the B / B boundaries, and the number of intersections of the A / B boundaries. The same procedure is performed on the same sample in 5 fields of view, and the average value of the ratio of the A / B boundaries in the 5 fields of view is determined as the dispersion index of the pearlite.
[0229] [Plate thickness]
[0230] The hot stamping steel plate of the embodiment of the present invention is not particularly limited, but has a plate thickness of 0.1 to 4.0 mm, for example. The plate thickness may be 0.2 mm or more, 0.4 mm or more, 0.6 mm or more, 0.8 mm or more, or 1.0 mm or more. Similarly, the plate thickness may be 3.6 mm or less, 3.2 mm or less, 2.8 mm or less, 2.4 mm or less, or 2.0 mm or less. In the case where the hot stamping steel plate is a hot-rolled steel plate, the plate thickness may be, for example, 1.0 to 4.0 mm. On the other hand, in the case where the hot stamping steel plate is a cold-rolled steel plate, the plate thickness may be, for example, 0.1 to 2.0 mm.
[0231] [Plating]
[0232] The hot stamping steel sheet of the embodiment of the present invention may also have a coating on the surface. By having a coating on the surface, the corrosion resistance can be improved after hot stamping. Examples of the coating include aluminum coating, aluminum-zinc coating, aluminum-silicon coating, hot-dip galvanizing, electroplated zinc coating, alloyed hot-dip galvanizing, zinc-nickel coating, aluminum-magnesium-zinc coating, and the like.
[0233] <Hot stamping body>
[0234] In the present invention, in addition to the above-mentioned hot stamping steel sheet, a hot stamping formed body manufactured using the hot stamping steel sheet is also provided. Therefore, the hot stamping formed body of an embodiment of the present invention is described in more detail below. The hot stamping formed body is characterized in that it has the following chemical composition in mass %:
[0235] C: 0.40~0.70%,
[0236] Si: 0.010~1.300%,
[0237] Mn: 0.60~3.00%,
[0238] P: 0.100% or less,
[0239] S: 0.0100% or less,
[0240] N: 0.0200% or less,
[0241] O: 0.0200% or less,
[0242] Al: 0.0010~0.5000%,
[0243] Nb: 0.0010~0.100%,
[0244] Ti: 0.010~0.200%,
[0245] B: 0.0005~0.0200%,
[0246] Cr: 0.010~0.80%,
[0247] Mo: 0.0010~1.000%,
[0248] Co: 0-2.00%,
[0249] Ni: 0-3.00%,
[0250] Cu: 0-1.00%,
[0251] V: 0~1.00%,
[0252] W: 0~1.000%、
[0253] Ca: 0~0.010%
[0254] Mg: 0~1.000%,
[0255] REM: 0~1.000%、
[0256] Sb: 0~1.000%,
[0257] Zr: 0~1.000%,
[0258] Sn: 0~1.000%,
[0259] As: 0 to 0.100%, and
[0260] The rest: Fe and impurities.
[0261] The hot stamping formed body has the following metal structure:
[0262] Contains at least one of martensite, bainite and tempered martensite in an area ratio of 90% or more in total,
[0263] The standard deviation of the hardness distribution of prior austenite grains at the position of 1 / 4 of the plate thickness is 150 Hv or less.
[0264] [Chemical composition of hot stamped body]
[0265] The chemical composition is substantially unchanged by hot stamping, so the chemical composition of the hot stamped body is the same as that of the hot stamping steel sheet described previously. Therefore, the description of each element and the remainder associated with the chemical composition of the hot stamping steel sheet described previously is applicable not only to the hot stamping steel sheet but also to the hot stamped body.
[0266] [At least one of martensite, bainite and tempered martensite: 90% or more in total]
[0267] The metal structure of the hot stamping formed body contains at least one of martensite, bainite and tempered martensite in total of more than 90% by area ratio. The remaining structure is not particularly limited, but it may also contain at least one of ferrite, residual austenite and pearlite in an amount of less than 10%. Martensite, bainite and tempered martensite are very hard structures, so by including at least one of martensite, bainite and tempered martensite in total of more than 90% by area ratio in the hot stamping formed body, high tensile strength, specifically a tensile strength of more than 2200MPa, can be achieved. The total area ratio of at least one of martensite, bainite and tempered martensite may also be preferably 92% or more or 94% or more, and more preferably 95% or more or 97% or more. The upper limit of the total area ratio of at least one of martensite, bainite and tempered martensite is not particularly limited, and may also be 100%.
[0268] [Identification of metal structure and calculation of area ratio]
[0269] The identification of the metal structure in the hot stamping formed body and the hot stamping steel sheet described above and the calculation of the area ratio are performed as follows. First, a sample is cut from an arbitrary position at a distance of 50 mm or more from the end face of the steel material (a position avoiding the end if the sample cannot be collected from this position) in such a way that a plate thickness section perpendicular to the surface can be observed. The size of the sample also varies depending on the measuring device, but is set to a size of about 10 mm that can be observed in a direction perpendicular to the plate thickness direction.
[0270] After the cross section of the above sample is polished with silicon carbide paper of #600 to #1500, it is finished into a mirror surface using a liquid obtained by dispersing diamond powder with a particle size of 1 to 6 μm in a diluent such as alcohol or pure water. Next, the observation surface is finished by electrolytic polishing. At any position in the length direction of the sample cross section and at a depth of 1 / 4 of the plate thickness, an area of 50 μm in length and 50 μm in the plate thickness direction is measured by electron backscatter diffraction at a measurement interval of 0.1 μm to obtain crystal orientation information. In the measurement, an EBSD analysis device consisting of a thermal field emission scanning electron microscope and an EBSD detector can be used. For example, an EBSD analysis device consisting of JSM-7001F manufactured by JEOL and a DVC5 detector manufactured by TSL can be used. At this time, the vacuum degree in the EBSD analysis device can also be set to 9.6×10 -5 Pa or less, the acceleration voltage can also be set to 15 kV, and the irradiation current level can also be set to 13.
[0271] For the obtained crystal orientation information, the "Phase Map" function in the software "OIM Analysis (registered trademark)" attached to the EBSD analysis device is used to judge the area with a crystal structure of fcc as retained austenite. By calculating the area ratio of the retained austenite, the area ratio of the retained austenite is obtained. Next, the area with a crystal structure of bcc is judged as bainite, tempered martensite, martensite and ferrite. For these areas, the "Grain Average Misorientation" function in the software "OIM Analysis (registered trademark)" attached to the EBSD analysis device is used. Under the condition that the 5° grain boundary is regarded as the crystal grain boundary, the area with a "Grain Average Misorientation" of less than 0.5° is extracted as ferrite. By calculating the area ratio of the extracted ferrite, the area ratio of ferrite is obtained.
[0272] Next, the remaining area (the area where "Grain Average Misorientation" exceeds 0.5°) is set to the total area ratio of martensite, tempered martensite and bainite. For carbides, in the same field of view as the EBSD observation, the material with a granular shape in the area with bright contrast in the secondary electron image taken using a scanning electron microscope is judged as carbide, and the area ratio of the corresponding area is calculated to obtain the area ratio of carbide. The area ratio of pearlite is calculated by subtracting the area ratio of retained austenite, the area ratio of bainite, tempered martensite, the area ratio of martensite and ferrite, and the area ratio of carbides from 100%.
[0273] [Standard deviation of hardness distribution of prior austenite grains at the 1 / 4 plate thickness position: 150 Hv or less]
[0274] In an embodiment of the present invention, the standard deviation of the hardness distribution of the original austenite grains at the 1 / 4 position of the plate thickness of the hot stamped formed body is less than 150Hv. If the hardness of the original austenite grains is uneven, it sometimes leads to an increase in local hardness and causes hydrogen embrittlement cracking. According to an embodiment of the present invention, by controlling the standard deviation of the hardness distribution of the original austenite grains at the 1 / 4 position of the plate thickness of the hot stamped formed body to be less than 150Hv and reducing the unevenness of the hardness of the original austenite grains, the increase in local hardness that becomes the starting point of hydrogen embrittlement cracking can be reliably suppressed. Preferably, the standard deviation is less than 140Hv, less than 130Hv, less than 120Hv or less than 110Hv. The lower limit is not particularly limited, but the standard deviation of the hardness distribution of the original austenite grains at the 1 / 4 position of the plate thickness of the hot stamped formed body can also be, for example, more than 50Hv, more than 60Hv or more than 80Hv.
[0275] In an embodiment of the present invention, as described above, it is important to control the standard deviation of the hardness distribution of the original austenite grains at the 1 / 4 position of the plate thickness of the hot stamped body (not the hardness distribution of the entire metal structure at the 1 / 4 position of the plate thickness, but the hardness distribution of the original austenite grains present in the metal structure) to be less than 150Hv to reduce the unevenness of the hardness of the original austenite grains, so it is not necessary to control the hardness of the original austenite grains themselves to a specific range. Therefore, the hardness of the original austenite grains at the 1 / 4 position of the plate thickness of the hot stamped body is not particularly limited, but for example, it can also be greater than 500Hv and / or less than 1000Hv. The hardness of the original austenite grains at the 1 / 4 position of the plate thickness of the hot stamped body refers to the average of the total hardness measurement values measured in the method for determining the standard deviation of the hardness distribution of the original austenite grains described below.
[0276] The standard deviation of the hardness distribution of the original austenite grains is determined as follows. First, a sample is cut out from any position of the hot stamping body that is more than 50 mm away from the end face in such a way that a cross section (plate thickness cross section) perpendicular to the surface can be observed. The sample also varies depending on the measuring device, but is set to a size that allows observation of 10 mm in a direction perpendicular to the plate thickness direction. After the cross section of the sample is ground using #600 to #1500 silicon carbide paper, it is finished into a mirror surface using a liquid obtained by dispersing diamond powder with a particle size of 1 to 6 μm in a diluent such as alcohol and pure water. For the cross section finished into a mirror surface, a micro-Vickers hardness tester is used at a depth of 1 / 4 of the plate thickness from the surface to measure the Vickers hardness in a direction parallel to the plate surface, with a load of 1 gf, and at intervals of more than 3 times the indentation, to obtain a total of more than 100 measured values. Next, the same sample is measured using an EBSD analyzer, and referring to the obtained structural analysis results, only the measurement points with indentations in the original austenite grains (i.e., the indentations are not covered by grain boundaries) are extracted. Finally, the standard deviation obtained based on the measured values of the Vickers hardness of more than 20 different original austenite grains extracted is determined as the standard deviation of the hardness distribution of the original austenite grains at the 1 / 4 position of the plate thickness of the hot stamped formed body. For EBSD measurement, an EBSD analyzer consisting of a thermal field emission scanning electron microscope and an EBSD detector can be used. For example, an EBSD analyzer consisting of a JSM-7001F manufactured by JEOL and a DVC5 detector manufactured by TSL can be used. At this time, the vacuum degree in the EBSD analyzer can also be set to 9.6×10 -5 Pa or less, the acceleration voltage may be set to 15 kV, and the irradiation current level may be set to 13. The crystal orientation map of prior austenite grains was prepared by the method described in Acta Materialia, 58 (2010), 6393-6403, and the prior austenite grains were identified based on the crystal orientation map.
[0277] [Plating]
[0278] The hot stamping body of this embodiment may also have a coating on the surface. By having a coating on the surface, corrosion resistance can be improved. Examples of the coating include aluminum coating, aluminum-zinc coating, aluminum-silicon coating, hot-dip galvanizing, electroplated zinc coating, alloyed hot-dip galvanizing, zinc-nickel coating, aluminum-magnesium-zinc coating, and the like.
[0279] [Mechanical properties]
[0280] According to the hot stamping formed body of the embodiment of the present invention, it is possible to achieve excellent mechanical properties, for example, a tensile strength of 2200 MPa or more. The tensile strength is preferably 2300 MPa or more, more preferably 2400 MPa or more, and most preferably 2500 MPa or more or 2600 MPa or more. The upper limit is not particularly limited, but for example, the tensile strength may be 3500 MPa or less, 3300 MPa or less, or 3000 MPa or less. The tensile strength of the hot stamping formed body is measured by making a No. 5 test piece according to JIS Z 2241:2011 and performing a tensile test.
[0281] The hot stamped parts according to the embodiments of the present invention have excellent hydrogen embrittlement resistance despite having a high tensile strength of 2200 MPa or more as described above, and are therefore very useful as automotive frame members, bumpers, and other structural members and reinforcing members requiring strength.
[0282] <Manufacturing method>
[0283] Next, a preferred method for manufacturing a hot stamping steel sheet and a hot stamping formed body according to an embodiment of the present invention is described. The following description is intended to exemplify a characteristic method for manufacturing a hot stamping steel sheet and a hot stamping formed body according to an embodiment of the present invention, and is not intended to limit the hot stamping steel sheet and the hot stamping formed body to the hot stamping steel sheet and the hot stamping formed body manufactured by the manufacturing method described below.
[0284] <Method for producing hot stamping steel sheet>
[0285] The method for manufacturing a hot stamping steel sheet according to an embodiment of the present invention is effective in controlling the finish rolling conditions and the subsequent cooling conditions. Specifically, the method for manufacturing a hot stamping steel sheet according to an embodiment of the present invention is characterized in that it includes the following steps:
[0286] A step of hot rolling a slab having the chemical composition described above in relation to a steel sheet for hot stamping, the step comprising heating the slab and then performing finish rolling, wherein the reduction ratio in the final stage of the finish rolling is 40% or more (hot rolling step);
[0287] A step of rapidly cooling the obtained hot-rolled steel sheet within 1.0 second after the finish rolling, and then cooling it at an average cooling rate of 90° C. / second or more (cooling step); and
[0288] A step of coiling the hot-rolled steel sheet at a temperature of 500 to 700° C. (coiling step).
[0289] Hereinafter, each step will be described in detail.
[0290] [Hot rolling process]
[0291] [Heating of slab]
[0292] First, a slab having the chemical composition described above in connection with a steel plate for hot stamping is heated. The casting method of the molten steel is not particularly limited, and the molten steel may be produced by a continuous casting method, an ingot casting method, or a thin slab casting method. The heating before hot rolling is not particularly limited, but the slab used contains a relatively large amount of alloying elements in order to obtain a high-strength steel plate. Therefore, for the purpose of heating the slab before hot rolling to dissolve the alloying elements in the slab, the heating temperature may be above 1100°C.
[0293] [Rough rolling]
[0294] In the present method, for example, the heated slab may be subjected to rough rolling before finish rolling for the purpose of adjusting the thickness of the slab, etc. The conditions for the rough rolling are not particularly limited as long as the desired thin slab size can be ensured.
[0295] [Finish rolling]
[0296] The heated slab or the slab that has been rough-rolled as needed is then subjected to finish rolling. In this method, it is important to set the reduction rate of the final section in the finish rolling to 40% or more. By setting the reduction rate of the final section in the finish rolling to 40% or more, pearlite is evenly dispersed in the hot-rolled steel sheet after rolling. The pearlite becomes the starting point of austenite during heating in the hot stamping forming process described in detail later in connection with the method for manufacturing the hot stamped formed body. Therefore, if the pearlite is evenly dispersed, the unevenness of the original austenite grain size can be reduced in the hot stamped formed body. As a result, the unevenness of the hardness of the original austenite grains in the metal structure of the hot stamped formed body can be reduced, and the increase in local hardness can be significantly suppressed. Therefore, despite having a high tensile strength, for example, a high tensile strength of more than 2200MPa, the hydrogen embrittlement resistance can be significantly improved. It is more preferred that the reduction rate of the final section in the finish rolling is 45% or more or 50% or more.
[0297] In hot stamping steel sheets, there is a tendency to increase the amount of Mn added, for example, to add 0.60% or more Mn, in order to ensure high hardenability. In connection with this, the present inventors' research has revealed that at such a high Mn content, pearlite tends to be relatively connected and arranged in the hot-rolled steel sheet, so it is very difficult to evenly disperse pearlite in the metal structure of the hot-rolled steel sheet compared to the case of low Mn content. Therefore, it is believed that when such a high Mn content steel is finish rolled at a relatively low reduction rate of less than 40%, the presence of the pearlite-connected portion in the metal structure becomes particularly significant.
[0298] However, by setting the reduction rate of the final section in the finishing rolling to 40% or more, pearlite can be fully dispersed and arranged in the hot-rolled steel sheet after the hot rolling process and the subsequent cooling process and coiling process despite the high Mn content of more than 0.60%. Therefore, in the metal structure of the hot-rolled steel sheet subjected to such a reduction, the part where the pearlite is connected does not exist or is sufficiently reduced, so the unevenness of the original austenite grain size can be reduced in the structure after hot stamping. As a result, the unevenness of the hardness of the original austenite grains in the metal structure of the hot stamped body can be reduced. The upper limit of the reduction rate of the final section in the finishing rolling is not particularly limited. Even for a steel material with a high Mn content like this, in particular, by appropriately controlling the reduction rate of the final section in the finishing rolling, pearlite can be fully dispersed and arranged in the metal structure of the hot-rolled steel sheet, thereby reducing the unevenness of the original austenite grain size and suppressing the increase in local hardness.
[0299] The morphology of such a metal structure is dominated by the reduction ratio of the final stage in the finishing rolling, the average cooling rate in the subsequent cooling process, and the coiling temperature in the coiling process. For example, it is not particularly affected by the optional cold rolling or the subsequent annealing. The reason is that if the reduction ratio of the final stage in the finishing rolling is set to 40% or more to form a hot-rolled steel sheet, even if the hot-rolled steel sheet is cold-rolled and then annealed at a relatively high temperature, there is a high tendency to generate a metal structure in which carbides, grain boundaries, and retained austenite, which are the starting points of austenite, are dispersed after cooling. In general, if the reduction ratio of the final stage in the finishing rolling is excessively increased, there is a concern about cracking of the steel sheet during rolling. In particular, in the case of a high-strength steel sheet with a C content of 0.40% or more, if the reduction ratio of the final stage is excessively increased, in addition to the concern about cracking of such a steel sheet, the rolling load of the rolling mill is also significantly increased. Therefore, in the steel material having the same chemical composition as the hot stamping steel sheet according to the embodiment of the present invention, finish rolling in which the reduction ratio of the final section is 40% or more has not been performed in the past. Therefore, by setting the reduction ratio of the final section in the finish rolling to 40% or more, and then appropriately controlling the average cooling rate in the subsequent cooling process and the coiling temperature in the coiling process and combining them, the pearlite that becomes the starting point of the austenite grains can be uniformly dispersed during the heating of the hot stamping forming, which is a fact that was previously unknown. Therefore, of course, in association with this, the original austenite grains in the hot stamping formed body are homogenized, thereby reducing the unevenness of the hardness of the original austenite grains in the metal structure of the hot stamping formed body, which is also a fact that was previously unknown, and these facts were first clarified by the present inventors this time.
[0300] [Cooling process]
[0301] Next, the hot-rolled steel sheet after finish rolling is quenched within 1.0 second after the finish rolling. Ferrite is generally generated from the grain boundaries of austenite grains, so if the austenite grains become larger, the number of grain boundaries that become the starting point of ferrite will decrease. In this case, it becomes difficult to prevent the connection of pearlite and make it evenly dispersed. Therefore, by quenching the hot-rolled steel sheet immediately after the finish rolling, specifically, quenching the hot-rolled steel sheet within 1.0 second after the finish rolling, preferably within 0.8 seconds, the grain growth of austenite grains is suppressed, which becomes extremely important in the aspect of uniformly dispersing and generating pearlite in the hot-rolled steel sheet. The average cooling rate and cooling time during quenching are not particularly limited. For example, the average cooling rate is preferably 200 to 1000°C / second, and the cooling time is preferably 0.2 to 2.0 seconds.
[0302] Next, the hot-rolled steel sheet after rapid cooling is cooled at an average cooling rate of more than 90°C / second. If the cooling rate is slow, a large amount of bainite or austenite is generated and remains as residual austenite, and it becomes impossible to form a metal structure mainly composed of ferrite and pearlite. As a result, it becomes difficult to control the configuration of ferrite and pearlite, and in particular, it becomes difficult to achieve uniform dispersion of pearlite. On the other hand, by cooling at an average cooling rate of more than 90°C / second, a metal structure mainly composed of ferrite and pearlite can be formed, and more specifically, a metal structure in which the total area ratio of ferrite and pearlite is more than 80% can be formed. The average cooling rate is preferably more than 95°C / second. The upper limit is not particularly limited, but the average cooling rate can also be, for example, less than 200°C / second or less than 150°C / second.
[0303] [Coiling process]
[0304] Next, the hot-rolled steel sheet after finish rolling is coiled at a temperature of 500 to 700°C. If the coiling temperature is high, grain growth sometimes occurs and the uniform dispersion of pearlite is hindered. On the other hand, if the coiling temperature is low, bainite and martensite are generated and it becomes impossible to form a metal structure mainly composed of ferrite and pearlite. In contrast, by controlling the coiling temperature to 500 to 700°C, grain growth can be suppressed, and the ferrite can be prevented from being arranged in a connected manner in the hot-rolled steel sheet after rolling, so that pearlite can be evenly dispersed. The preferred coiling temperature is 505 to 650°C or 550 to 650°C. In addition, for the purpose of softening the hot-rolled steel sheet, the coiled material can also be subjected to a softening heat treatment. The method of the softening heat treatment is not particularly limited, and it can be set to general conditions.
[0305] [Pickling process]
[0306] After the coiling process and before the optional cold rolling process, pickling may be performed to remove the oxide scale formed on the surface of the hot-rolled steel sheet. Pickling may be performed under conditions suitable for removing the oxide scale, and may be performed once or in multiple times to reliably remove the oxide scale.
[0307] [Cold rolling process]
[0308] After the coiling process, cold rolling may be optionally performed. There is no particular limitation on cold rolling, and it may be performed under any suitable conditions. For example, the reduction ratio of cold rolling may be 30 to 80%. There is no particular limitation on the number of rolling passes and the reduction ratio of each pass, and they may be appropriately set so that the overall reduction ratio of cold rolling falls within the above range.
[0309] [Annealing process]
[0310] For example, after the cold rolling step, annealing may be optionally performed in order to adjust the metal structure and / or properties. The heating temperature of the annealing step is not particularly limited, but may be, for example, 800° C. or less.
[0311] [Plating process]
[0312] For the purpose of improving corrosion resistance, the surface of the hot-rolled steel sheet or the cold-rolled steel sheet may also be subjected to a plating treatment. The plating treatment may be a treatment such as hot-dip plating, alloyed hot-dip plating, or electroplating. For example, as a plating treatment, the steel sheet may be subjected to a hot-dip galvanizing treatment, or may be subjected to an alloying treatment after the hot-dip galvanizing treatment. As a coating, an aluminum coating, an aluminum-zinc coating, an aluminum-silicon coating, a hot-dip galvanizing layer, an electroplated zinc coating, an alloyed hot-dip galvanizing layer, a zinc-nickel coating, an aluminum-magnesium-zinc coating, or the like may be exemplified. The specific conditions of the plating treatment and the alloying treatment are not particularly limited, and may be any suitable conditions known to those skilled in the art.
[0313] [Quenching and tempering process]
[0314] For the purpose of correcting the shape of the steel sheet or adjusting the surface roughness, for example, the steel sheet after the annealing step or the plating step may be subjected to temper rolling.
[0315] <Method for producing hot stamped body>
[0316] Next, a method for manufacturing a hot stamped formed body according to an embodiment of the present invention is described. Specifically, the manufacturing method is characterized in that it includes a step of hot stamping a hot stamping steel sheet obtained by the manufacturing method of the hot stamping steel sheet described above, in which the hot stamping steel sheet is heated to a temperature range of 800°C to 1000°C and then maintained for 60 to 600 seconds.
[0317] [Hot stamping process]
[0318] The hot stamping steel sheet is hot stamped in the hot stamping process to produce a hot stamped body having a desired chemical composition and metal structure. In the present embodiment, austenite is generated starting from uniformly dispersed pearlite in the metal structure of the steel sheet during the heating of the hot stamping, and a hot stamped body having a metal structure with a desired hard structure and a desired original austenite grain size distribution with reduced unevenness, and thus having a metal structure with reduced unevenness of the hardness of the original austenite grains, can be produced through subsequent forming and cooling operations. From the viewpoint of obtaining such a desired hard structure and hardness distribution of the original austenite grains, it is preferred to heat the hot stamping steel sheet to a temperature range of 800°C to 1000°C and maintain it in the temperature range for 60 to 600 seconds. When the heating temperature is lower than 800°C, austenitization becomes insufficient, the area ratio of the desired hard structure (at least one of martensite, bainite and tempered martensite) cannot be obtained, and sometimes the tensile strength deteriorates. On the other hand, if the heating temperature exceeds 1000°C, the austenite undergoes excessive grain growth, and the desired original austenite grain size distribution cannot be obtained. As a result, the desired hardness distribution of the original austenite grains cannot be obtained, and the hydrogen embrittlement resistance is sometimes deteriorated. When the holding time is less than 60 seconds, as in the case where the heating temperature is less than 800°C, austenitization becomes insufficient, and the desired hard structure (at least one of martensite, bainite and tempered martensite) area ratio cannot be obtained, and the tensile strength is sometimes deteriorated. If the holding time exceeds 600 seconds, the austenite undergoes excessive grain growth, and the desired original austenite grain size distribution cannot be obtained. As a result, the desired hardness distribution of the original austenite grains cannot be obtained, and the hydrogen embrittlement resistance is sometimes deteriorated.
[0319] The heating atmosphere is not particularly limited and can be a normal condition, for example, as long as it is in the air, or a gas combustion atmosphere with a controlled air-fuel ratio, or a nitrogen atmosphere, the dew point can also be controlled in these gases. After being maintained in a temperature range of 800°C to 1000°C, hot stamping is performed. After hot stamping, it is cooled to a temperature range of 250°C or less at an average cooling rate of 20°C / second or more.
[0320] Examples of the heating method before hot stamping include furnace heating using an electric furnace, a gas furnace, or the like, flame heating, electric heating, high-frequency heating, and induction heating.
[0321] The hot stamping body of the present embodiment is obtained by the above method. After hot stamping, a tempering treatment at 130 to 600° C. or a baking hardening treatment after painting may also be performed. In addition, a part of the hot stamping body may be tempered by laser irradiation or the like to partially set a softened area.
[0322] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples at all.
[0323] Example
[0324] In the following examples, hot stamped bodies according to the embodiments of the present invention were produced under various conditions, and the tensile strength and hydrogen embrittlement resistance of the obtained hot stamped bodies were examined.
[0325] First, a molten steel having a chemical composition shown in Table 1 is cast by a continuous casting method to produce a slab. The remainder other than the components shown in Table 1 is Fe and impurities. The slabs are heated to a temperature of 1100°C or higher and rough rolled under specified conditions, followed by finish rolling, cooling and coiling under the conditions shown in Table 2. In all the inventive examples and comparative examples, the average cooling rate during rapid cooling after the finish rolling is in the range of 200 to 1000°C / second, and the cooling time is in the range of 0.2 to 2.0 seconds. Then, the obtained hot-rolled steel sheet is cold rolled at a specified reduction rate of 30 to 80%. Then, annealing, plating or temper rolling is performed on a portion of the steel sheets under specified conditions. Then, the obtained steel sheets are hot stamped under the conditions shown in Table 2. The heating atmosphere and heating method in the hot stamping process are gas combustion atmosphere (air-fuel ratio 0.85) and furnace heating except for those specifically indicated. After hot stamping, a portion of the hot stamped body is subjected to a tempering treatment or a partial softening treatment.
[0326] Table 1-1
[0327]
[0328] The underlined characters indicate outside the scope of the present invention.
[0329] Table 1-2
[0330]
[0331] The underlined characters indicate outside the scope of the present invention.
[0332] Table 1-3
[0333]
[0334] The underlined characters indicate outside the scope of the present invention.
[0335] Table 1-4
[0336]
[0337] The underlined characters indicate outside the scope of the present invention.
[0338] Table 1-5
[0339]
[0340] The underlined characters indicate outside the scope of the present invention.
[0341] Table 1-6
[0342]
[0343] The underlined characters indicate outside the scope of the present invention.
[0344] Table 1-7
[0345]
[0346] The underlined characters indicate outside the scope of the present invention.
[0347] Table 1-8
[0348]
[0349] The underlined characters indicate outside the scope of the present invention.
[0350] Table 2-1
[0351]
[0352] The underline indicates that the manufacturing conditions are not preferred.
[0353] Table 2-2
[0354]
[0355] The underline indicates that the manufacturing conditions are not preferred.
[0356] Table 2-3
[0357]
[0358] The underline indicates that the manufacturing conditions are not preferred.
[0359] Table 2-4
[0360]
[0361] The underline indicates that the manufacturing conditions are not preferred.
[0362] Table 2-5
[0363]
[0364] The underline indicates that the manufacturing conditions are not preferred.
[0365] Table 2-6
[0366]
[0367] The underline indicates that the manufacturing conditions are not preferred.
[0368] The properties of the obtained hot stamped parts were measured and evaluated by the following methods.
[0369] [tensile strength]
[0370] The tensile strength of the hot stamped body was obtained by preparing a No. 5 test piece from an arbitrary position of the hot stamped body and conducting a tensile test in accordance with JIS Z 2241: 2011. The crosshead speed was set to 1 mm / min.
[0371] [Hydrogen embrittlement resistance]
[0372] The hydrogen embrittlement resistance of the hot stamped formed body was evaluated as follows. First, a test piece of 1.2t×7.0W×68L (mm) was prepared and subjected to various stresses using a 4-point bending fixture.
[0373] The samples were immersed in hydrochloric acid (room temperature, pH = 4) for 48 hours to investigate the limit strain at which cracks occurred. The samples with a limit strain of 0.6% or more were evaluated as acceptable (O), and the samples with a limit strain of less than 0.6% were evaluated as unacceptable (×).
[0374] The hot stamping formed body with a tensile strength of 2200MPa or more and a qualified hydrogen embrittlement resistance is evaluated as a high-strength hot stamping formed body capable of suppressing hydrogen embrittlement. The results are shown in Table 3. In Table 3, the area ratio of ferrite and pearlite in the hot stamping steel plate after the coiling process and the dispersion index of pearlite are shown. The remaining structure other than ferrite and pearlite is bainite, martensite, residual austenite and / or a trace amount of carbide. Similarly, in Table 3, the area ratio of the hard structure in the hot stamping formed body and the standard deviation of the hardness distribution of the original austenite grains (original γ grains) at the 1 / 4 position of the plate thickness are shown. The area ratio of the hard structure refers to the sum of the area ratios of martensite, bainite and tempered martensite. In addition, the remaining structure other than the hard structure is ferrite, residual austenite and / or pearlite.
[0375] Table 3-1
[0376]
[0377] The underlined characters are outside the scope of the present invention and indicate undesirable property values.
[0378] Table 3-2
[0379]
[0380] The underlined characters are outside the scope of the present invention and indicate undesirable property values.
[0381] Table 3-3
[0382]
[0383] The underlined characters are outside the scope of the present invention and indicate undesirable property values.
[0384] Table 3-4
[0385]
[0386] The underlined characters are outside the scope of the present invention and indicate undesirable property values.
[0387] Table 3-5
[0388]
[0389] The underlined characters are outside the scope of the present invention and indicate undesirable property values.
[0390] Table 3-6
[0391]
[0392] The underlined characters are outside the scope of the present invention and indicate undesirable property values.
[0393] Referring to Table 3, for Comparative Example 1, the tensile strength is reduced due to the low C content. For Comparative Example 13, the strength becomes too high due to the high C content, and the hydrogen embrittlement resistance is reduced. For Comparative Example 14, the tensile strength is reduced due to the low Si content. For Comparative Example 25, due to the high Si content, the amount of ferrite in the hot stamping steel sheet increases, the desired metal structure cannot be obtained, and the dispersion index of pearlite becomes less than 0.50. As a result, the standard deviation of the hardness distribution of the original austenite grains in the hot stamping formed body cannot be controlled to the desired range, and the hydrogen embrittlement resistance is reduced. For Comparative Example 26, due to the low Mn content, the dispersion index of pearlite in the hot stamping steel sheet and the standard deviation of the hardness distribution of the original austenite grains in the hot stamping formed body cannot be controlled within the desired range, and the hydrogen embrittlement resistance is reduced. For Comparative Example 41, it is believed that due to the high Mn content, the phase transformation from austenite to pearlite in the hot rolled steel sheet is excessively promoted. As a result, the dispersion index of pearlite in the steel sheet for hot stamping and the standard deviation of the hardness distribution of the original austenite grains in the hot stamping formed body cannot be controlled within the desired range, and the hydrogen embrittlement resistance is reduced. Comparative Examples 50, 59, 68, 77, 78 and 90 have inappropriate P, S, N, O or Al contents, so the hydrogen embrittlement resistance is reduced. For Comparative Examples 91, 103, 115, 127 and 139, the strength cannot be fully improved due to the low Nb, Ti, B, Cr and Mo contents, and the tensile strength is reduced. For Comparative Examples 102, 114, 126, 138 and 150, it is believed that due to the high Nb, Ti, B, Cr and Mo contents, a large amount of carbonitrides or coarse intermetallic compounds are generated in the steel, resulting in a reduction in hydrogen embrittlement resistance.
[0394] As for Comparative Example 259, it is believed that due to the low reduction rate in the final stage of the hot rolling process, the pearlite cannot be uniformly dispersed in the hot rolled steel sheet after rolling. As a result, the dispersion index of pearlite in the steel sheet for hot stamping and the standard deviation of the hardness distribution of the original austenite grains in the hot stamping body cannot be controlled within the desired range, and the hydrogen embrittlement resistance is reduced. As for Comparative Example 270, it is believed that due to the long time from the end of the finish rolling to the start of the quenching, the grain growth of the austenite grains cannot be fully suppressed, and the ferrite is connected and arranged, and the pearlite cannot be uniformly dispersed. As a result, the dispersion index of pearlite in the steel sheet for hot stamping and the standard deviation of the hardness distribution of the original austenite grains in the hot stamping body cannot be controlled within the desired range, and the hydrogen embrittlement resistance is reduced. As for Comparative Example 271, since the average cooling rate after the quenching in the cooling process is slow, the desired metal structure cannot be formed in the steel sheet for hot stamping. As a result, the dispersion index of pearlite in the steel sheet for hot stamping and the standard deviation of the hardness distribution of the original austenite grains in the hot stamping formed body cannot be controlled within the desired range, and the hydrogen embrittlement resistance is reduced. For Comparative Example 276, due to the low coiling temperature, the desired metal structure cannot be formed in the steel sheet for hot stamping. As a result, the standard deviation of the hardness distribution of the original austenite grains in the hot stamping formed body cannot be controlled within the desired range, and the hydrogen embrittlement resistance is reduced. For Comparative Example 284, it is believed that due to the high coiling temperature, grain growth occurs and the uniform dispersion of pearlite is hindered. As a result, the dispersion index of pearlite in the steel sheet for hot stamping and the standard deviation of the hardness distribution of the original austenite grains in the hot stamping formed body cannot be controlled within the desired range, and the hydrogen embrittlement resistance is reduced.
[0395] In contrast, in the hot stamping steel sheets and hot stamping parts of all the inventive examples, the dispersion index of pearlite in the hot stamping steel sheets is controlled to be 0.50 or more by having a predetermined chemical composition and metal structure, and the standard deviation of the hardness distribution of the original austenite grains in the hot stamping parts is controlled to be 150 Hv or less, so that hydrogen embrittlement can be reliably suppressed despite having a high tensile strength of more than 2200 MPa. In addition, in the hot stamping parts of all the inventive examples, the hardness of the original austenite grains at the 1 / 4 position of the plate thickness (the average of the total hardness measurement values in each inventive example) is controlled within the range of 500 to 1000 Hv.
Claims
1. A steel sheet for hot stamping, which has the following chemical composition in mass %: C: 0.40-0.70%, Si: 0.010~1.300%, Mn: 0.60~3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0200% or less, O: 0.0200% or less, Al:0.0010~0.5000%、 Nb: 0.0010~0.100%, Ti: 0.010~0.200%, B:0.0005~0.0200%、 Cr:0.010~0.80%、 Mo: 0.0010~1.000%, Co: 0-2.00%, Ni: 0-3.00%, Cu: 0-1.00%, V:0~1.00%、 W:0~1.000%、 Ca: 0~0.010% Mg: 0~1.000%, REM: 0~1.000%、 Sb: 0~1.000%, Zr:0~1.000%、 Sn: 0~1.000%, As: 0 to 0.100%, and The rest: Fe and impurities. The hot stamping steel sheet has the following metal structure: Ferrite: 10% or more Pearlite: more than 10%, The total of ferrite and pearlite is more than 80%, The dispersion index of pearlite is 0.50 or more.
2. The hot stamping steel sheet according to claim 1, wherein: The chemical composition includes, by mass%, one or more selected from the group consisting of the following elements: Co: 0.001~2.00% Ni: 0.001~3.00%, Cu: 0.001~1.00%, V:0.001~1.00%、 W:0.001~1.000%、 Ca: 0.0001~0.010%, Mg: 0.0001~1.000%, REM: 0.0001~1.000%, Sb: 0.001~1.000%, Zr:0.001~1.000%、 Sn: 0.001~1.000% and As: 0.001~0.100%.
3. A hot stamping formed body having the following chemical composition in mass %: C:0.40~0.70%、 Si: 0.010~1.300%, Mn: 0.60~3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0200% or less, O: 0.0200% or less, Al:0.0010~0.5000%、 Nb: 0.0010~0.100%, Ti: 0.010~0.200%, B:0.0005~0.0200%、 Cr:0.010~0.80%、 Mo: 0.0010~1.000%, Co: 0-2.00%, Ni: 0-3.00%, Cu: 0-1.00%, V:0~1.00%、 W:0~1.000%、 Ca: 0~0.010% Mg: 0~1.000%, REM: 0~1.000%、 Sb: 0~1.000%, Zr:0~1.000%、 Sn: 0~1.000%, As: 0 to 0.100%, and The rest: Fe and impurities. The hot stamping formed body has the following metal structure: Contains at least one of martensite, bainite and tempered martensite in an area ratio of 90% or more in total, The standard deviation of the hardness distribution of prior austenite grains at the position of 1 / 4 of the plate thickness is 150 Hv or less.
4. The hot stamped body according to claim 3, wherein: The chemical composition includes, by mass%, one or more selected from the group consisting of the following elements: Co: 0.001~2.00% Ni: 0.001~3.00%, Cu: 0.001~1.00%, V:0.001~1.00%、 W:0.001~1.000%、 Ca: 0.0001~0.010%, Mg: 0.0001~1.000%, REM: 0.0001~1.000%, Sb: 0.001~1.000%, Zr: 0.001~1.000%, Sn: 0.001~1.000% and As: 0.001~0.100%.
Citation Information