Nonaqueous electrolyte solution and nonaqueous secondary battery

By adding vinyl carbonate and vinyl sulfite to the electrolyte of lithium-ion batteries and adopting a multi-stage injection process, the reduction and decomposition of acetonitrile electrolyte and insufficient coating are solved, and the lithium-ion secondary battery is realized Efficient charging, discharge and stabilization improve manufacturing efficiency and battery performance.

CN118901158APending Publication Date: 2024-11-05ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028278.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-10-24
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

When using acetonitrile as the electrolyte, existing lithium-ion batteries are prone to reduction and decomposition, resulting in a degradation of battery performance and insufficient negative electrode coating during the first charge, which affects battery capacity stability and manufacturing efficiency.

Method used

By adding vinyl carbonate and vinyl sulfite as coating forming agents to the electrolyte of a nonaqueous lithium-ion secondary battery, and using a multi-stage injection process, the concentration of acetonitrile and the proportion of electrolyte are adjusted to form a strong The negative electrode coating inhibits the reduction and decomposition of acetonitrile and the excessive reduction reaction of vinyl sulfite.

Benefits of technology

It realizes the efficient charging and discharge cycle characteristics and capacity stabilization of lithium-ion secondary batteries, improves manufacturing process efficiency, reduces negative electrode coating defects and overreactions, and improves battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901158A_ABST
    Figure CN118901158A_ABST
Patent Text Reader

Abstract

Provided is a non-aqueous electrolyte solution for a non-aqueous lithium ion secondary battery which is provided with a negative electrode containing graphite and which contains X mass% of the non-aqueous electrolyte solution with respect to the mass of the negative electrode excluding a negative electrode current collector (where X is 50-2000, inclusive). The non-aqueous electrolyte solution contains a lithium salt and a non-aqueous solvent, the non-aqueous solvent contains A vol% of acetonitrile with respect to the volume of the non-aqueous solvent, A is 5-70, and the non-aqueous electrolyte solution contains vinylene carbonate (VC) as an additive, and A is 5-70, inclusive, with respect to the non-aqueous electrolyte solution. The content of VC is (7 * A / X) mass% or more and 10 mass% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nonaqueous electrolyte and a nonaqueous secondary battery using the nonaqueous electrolyte. Background Art

[0002] The use of non-aqueous secondary batteries such as lithium-ion batteries is changing in the global trend of automobile electrification. Non-aqueous secondary batteries are characterized by light weight, high energy and long life, and are also widely used as power sources for various portable electronic devices. In recent years, they have also attracted attention in industrial uses represented by power tools such as electric tools and in power storage fields such as residential power storage systems. In particular, in order to develop batteries with excellent output performance in automotive batteries, research has also been conducted on electrolytes such as acetonitrile with low viscosity. On the other hand, in order to prevent the easily reduced solvent from undergoing reduction and decomposition in the negative electrode, additives that form a film on the negative electrode have been studied.

[0003] For example, Patent Document 1 describes that an additive such as vinylene carbonate is added to an electrolyte solvent to prevent decomposition of the electrolyte solvent in the negative electrode.

[0004] Patent document 2 discloses an invention related to a non-aqueous electrolyte for use in non-aqueous secondary batteries such as lithium ion batteries. Patent document 1 discloses a non-aqueous electrolyte solution formed by combining acetonitrile (AcN) and an additive having a LUMO (Lowest Unoccupied Molecular Orbital) and a HOMO (Highest Occupied Molecular Orbital) in a specific potential band.

[0005] Patent Document 3 describes an invention related to a multi-stage injection process when manufacturing lithium-ion batteries. Patent Document 3 studies that by adding a negative electrode coating forming additive exceeding 50% of the total electrolyte during initial injection, and then injecting again after initial charge and discharge, the battery cell expansion caused by gas during coating formation can be eliminated.

[0006] Patent document 4 describes an invention related to a multi-stage injection process when manufacturing a lithium ion battery. Patent document 4 studies a lithium ion secondary battery that can provide improved cycle characteristics by forming a good coating on the newly formed surface accompanied by the expansion of the negative electrode active material by injecting again after the initial charge and discharge.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2005-166553.

[0010] Patent document 2: International Publication No. 2012 / 057311.

[0011] Patent document 3: Japanese Patent Application Publication No. 2006-294282.

[0012] Patent document 4: Japanese Patent Application Publication No. 2010-129192. Summary of the invention

[0013] Problems to be solved by the invention

[0014] However, in an electrolyte solution containing a solvent as a main component, such as acetonitrile, which increases the resistance of a battery due to reduction, in order to prevent the reduction and decomposition thereof, a more detailed study of additives is required.

[0015] Vinylene carbonate, a representative additive for forming a negative electrode coating, is effective in preventing acetonitrile from decomposing on the negative electrode, but if a sufficient amount of the negative electrode active material is not added to form a coating, a high-quality negative electrode coating cannot be formed during the initial charge of the battery. In addition, the ratio of the amount of the negative electrode active material to the electrolyte varies depending on the design of the battery shape or battery capacity, and it is important to design the electrolyte so that the additive can be added in an appropriate amount accordingly.

[0016] This problem is not observed in the electrolyte with the carbonate ester having less influence produced by the reduction decomposition in the negative electrode as the main component, and it can be considered that it will only occur when the solvent that is easily reduced is the main component. However, in the above-mentioned patent document, there is no record of changing the amount of additives according to the battery design. Therefore, the first problem to be solved by the present invention is to provide an electrolyte that can stably drive the battery even if a solvent that is easily reductively decomposed such as acetonitrile is used as the main component.

[0017] Second, when manufacturing lithium-ion secondary batteries, the discharge capacity of the battery is not constant, especially when the initial capacity gradually increases from a state smaller than the expected capacity in the design. This change in capacity can be considered to be a phenomenon that is significantly different from the capacity reduction that occurs when the battery deteriorates normally, and is expected to occur when the electrolyte is difficult to diffuse in the electrode. If the capacity continues to increase in an unstable state, a large amount of charging and discharging is required until it stabilizes, and the manufacturing time increases, thereby reducing the efficiency of the manufacturing process.

[0018] Therefore, the second problem to be solved by the present invention is to promote the diffusion of lithium inside the electrode by using acetonitrile with low viscosity, and to prevent the reduction of acetonitrile by forming a strong negative electrode film during the initial charge, thereby quickly stabilizing the capacity of the battery.

[0019] Third, the electrolyte based on acetonitrile needs to form a coating on the negative electrode surface for suppressing reduction electrolysis, using a coating forming agent such as vinylene carbonate (VC) and vinyl sulfite (ES). As the effect of ES in the electrolyte, there are many patents on the film forming ability so far. On the other hand, the compounds produced by the excessive reduction of ES have not been discussed. In this context, the inventors found that when acetonitrile is contained in the electrolyte, due to the excessive reduction reaction of ES, a large amount of compounds containing sulfur atoms with a valence of more than -2 and less than 0 are deposited on the negative electrode coating. In addition, since they do not have ion conductivity, the battery performance is reduced.

[0020] In addition, in recent years, in the battery manufacturing process, a method of performing initial charge and discharge under reduced pressure conditions has been developed for the purpose of exhausting gas from the battery cell and impregnating the electrolyte. However, it has been confirmed that when applied to a high-concentration acetonitrile electrolyte, in addition to the volatilization of acetonitrile causing a significant change in the composition of the electrolyte, it can also cause defects due to insufficient electrolyte.

[0021] In order to solve this conventional problem, multi-stage injection has been considered as a method of increasing the concentration of the film-forming agent in the electrolyte before the initial charge while reducing the acetonitrile concentration. However, there is no report of applying this multi-stage injection process to an acetonitrile-based electrolyte.

[0022] Therefore, the third problem to be solved by the present invention is to provide a non-aqueous battery. In the manufacture of a non-aqueous battery containing an acetonitrile electrolyte, the concentration of the negative electrode film forming agent in the initial electrolyte can be increased by multi-stage injection, and the acetonitrile concentration can be reduced. In addition to suppressing the volatilization of the electrolyte under reduced pressure conditions, the reduction reaction of excess vinyl sulfite in the initial charge is also suppressed, and the desired battery performance is achieved.

[0023] Means for solving problems

[0024] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that the problems can be solved by the following technical means. That is, the present invention is as follows.

[0025] (1) A non-aqueous electrolyte, wherein the non-aqueous electrolyte is for a non-aqueous lithium ion secondary battery, the non-aqueous lithium ion secondary battery having a negative electrode containing graphite and containing X mass % of the non-aqueous electrolyte relative to the mass of the negative electrode excluding the negative electrode current collector, wherein X is 50 or more and 2000 or less, the non-aqueous electrolyte containing a lithium salt and a non-aqueous solvent, wherein the non-aqueous solvent contains A volume % of acetonitrile relative to the volume of the non-aqueous solvent, A is 5 or more and 70 or less, and the non-aqueous electrolyte contains vinylene carbonate (VC) as an additive, and the content of VC is (7×A / X) mass % or more and 10 mass % or less relative to the non-aqueous electrolyte.

[0026] (2) The non-aqueous electrolyte solution according to item 1, wherein X is 200 or less.

[0027] (3) The non-aqueous electrolyte solution according to item 1 or 2, wherein A is 16 or more and 35 or less.

[0028] (4) The nonaqueous electrolyte solution according to any one of items 1 to 3, wherein the content of the VC is (15×A / X) mass % or more and 9 mass % or less relative to the nonaqueous electrolyte solution.

[0029] (5) The non-aqueous electrolyte solution according to any one of items 1 to 4, wherein X is 98 or less.

[0030] (6) The nonaqueous electrolyte solution according to any one of items 1 to 5, wherein the nonaqueous electrolyte solution contains vinyl sulfite.

[0031] (7) The nonaqueous electrolyte solution according to any one of items 1 to 6, wherein the nonaqueous electrolyte solution contains at least one of sulfate ions and sulfite ions.

[0032] (8) The nonaqueous electrolyte solution according to any one of items 1 to 7, wherein the content of the VC is 7% by mass or less based on the nonaqueous electrolyte solution.

[0033] (9) The nonaqueous electrolyte solution according to any one of items 1 to 8, wherein X is 65 or more.

[0034] (10) A non-aqueous lithium ion secondary battery, wherein the non-aqueous lithium ion secondary battery comprises: a positive electrode having a positive electrode active material layer on one or both sides of a positive electrode collector; a negative electrode having a negative electrode active material layer containing the graphite on one or both sides of the negative electrode collector; a separator; and the non-aqueous electrolyte described in any one of items 1 to 9.

[0035] (11) A non-aqueous secondary battery comprising a negative electrode, a positive electrode, a separator and a non-aqueous electrolyte, wherein the non-aqueous secondary battery is charged at least once, the negative electrode comprising at least one inorganic lithium compound and one organic lithium compound that can be extracted by immersion in an extraction solvent, and the non-aqueous electrolyte comprising a lithium salt, acetonitrile as a non-aqueous solvent, and a cyclic carbonate.

[0036] (12) A non-aqueous secondary battery as described in item 11, wherein the non-aqueous secondary battery contains a component that can be extracted from the negative electrode by using water as the extraction solvent, and contains at least the following inorganic lithium compound (a) and the following organic lithium compounds (b) to (d), respectively.

[0037] (a) LiF.

[0038] (b) LiOCOOCH2CH2OCOOLi.

[0039] (c) CH3CH2OCOOLi.

[0040] (d) CH3OCOOLi.

[0041] Furthermore, the molar ratios of (a) to (d) relative to the total content of (a) to (d) are: (a) is 20 mol% to 70 mol%, (b) is 20 mol% to 70 mol%, (c) is 1 mol% to 20 mol%, and (d) is 1 mol% to 20 mol%.

[0042] (13) The nonaqueous secondary battery according to item 11 or 12, wherein the cyclic carbonate comprises ethylene carbonate and vinylene carbonate, and the molar ratio of vinylene carbonate to ethylene carbonate is 0.01 mol % to 30 mol %.

[0043] (14) The nonaqueous lithium ion secondary battery according to item 10 or the nonaqueous secondary battery according to any one of items 11 to 13, wherein the positive electrode active material of the positive electrode comprises lithium iron phosphate.

[0044] (15) The nonaqueous secondary battery according to any one of items 11 to 13, wherein the nonaqueous secondary battery uses the nonaqueous electrolyte solution according to any one of items 1 to 9.

[0045] (16) A secondary battery manufacturing process, wherein the secondary battery manufacturing process has at least two electrolyte injection steps of injecting a non-aqueous electrolyte into a battery casing, and has at least one charging step after the initial electrolyte injection step and before the final electrolyte injection step, and in the electrolyte injection step after the initial one, an electrolyte having a higher volume ratio of acetonitrile to the total electrolyte than the electrolyte used in the initial electrolyte injection step is injected into the battery casing.

[0046] (17) The secondary battery manufacturing process according to item 16, wherein in the electrolyte injection step after the first injection, an electrolyte containing 20 volume % or more and 100 volume % or less of acetonitrile is injected into the battery exterior.

[0047] (18) A non-aqueous secondary battery, wherein the non-aqueous secondary battery is a non-aqueous secondary battery comprising a non-aqueous electrolyte containing acetonitrile and vinyl sulfite in an amount of not less than 5 volume % and not more than 60 volume %, a positive electrode having a positive electrode active material layer on one or both sides of a positive electrode collector, a negative electrode having a negative electrode active material layer on one or both sides of a negative electrode collector, and a separator; and the non-aqueous secondary battery is a non-aqueous secondary battery in which the negative electrode coating after the initial charge and discharge contains a compound containing sulfur atoms with a valence of not less than -2 and not more than 0, and the compound contains at least one of sulfur or copper sulfide; and the non-aqueous secondary battery is obtained by the following method: having at least one charging step after the initial electrolyte injection step and before the final electrolyte injection step, and in the electrolyte injection step after the initial step, injecting into the battery outer casing an electrolyte having a higher volume ratio of acetonitrile to the total electrolyte than the electrolyte used in the initial electrolyte injection step.

[0048] (19) The nonaqueous secondary battery according to item 18, wherein the concentration of the vinyl sulfite in the nonaqueous electrolyte is 0.01% by volume or more and 4% by volume or less.

[0049] (20) The nonaqueous secondary battery according to item 18 or 19, wherein the nonaqueous electrolyte further contains vinylene carbonate.

[0050] Effects of the Invention

[0051] According to the first embodiment of the present invention, it is possible to provide a lithium ion secondary battery having high charge and discharge efficiency and stable charge and discharge cycle characteristics even when using an electrolyte solution containing acetonitrile.

[0052] According to the second embodiment of the present invention, a secondary battery having a coating suitable for preventing reductive decomposition of acetonitrile and containing low-viscosity acetonitrile to rapidly stabilize the initial battery capacity can be provided, which contributes to improving the efficiency of the manufacturing process.

[0053] According to the third embodiment of the present invention, as a method for reducing deposits on the negative electrode, a two-stage injection method has been developed, which can suppress the reduction reaction at the defective portion of the negative electrode coating that is unique to battery cells using a high-concentration acetonitrile electrolyte. In addition, by controlling or reducing the compounds containing sulfur atoms with a valence of greater than -2 and less than 0 produced on the negative electrode coating due to the reduction reaction of vinyl sulfite (ES), a non-aqueous secondary battery with high stability can also be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 It is a plan view schematically showing an example of the non-aqueous secondary battery according to the present embodiment.

[0055] Figure 2 is along Figure 1 Cross-sectional view along line AA. DETAILED DESCRIPTION

[0056] Hereinafter, a mode for carrying out the present invention (hereinafter, simply referred to as “embodiment”) will be described in detail. In addition, in this specification, a numerical range described using “to” includes the numerical values ​​described before and after the range.

[0057] The nonaqueous secondary battery of the first, second and third embodiments of the present invention is a secondary battery having a positive electrode, a negative electrode and a nonaqueous electrolyte, and may be, for example, a lithium ion battery. More specifically, it may be Figure 1 A top view is schematically shown in FIG. Figure 2 A lithium-ion battery is schematically shown in cross-section. Figure 1 , 2 The lithium ion battery 100 shown in the figure comprises: a separator 170; a positive electrode 150 and a negative electrode 160, the positive electrode 150 and the negative electrode 160 sandwiching the separator 170 from both sides; a positive electrode lead 130 (connected to the positive electrode 150) and a negative electrode lead 140 (connected to the negative electrode 160), the positive electrode lead 130 and the negative electrode lead 140 further sandwiching a stack of the separator 170, the positive electrode 150 and the negative electrode 160; and a battery exterior 110 accommodating the stack. The stack of the positive electrode 150, the separator 170 and the negative electrode 160 is impregnated with the non-aqueous electrolyte of the first, second and third embodiments.

[0058] <I. First embodiment>

[0059] The first embodiment of the present invention is described in detail below. In the first embodiment, a non-aqueous electrolyte for a non-aqueous lithium ion secondary battery and a non-aqueous lithium ion secondary battery having the non-aqueous electrolyte are provided. The non-aqueous lithium ion secondary battery of the first embodiment is not limited and may have Figure 1 , 2 The structure of the lithium-ion battery 100 is shown.

[0060] <I-1. Non-aqueous electrolyte>

[0061] The "non-aqueous electrolyte" in the first embodiment refers to a non-aqueous electrolyte in which water is less than 1% by mass relative to the total amount of the non-aqueous electrolyte and contains a non-aqueous solvent and a lithium salt. The non-aqueous electrolyte of the first embodiment preferably contains no water as much as possible, and may contain a very small amount of water as long as it does not hinder the solution of the problem of the present invention. As an amount relative to the total amount of the non-aqueous electrolyte, such a moisture content is less than 300 mass ppm, preferably less than 200 mass ppm. For the non-aqueous electrolyte, as long as it has a structure for achieving the solution of the problem of the present invention, as for other constituent elements, the constituent materials in the known non-aqueous electrolyte for lithium ion batteries can be appropriately selected for application.

[0062] <I-1-1. Non-aqueous solvent>

[0063] In the first embodiment, the "non-aqueous solvent" refers to the elements other than lithium salts and various additives removed from the non-aqueous electrolyte. In the first embodiment, when the non-aqueous electrolyte contains an electrode protection additive, the "non-aqueous solvent" refers to the elements other than lithium salts and additives other than the electrode protection additive removed from the non-aqueous electrolyte. As the non-aqueous solvent, for example, alcohols such as methanol and ethanol; aprotic solvents, etc. can be cited. Among them, as the non-aqueous solvent, aprotic solvents are preferred. The non-aqueous solvent may also include solvents other than non-protonic solvents as long as it does not hinder the solution of the subject of the present invention.

[0064] The non-aqueous solvent of the non-aqueous electrolyte of the first embodiment contains acetonitrile as a non-protonic solvent. By containing acetonitrile in the non-aqueous solvent, since the ion conductivity of the non-aqueous electrolyte is improved, the diffusivity of the lithium ions in the battery can be improved. Therefore, when the non-aqueous electrolyte contains acetonitrile, especially in the positive electrode in which the filling amount of the positive electrode active material is increased by thickening the positive electrode active material layer, the lithium ions can also be well diffused to the area near the collector that is difficult for the lithium ions to reach during high-load discharge. Thus, sufficient capacity can also be derived during high-load discharge, and a non-aqueous secondary battery with excellent load characteristics can be obtained.

[0065] In addition, by containing acetonitrile in the non-aqueous solvent, the rapid charging characteristics of the non-aqueous secondary battery can be improved. In the constant current (CC)-constant voltage (CV) charging of the non-aqueous secondary battery, the capacity per unit time during the CC charging period is greater than the charging capacity per unit time during the CV charging period. When acetonitrile is used in the non-aqueous solvent of the non-aqueous electrolyte, in addition to increasing the area where CC charging can be performed (extending the time of CC charging), the charging current can also be increased, and therefore, the time from the start of charging of the non-aqueous secondary battery to the fully charged state can be significantly shortened.

[0066] It should be noted that acetonitrile is easily decomposed by electrochemical reduction. Therefore, when using acetonitrile, preferably, as a non-aqueous solvent, other solvents (for example, aprotic solvents except acetonitrile) are used together with acetonitrile, and / or an electrode protection additive for forming a protective coating to an electrode is added.

[0067] Relative to the total amount of non-aqueous solvent, the content of acetonitrile in the non-aqueous solvent is preferably 5 to 70 volume %. Relative to the total amount of non-aqueous solvent, the lower limit of the content of acetonitrile is more preferably 8 volume % or more, and more preferably 16 volume % or more. Relative to the total amount of non-aqueous solvent, the upper limit of the content of acetonitrile is more preferably 60 volume % or less, and more preferably 35 volume % or less. When the content of acetonitrile is more than 5 volume % relative to the total amount of non-aqueous solvent, the ion conductivity of the non-aqueous electrolyte increases, and it has a tendency to show the high output characteristics of non-aqueous secondary batteries, and further, it is possible to promote the dissolution of lithium salts. In addition, when the content of acetonitrile in the non-aqueous solvent is within the above range, it has the tendency to maintain the excellent performance of acetonitrile and to make the high temperature cycle characteristics of non-aqueous secondary batteries and other battery characteristics better.

[0068] As the aprotic solvent other than acetonitrile, for example, cyclic carbonates, fluoroethylene carbonates, lactones, organic compounds having sulfur atoms, chain fluorinated carbonates, cyclic ethers, mononitriles other than acetonitrile, alkoxy-substituted nitriles, dinitriles, cyclic nitriles, short-chain fatty acid esters, chain ethers, fluorinated ethers, ketones, compounds in which a part or all of the H atoms of the aprotic solvent are substituted with halogen atoms, etc. can be cited.

[0069] Since acetonitrile, a component of the non-aqueous solvent, is easily decomposed by electrochemical reduction, the non-aqueous electrolyte of the first embodiment adds vinylene carbonate to the non-aqueous solvent in addition to acetonitrile, so that the charge and discharge capacity of the battery is stabilized when used in a non-aqueous secondary battery.

[0070] When the nonaqueous solvent of the first embodiment contains acetonitrile, vinylene carbonate (VC) as a cyclic carbonate, and vinyl sulfite as an organic compound having a sulfur atom, the nonaqueous electrolyte solution can operate the battery at a high current density when used in a nonaqueous secondary battery.

[0071] Due to the high resistance of the negative electrode protection coating from vinyl carbonate, therefore, there is a tendency that the performance under fast charging, low temperature environment is degraded and gas is produced during decomposition to cause battery expansion. Compared with other oxygen-containing / sulfur compounds, the lowest unoccupied molecular orbital (LUMO) energy level of vinyl sulfite is low, and it can be reduced and decomposed to form a negative electrode protection coating with a potential lower than vinyl carbonate, and the addition amount of vinyl carbonate can be reduced to solve the problem brought by the negative electrode protection coating from vinyl carbonate. In addition, the negative electrode protection coating from vinyl sulfite has a small resistance in a wide range of temperature regions, further, promotes the formation of a negative electrode SEI (Solid Electrolyte Interface, solid electrolyte interface film) with high durability for acetonitrile and its decomposition products, thereby providing a non-aqueous electrolyte and a non-aqueous secondary battery that can stably work with a high current density.

[0072] From the viewpoint of suppressing the increase of internal resistance, it is preferred that the total content of vinylene carbonate and vinyl sulfite in the non-aqueous electrolyte in the first embodiment is 0.1 volume % or more and less than 15 volume % relative to the total amount of the non-aqueous solvent. In addition, the content of vinyl sulfite is preferably 0.1 volume % or more and less than 6 volume %, and more preferably 1 volume % or more and less than 5 volume % relative to the total amount of the non-aqueous solvent.

[0073] Examples of the cyclic carbonate include ethylene carbonate, propylene carbonate, 1,2-butenyl carbonate, trans-2,3-butenyl carbonate, cis-2,3-butenyl carbonate, 1,2-pentenyl carbonate, trans-2,3-pentenyl carbonate, cis-2,3-pentenyl carbonate, vinylene carbonate (VC), 4,5-dimethylvinylene carbonate, and vinyl ethylene carbonate.

[0074] Examples of the fluoroethylene carbonate include 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one.

[0075] Examples of the lactone include γ-butyrolactone, α-methyl-γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone.

[0076] Examples of the organic compound having a sulfur atom include ethylene sulfite, propylene sulfite, butylene sulfite, pentenyl sulfite, sulfolane, 3-butylene sulfite, 3-methylsulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propylene-1,3-sultone, dimethyl sulfoxide, tetramethylene sulfoxide, and ethylene glycol sulfite.

[0077] Examples of the chain carbonate include ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, ethyl propyl carbonate, and diisobutyl carbonate.

[0078] Examples of the cyclic ether include tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and 1,3-dioxane.

[0079] Examples of the mononitriles other than acetonitrile include propionitrile, butyronitrile, valeronitrile, benzonitrile, and acrylonitrile.

[0080] Examples of the alkoxy-substituted nitrile include methoxyacetonitrile and 3-methoxypropionitrile.

[0081] Examples of the dinitriles include malononitrile, succinonitrile, glutaronitrile, adiponitrile, 1,4-dicyanoheptane, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 2,6-dicyanoheptane, 1,8-dicyanooctane, 2,7-dicyanooctane, 1,9-dicyanononane, 2,8-dicyanononane, 1,10-dicyanodecane, 1,6-dicyanodecane, and 2,4-dimethylglutaronitrile.

[0082] Examples of the cyclic nitrile include benzonitrile.

[0083] Examples of the short-chain fatty acid esters include methyl acetate, methyl propionate, methyl isobutyrate, methyl butyrate, methyl isovalerate, methyl valerate, methyl pivalate, methyl 2-methylbutyrate, methyl hexanoate, ethyl acetate, ethyl propionate, ethyl isobutyrate, ethyl butyrate, ethyl isovalerate, ethyl valerate, ethyl pivalate, ethyl 2-methylbutyrate, ethyl hexanoate, propyl acetate, propyl propionate, propyl isobutyrate, propyl butyrate, propyl isovalerate, propyl valerate, propyl pivalate, propyl 2-methylbutyrate, propyl hexanoate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, propyl valerate, propyl pivalate, propyl 2-methylbutyrate, propyl hexanoate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, isopropyl valerate, isopropyl pivalate, isopropyl 2-methylbutyrate, isopropyl hexanoate, butyl acetate, butyl propionate, butyl isobutyrate, butyl butyrate, butyl isovalerate, butyl valerate, butyl pivalate, butyl 2-methylbutyrate, butyl hexanoate, isobutyl acetate, isobutyl propionate, isobutyl isobutyrate, isobutyl butyrate, isobutyl isovalerate, isobutyl valerate, isobutyl pivalate, isobutyl 2-methylbutyrate, isobutyl hexanoate, tert-butyl acetate, tert-butyl propionate, tert-butyl isobutyrate, tert-butyl butyrate, tert-butyl isovalerate, tert-butyl valerate, tert-butyl pivalate, tert-butyl 2-methylbutyrate, and tert-butyl hexanoate.

[0084] Examples of the chain ether include dimethoxyethane, diethyl ether, 1,3-dioxolane, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), and tetraethylene glycol dimethyl ether (tetraglyme).

[0085] Examples of the fluorinated ether include Rf 20 -OR 21 (Where Rf 20 represents an alkyl group containing a fluorine atom, and R 7 represents a monovalent organic group which may contain a fluorine atom).

[0086] Examples of the ketone include acetone, methyl ethyl ketone, and methyl isobutyl ketone.

[0087] Examples of the compound in which a part or all of the H atoms of the aprotic solvent are substituted with halogen atoms include compounds in which the halogen atom is fluorine.

[0088] Here, as the fluoride of linear carbonate, for example, can enumerate methyl trifluoroethyl carbonate, dimethyl trifluorocarbonate, diethyl trifluorocarbonate, methyl ethyl trifluorocarbonate, methyl 2,2-difluoroethyl carbonate, methyl 2,2,2-trifluoroethyl carbonate, methyl 2,2,3,3-tetrafluoropropyl carbonate.Above-mentioned fluorinated linear carbonate can be represented by following general formula.

[0089] R 1 -OC(O)OR 2

[0090] {In the formula, R 1 and R 2 It is composed of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2 and CH2Rf 3 At least one selected from the group consisting of 3 is an alkyl group having 1 to 3 carbon atoms in which at least one fluorine atom replaces a hydrogen atom, and R 1 and / or R 2 contains at least one fluorine atom}.

[0091] Examples of the fluorinated short-chain fatty acid ester include fluorinated short-chain fatty acid esters represented by 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, and 2,2,3,3-tetrafluoropropyl acetate. The fluorinated short-chain fatty acid ester can be represented by the following general formula.

[0092] R 10 -C(O)OR 11

[0093] {In the formula, R 10 It is made of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, CF3CF2H, CFH2, CF2Rf 12 CFHRf 12 and CH2Rf 13 At least one selected from the group consisting of 11 It is composed of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2 and CH2Rf 13 At least one selected from the group consisting of 12 is an alkyl group having 1 to 3 carbon atoms which may be formed by replacing a hydrogen atom with at least one fluorine atom, Rf 13 is an alkyl group having 1 to 3 carbon atoms in which at least one fluorine atom replaces a hydrogen atom, and R 10 and / or R 11 Contains at least one fluorine atom, when R 10 When it is CF2H, R 11 Not CH3}.

[0094] The aprotic solvent other than acetonitrile in the first embodiment may be used alone or in combination of two or more.

[0095] From the viewpoint that improves the stability of nonaqueous electrolyte, preferably, the nonaqueous solvent in the first embodiment is to use more than one in cyclic carbonate and the linear carbonate and acetonitrile.From this viewpoint, the nonaqueous solvent in the first embodiment more preferably uses cyclic carbonate and acetonitrile, further preferably uses cyclic carbonate and linear carbonate together with acetonitrile.

[0096] When a cyclic carbonate other than vinylene carbonate (VC) is used together with acetonitrile, it is particularly preferred that the cyclic carbonate contains ethylene carbonate and / or fluoroethylene carbonate.

[0097] <I-1-2. Electrolyte salt>

[0098] The non-aqueous electrolyte of the first embodiment is used for a lithium ion secondary battery, and other electrolyte salts are not particularly limited as long as they contain a lithium salt as an electrolyte salt. For example, in the first embodiment, as lithium salts, LiPF6 and lithium-containing imide salts may be contained.

[0099] Lithium imide salt is LiN(SO2C m F 2m+1 )2〔wherein m is an integer of 0 to 8〕, specifically, preferably including at least one of LiN(SO2F)2 and LiN(SO2CF3)2. It may include only one of these imide salts, or two of them. Alternatively, it may include imide salts other than these imide salts.

[0100] When acetonitrile is contained in the non-aqueous solvent, since the saturation concentration of the lithium imide salt relative to acetonitrile is higher than the saturation concentration of LiPF6, it is preferred to contain the lithium imide salt in a molar concentration of LiPF6≤lithium imide salt, which can inhibit the association and precipitation of lithium salt and acetonitrile under low temperature conditions. In addition, from the perspective of ion supply, it is preferred that the content of lithium imide salt is 0.5 mol or more and 3 mol or less relative to 1L of non-aqueous solvent. According to the non-aqueous electrolyte containing acetonitrile containing at least one of LiN(SO2F)2 and LiN(SO2CF3)2, the decrease in ion conductivity in a low temperature region such as -10°C or -30°C can be effectively suppressed, and excellent low temperature characteristics can be obtained. As described above, by limiting the content, the increase in resistance during high temperature heating can also be more effectively suppressed.

[0101] In addition, as a lithium salt, a fluorine-containing inorganic lithium salt other than LiPF6 may be included, for example, LiBF4, LiAsF6, Li2SiF6, LiSbF6, Li2B 12 F b H 12-b[wherein b is an integer of 0 to 3] and the like. In the first embodiment, the "inorganic lithium salt" refers to a lithium salt that does not contain carbon atoms in the anion and is soluble in acetonitrile. In addition, in the first embodiment, the "fluorine-containing inorganic lithium salt" refers to a lithium salt that does not contain carbon atoms in the anion, contains fluorine atoms in the anion and is soluble in acetonitrile. The fluorine-containing inorganic lithium salt forms a passivation film on the surface of the metal foil serving as the positive electrode collector, and is excellent in inhibiting the corrosion of the positive electrode collector. These fluorine-containing inorganic lithium salts are used alone or in combination of two or more. As the fluorine-containing inorganic lithium salt, a compound that is a complex salt of LiF and a Lewis acid is preferred, among which, if a fluorine-containing inorganic lithium salt having a phosphorus atom is used, free fluorine atoms are easily released, and therefore it is more preferred. A representative fluorine-containing inorganic lithium salt is LiPF6 that dissolves and releases PF6 anions. When a fluorine-containing inorganic lithium salt having a boron atom is used as the fluorine-containing inorganic lithium salt, it is preferred because it is easy to capture excess free acid components that may cause battery degradation. From this viewpoint, LiBF 4 is particularly preferred.

[0102] The content of the fluorine-containing inorganic lithium salt in the non-aqueous electrolyte of the first embodiment is not particularly limited, and is preferably 0.01 mol or more, more preferably 0.02 mol or more, and further preferably 0.03 mol or more relative to 1L of the non-aqueous solvent. When the content of the fluorine-containing inorganic lithium salt is within the above-mentioned range of 0.01 mol or more, the ion conductivity increases, and it has a tendency to exhibit high output characteristics. In addition, relative to 1L of the non-aqueous solvent, the content of the fluorine-containing inorganic lithium salt is preferably less than 1.5 mol, more preferably less than 0.5 mol, and further preferably less than 0.1 mol. When the content of the fluorine-containing inorganic lithium salt is within the above-mentioned range of 1.5 mol or less, the ion conductivity increases, and it has a tendency to exhibit high output characteristics and to suppress the decrease in ion conductivity associated with the increase in viscosity under low temperature conditions, and it has a tendency to maintain the excellent performance of the non-aqueous electrolyte and to make the high temperature cycle characteristics and other battery characteristics of the non-aqueous secondary battery better.

[0103] The non-aqueous electrolyte solution of the first embodiment may further contain an organic lithium salt. In the first embodiment, the "organic lithium salt" refers to a lithium salt having a carbon atom in its anion and being soluble in acetonitrile.

[0104] As an organic lithium salt, an organic lithium salt having an oxalic acid group can be cited. As a specific example of an organic lithium salt having an oxalic acid group, for example, organic lithium salts represented by LiB(C2O4)2, LiBF2(C2O4), LiPF4(C2O4) and LiPF2(C2O4)2 can be cited, among which at least one lithium salt selected from the lithium salts represented by LiB(C2O4)2 and LiBF2(C2O4) is preferred. In addition, it is more preferred to use one or more of them together with a fluorine-containing inorganic lithium salt. In addition to being added to a non-aqueous electrolyte, the organic lithium salt having an oxalic acid group can also be included in the negative electrode (negative electrode active material layer).

[0105] From the viewpoint of better ensuring the effect of its use, the amount of the organic lithium salt with oxalate group added in the non-aqueous electrolyte is preferably 0.005 moles or more, more preferably 0.02 moles or more, and further preferably 0.05 moles or more, relative to the amount of 1L of the non-aqueous solvent of the non-aqueous electrolyte. However, when the amount of the above-mentioned organic lithium salt with oxalate group in the non-aqueous electrolyte is too much, it is possible to precipitate. Therefore, based on the amount of 1L of the non-aqueous solvent of the non-aqueous electrolyte, the amount of the above-mentioned organic lithium salt with oxalate group added in the non-aqueous electrolyte is preferably less than 1.0 moles, more preferably less than 0.5 moles, and further preferably less than 0.2 moles.

[0106] It is known that organic lithium salts having oxalic acid groups are poorly soluble in organic solvents with low polarity, especially in linear carbonates. Organic lithium salts having oxalic acid groups sometimes contain trace amounts of lithium oxalate, and further, when mixed as a non-aqueous electrolyte, sometimes react with trace amounts of water contained in other raw materials to produce new white precipitates of lithium oxalate. Therefore, the content of lithium oxalate in the non-aqueous electrolyte of the first embodiment is not particularly limited, and is preferably 0 to 500 ppm.

[0107] As the lithium salt in the first embodiment, in addition to the substances listed above, lithium salts commonly used in non-aqueous secondary batteries may be added as an auxiliary. Specific examples of other lithium salts include LiClO4, LiAlO4, LiAlCl4, LiB 10 Cl 10 , inorganic lithium salts containing no fluorine atoms in anions such as lithium borochloride; LiCF3SO3, LiCF3CO2, Li2C2F4(SO3)2, LiC(CF3SO2)3, LiC n F (2n+1) SO3{where n≥2}, organic lithium salts such as lower aliphatic carboxylic acid Li, tetraphenylborate Li, LiB(C3O4H2)2, etc.; LiPF5(CF3) etc. n (C p F 2p+1 )6-n [wherein n is an integer of 1 to 5, and p is an integer of 1 to 8] an organic lithium salt represented by LiBF3(CF3) or the like q (C s F 2s+1 ) 4-q [wherein q is an integer of 1 to 3 and s is an integer of 1 to 8] an organic lithium salt represented by; a lithium salt bonded to a polyvalent anion; an organic lithium salt represented by the following formula (sa), the following formula (sb) and the following formula (sc), etc.

[0108] LiC(SO2R A )(SO2R B )(SO2R C )(sa)

[0109] {In the formula, R A , R B and R C They may be the same as or different from each other and represent a perfluoroalkyl group having 1 to 8 carbon atoms.

[0110] LiN(SO2OR D )(SO2OR E )(sb)

[0111] {In the formula, R D and R E They may be the same as or different from each other and represent a perfluoroalkyl group having 1 to 8 carbon atoms.

[0112] LiN(SO2R F )(SO2OR G )(sc)

[0113] {In the formula, R F and R G They may be the same as or different from each other and represent a perfluoroalkyl group having 1 to 8 carbon atoms.

[0114] One or two or more of these can be used together with the fluorine-containing inorganic lithium salt.

[0115] <I-1-3. Additives>

[0116] The nonaqueous electrolyte solution of the first embodiment may contain additives in addition to the nonaqueous solvent and electrolyte salt described above.

[0117] <Vinylene carbonate>

[0118] The non-aqueous electrolyte in the first embodiment contains vinylene carbonate (VC). Vinylene carbonate (VC) undergoes a reduction reaction on the surface of the negative electrode active material to form a coating, so an amount of addition commensurate with the mass of the negative electrode is required. Relative to the mass of the negative electrode other than the negative electrode collector, when containing a non-aqueous electrolyte containing A volume % acetonitrile of X mass %, the content of vinylene carbonate (VC) in the non-aqueous electrolyte is 7×A / X mass % or more. Within this range, the formation of the coating is well performed in the initial charge after containing the non-aqueous electrolyte, and there is a tendency to improve the capacity efficiency under room temperature conditions. In addition, the VC content is preferably 10×A / X mass % or more, more preferably 15×A / X mass % or more. Within this range, under a longer-term and high-temperature environment, the capacity efficiency is also improved, and in the non-aqueous electrolyte containing acetonitrile, the charge capacity and discharge capacity are also stable. On the other hand, the addition of excessive vinylene carbonate (VC) may lead to a decrease in the viscosity of the non-aqueous electrolyte, a decrease in low-temperature characteristics, and the generation of excessive gas. Therefore, relative to the mass of the non-aqueous electrolyte, the addition of vinylene carbonate (VC) is preferably less than 10% by mass, more preferably less than 9% by mass, further preferably less than 8% by mass, and particularly preferably less than 7% by mass. From the viewpoint of suppressing the reduction reaction on the surface of the negative electrode active material, the formation of the negative electrode SEI, the decrease in the viscosity and low-temperature characteristics of the non-aqueous electrolyte, and suppressing the generation of excessive gas, X is preferably more than 50 and less than 2000, and / or, A is preferably more than 5 and less than 70.

[0119] In addition, by reducing the content of the non-aqueous electrolyte in the non-aqueous lithium ion secondary battery, the battery capacity per unit volume / unit weight of the battery can be optimized. From this viewpoint, relative to the mass of the negative electrode excluding the negative electrode collector, the non-aqueous lithium ion secondary battery containing the non-aqueous electrolyte of the first embodiment of X mass% is preferably less than 200, and more preferably less than 98. However, when the content of the non-aqueous electrolyte relative to the mass of the negative electrode excluding the negative electrode collector is less than the specified value, the impregnation into the electrode or separator may be insufficient. From this viewpoint, as X in the non-aqueous lithium ion secondary battery containing the non-aqueous electrolyte of the first embodiment, it is more preferably 55 or more, more preferably 60 or more, and particularly preferably 65 or more. When the content of acetonitrile relative to the volume of the non-aqueous solvent is expressed as A volume %, acetonitrile is contained in the non-aqueous electrolyte as A, thereby expecting to improve the output performance. From this viewpoint, A is more preferably 8 or more, and more preferably 16 or more. In addition, when the content of acetonitrile is below a predetermined value, the impregnation into the electrode and the separator is further improved, and the thermal stability tends to be improved. From this viewpoint, A is more preferably 60 or less, and further preferably 35 or less.

[0120] <Sulfate / sulfite ions>

[0121] The non-aqueous electrolyte in the first embodiment preferably contains one or both of sulfate ions and sulfite ions. It can be considered that by combining sulfate ions with metal impurities, metal impurities can be prevented from accumulating on the negative electrode and damaging SEI. The lower limit of the amount of sulfate ions added is not particularly limited, preferably above the concentration of metal impurities in the electrolyte material, and if the metal is also dissolved from the electrode, relative to the mass of the non-aqueous electrolyte, preferably 1 ppm or more, more preferably 10 ppm or more. In addition, excessive addition leads to a large amount of precipitation of sulfates and sulfites, which may damage SEI, and because sulfate ions can be reduced, they sometimes react with vinyl carbonate (VC) and the like on the negative electrode and become an obstacle to the formation of the coating, therefore, relative to the mass of the non-aqueous electrolyte, the content of sulfate ions is 7×A / X mass% or less or less than 7×A / X mass%, and relative to the mass of vinyl carbonate (VC), preferably 10 mass% or less, more preferably 8 mass% or less, particularly preferably 5 mass% or less. In addition, the non-aqueous electrolyte in the first embodiment may also contain sulfite ions, and it is also possible to expect that it combines with the metal leaching component to prevent damage to SEI. Relative to the mass of vinylene carbonate (VC) in the non-aqueous electrolyte, the addition amount of sulfite ions is preferably less than 10 mass %, more preferably less than 8 mass %, and particularly preferably less than 5 mass %.

[0122] From the same viewpoint as above, the total content of sulfate ions and sulfite ions in the non-aqueous electrolyte is greater than 1 ppm and less than 7×A / X mass % relative to the mass of the non-aqueous electrolyte, and is preferably less than 10 mass % of the content of VC in the non-aqueous electrolyte.

[0123] The method of adding each ion to the non-aqueous electrolyte is not particularly limited, as long as it is included in the non-aqueous electrolyte by decomposition of the organic compound in the non-aqueous electrolyte, addition of sulfate or sulfite, etc. When added by an inorganic salt, for example, by adding lithium sulfate or lithium sulfite, it will not bring metal impurities to the composition of the non-aqueous electrolyte for lithium ion secondary batteries, so it is preferred.

[0124] <Other electrode protection additives>

[0125] As other electrode protection additives, there is no particular limitation as long as they do not hinder the solution of the subject of the present invention, and they can be substantially repeated with the substance that acts as a solvent for dissolving lithium salts (i.e., the above-mentioned non-aqueous solvent) (wherein, acetonitrile, vinylene carbonate, and vinyl sulfite as an organic compound having a sulfur atom described above are excluded). The electrode protection additive is preferably a substance that helps to improve the performance of the non-aqueous electrolyte and the non-aqueous secondary battery in the first embodiment, but also includes substances that do not directly participate in the electrochemical reaction.

[0126] Specific examples of other electrode protection additives include, for example, fluoroethylene carbonate represented by 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one; cyclic carbonates containing unsaturated bonds represented by 4,5-dimethyl vinylene carbonate and vinyl carbonate; γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone ...4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one, 4,4 The present invention also includes lactones represented by -caprolactone and ε-caprolactone; cyclic ethers represented by 1,4-dioxane; cyclic sulfur compounds represented by propylene sulfite, butylene sulfite, pentenyl sulfite, sulfolane, 3-butylene sulfone, 3-methylsulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propylene-1,3-sultone, and tetramethylene sulfoxide; chain acid anhydrides represented by acetic anhydride, propionic anhydride, and benzoic anhydride; cyclic acid anhydrides represented by malonic anhydride, succinic anhydride, glutaric anhydride, maleic anhydride, phthalic anhydride, 1,2-cyclohexane dicarboxylic anhydride, 2,3-naphthalene dicarboxylic anhydride, or naphthalene-1,4,5,8-tetracarboxylic dianhydride; mixed acid anhydrides having a structure formed by dehydration condensation of two different carboxylic acids or different types of acids such as carboxylic acid and sulfonic acid. These can be used alone or in combination of two or more.

[0127] There is no particular limitation on the content of the electrode protection additive in the non-aqueous electrolyte in the first embodiment. The content of the electrode protection additive relative to the total amount of the non-aqueous solvent is preferably 0.1 volume % to 30 volume %, more preferably 0.3 volume % to 15 volume %, and further preferably 0.5 volume % to 4 volume %.

[0128] In the first embodiment, the more the content of the electrode protection additive is, the more the degradation of the non-aqueous electrolyte is suppressed. However, the less the content of the electrode protection additive is, the more the high output characteristics of the non-aqueous secondary battery in a low temperature environment are improved. Therefore, by adjusting the content of the electrode protection additive within the above range, there is a tendency to maximize the excellent performance based on the high ion conductivity of the non-aqueous electrolyte without damaging the basic function of the non-aqueous secondary battery. By preparing the non-aqueous electrolyte with such a composition, there is a tendency to make the cycle performance of the non-aqueous secondary battery, the high output performance in a low temperature environment and other battery characteristics all better.

[0129] <Other optional additives>

[0130] In the first embodiment, for the purpose of improving the charge and discharge cycle characteristics of the non-aqueous secondary battery, improving the high-temperature storage property, safety (for example, preventing overcharging, etc.), etc., the non-aqueous electrolyte can also appropriately contain any additive selected from, for example, sulfonates, diphenyl disulfide, cyclohexylbenzene, biphenyl, fluorobenzene, tert-butylbenzene, phosphates [ethyl diethylphosphonoacetate (EDPA): (C2H5O)2(P=O)-CH2(C=O)OC2H5; tris(trifluoroethyl) phosphate (TFEP): (CF3CH2O)3P=O; triphenyl phosphate (TPP): (C6H5O)3P=O; triallyl phosphate: (CH2=CHCH2O)3P=O, etc.], nitrogen-containing cyclic compounds having no steric hindrance around non-covalent electron pairs [pyridine, 1-methyl-1H-benzotriazole, 1-methylpyrazole, etc.], and derivatives of these compounds. In particular, phosphoric acid esters are effective in suppressing side reactions during storage.

[0131] The content of other arbitrary additives in the first embodiment is calculated by the mass percentage relative to the total mass of all components constituting the non-aqueous electrolyte. The content of other arbitrary additives is not particularly limited, and relative to the total amount of the non-aqueous electrolyte, it is preferably in the range of 0.01 mass % or more and 10 mass % or less, more preferably 0.02 mass % or more and 5 mass % or less, and further preferably 0.05 mass % or more and 3 mass % or less. By adjusting the content of other arbitrary additives to the above range, there is a tendency to be able to add better battery characteristics without damaging the basic function as a non-aqueous secondary battery.

[0132] <I-2. Positive Electrode and Positive Electrode Collector>

[0133] Figure 1 , 2The positive electrode 150 shown is composed of a positive electrode active material layer and a positive electrode current collector, and the positive electrode active material layer is made of a positive electrode mixture. The positive electrode 150 is not particularly limited as long as it functions as a positive electrode of a non-aqueous secondary battery, and may also be a known positive electrode. Preferably, the positive electrode in the first embodiment contains a lithium-containing compound containing Fe, and more preferably also contains nickel (Ni) at a relatively high ratio.

[0134] Preferably, the positive electrode active material layer is disposed on one side or both sides of the positive electrode current collector, and contains the positive electrode active material and, if necessary, further contains a conductive auxiliary agent and a binder.

[0135] The positive electrode active material layer preferably contains a material capable of absorbing and releasing lithium ions as the positive electrode active material. When such a material is used, high voltage and high energy density tend to be obtained, which is preferred.

[0136] The positive electrode active material contained in the positive electrode active material layer is preferably a metal phosphate compound containing lithium and a transition metal element represented by the following general formula (1) and / or at least one Li-containing metal oxide selected from lithium (Li)-containing metal oxides represented by the following general formula (2) containing at least one transition metal element selected from the group consisting of Ni, Mn and Co.

[0137] Li w MPO4(1)

[0138] {wherein, M represents one or more transition metal elements, and the value of w is determined by the charge and discharge state of the battery and represents a number of 0 to 1.2, preferably a number of 0.05 to 1.10}.

[0139] Li p Ni q Co r Mn s M t O u (2)

[0140] {wherein, M is at least one metal selected from the group consisting of aluminum (Al), tin (Sn), indium (In), iron (Fe), vanadium (V), copper (Cu), magnesium (Mg), titanium (Ti), zinc (Zn), molybdenum (Mo), zirconium (Zr), strontium (Sr) and barium (Ba), and is in the range of 0<p<1.3, 0<q<1.2, 0<r<1.2, 0≤s<0.5, 0≤t<0.3, 0.7≤q+r+s+t≤1.2, 1.8<u<2.2, and p is a value determined by the charge and discharge state of the battery}.

[0141] Specific examples of the positive electrode active material include Li wLi compounds such as FePO4 or lithium cobalt oxides represented by LiCoO2; lithium manganese oxides represented by LiMnO2, LiMn2O4 and Li2Mn2O4; lithium nickel oxides represented by LiNiO2; 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.2 O2 represented by Li z Lithium-containing composite metal oxides represented by MO2 (wherein M includes at least one transition metal element selected from the group consisting of Ni, Mn and Co, and represents two or more metal elements selected from the group consisting of Ni, Mn, Co, Al and Mg, and z represents a number greater than 0.9 and less than 1.2).

[0142] In particular, when the Ni content ratio q of the Li-containing metal oxide represented by the general formula (2) is 0.5<q<1.2, it is preferred because both the amount of Co used as a rare metal and the high energy density can be achieved. As such a positive electrode active material, for example, LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.75 Co 0.15 Mn 0.15 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.85 Co 0.075 Mn 0.075 O2、LiNi 0.8 Co 0.15 Al 0.05 O2、LiNi 0.81 Co 0.1 Al 0.09 O2、LiNi 0.85 Co 0.1 Al 0.05 Lithium-containing composite metal oxides represented by O2, etc.

[0143] On the other hand, the higher the Ni content ratio in the positive electrode active material layer, the more it has a tendency to degrade at a low voltage. In the positive electrode active material containing Li metal oxide represented by the general formula (2), there are actually active sites that cause oxidation degradation of the non-aqueous electrolyte, but the active sites sometimes unintentionally consume the compounds added to protect the negative electrode on the positive electrode side. Among them, acid anhydrides have a tendency to be easily affected by them. In particular, in the case of containing acetonitrile as a non-aqueous solvent, the addition effect of acid anhydrides is huge, and therefore, the consumption of acid anhydrides on the positive electrode side is a fatal issue.

[0144] In addition, these additive decomposition products that enter the positive electrode side and accumulate will not only become the main cause of the increase in the internal resistance of the non-aqueous secondary battery, but also accelerate the degradation of the lithium salt. Furthermore, the protection of the negative electrode surface, which is the original purpose, becomes insufficient. In order to deactivate the active sites that substantially oxidize and degrade the non-aqueous electrolyte, it is important to coexist with components that act as a control or neutralizer for the Jahn-Teller distortion. Therefore, it is preferred that the positive electrode active material contains at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba.

[0145] For the same reason, it is preferred that the surface of the positive electrode active material is coated with a compound containing at least one metal element selected from the group consisting of Zr, Ti, Al and Nb. In addition, it is more preferred that the surface of the positive electrode active material is coated with an oxide containing at least one metal element selected from the group consisting of Zr, Ti, Al and Nb. Furthermore, since it will not hinder the permeation of lithium ions, it is particularly preferred that the surface of the positive electrode active material is coated with at least one oxide selected from the group consisting of ZrO2, TiO2, Al2O3, NbO3 and LiNbO2.

[0146] The positive electrode active material may be a lithium-containing compound other than the Li-containing metal oxide represented by formula (1) and (2), and is not particularly limited as long as it contains lithium. As such lithium-containing compounds, for example, composite oxides containing lithium and transition metal elements, metal sulfides having lithium, and metal silicate compounds containing lithium and transition metal elements may be cited. From the viewpoint of obtaining a higher voltage, as a lithium-containing compound, in particular, a metal phosphate compound containing lithium and at least one transition metal element selected from the group consisting of Co, Ni, Mn, Fe, Cu, Zn, Cr, V and Ti is preferred.

[0147] More specifically, the lithium-containing compound includes compounds represented by the following formula (Xa) and the following formula (Xb).

[0148] Li vM I D2(Xa)

[0149] {wherein, D represents a chalcogen element, M I Indicates one or more transition metal elements. The v value is determined by the charge and discharge state of the battery and is a number between 0.05 and 1.10.

[0150] Li t M II u SiO4(Xb)

[0151] {In the formula, M II represents one or more transition metal elements, t value is determined by the charge and discharge state of the battery and represents a number from 0.05 to 1.10, and u represents a number from 0 to 2.}

[0152] The lithium-containing compound represented by the above formula (Xa) has a layered structure, and the compounds represented by the above formula (1) and the above formula (Xb) have an olivine structure. For the purpose of stabilizing the structure, these lithium-containing compounds can be compounds in which a part of the transition metal elements are replaced by Al, Mg or other transition metal elements, compounds in which these metal elements are contained in the grain boundaries, compounds in which a part of the oxygen atoms are replaced by fluorine atoms, compounds in which other positive electrode active materials are coated on at least a part of the surface of the positive electrode active material, etc.

[0153] As the positive electrode active material in the first embodiment, only the lithium-containing compound described above may be used, or other positive electrode active materials may be used in combination with the lithium-containing compound.

[0154] As such other positive electrode active materials, for example, metal oxides or metal chalcogenides having a tunnel structure and a layered structure; sulfur; conductive polymers, etc. As metal oxides or metal chalcogenides having a tunnel structure and a layered structure, for example, MnO2, FeO2, FeS2, V2O5, V6O 13 Oxides, sulfides, selenides, etc. of metals other than lithium represented by TiO2, TiS2, MoS2, and NbSe2. As conductive polymers, for example, conductive polymers represented by polyaniline, polythiophene, polyacetylene, and polypyrrole can be cited.

[0155] The above-mentioned other positive electrode active materials can be used alone or in combination of two or more, without particular limitation. However, since lithium ions can be reversibly and stably absorbed and released, and high energy density can be achieved, it is preferred that the positive electrode active material layer contains at least one transition metal element selected from Ni, Mn and Co.

[0156] When a lithium-containing compound and other positive electrode active materials are used together as positive electrode active materials, the ratio of the two, as well as the ratio of the lithium-containing compound to the total positive electrode active materials, is preferably 80% by mass or more, more preferably 85% by mass or more.

[0157] Examples of the conductive aid include carbon black represented by graphite, acetylene black and Ketjen black, and carbon fiber. The conductive aid content is preferably 10 parts by mass or less, more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the positive electrode active material.

[0158] Examples of the binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid, styrene butadiene rubber, and fluororubber. The binder content is preferably 10 parts by mass or less, more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the positive electrode active material.

[0159] The positive electrode mixture formed by mixing the positive active material, the conductive aid as needed and the binder is dispersed in a solvent to form a slurry containing the positive electrode mixture, the slurry containing the positive electrode mixture is applied to the positive electrode collector and dried (removing the solvent), and pressed as needed to form a positive electrode active material layer. As such solvent, it is not particularly limited, and a conventionally known solvent can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be cited.

[0160] The positive electrode current collector is composed of metal foil such as aluminum foil, nickel foil, stainless steel foil, etc. The positive electrode current collector may be carbon-coated on the surface or processed into a mesh shape. The thickness of the positive electrode current collector is preferably 5 μm to 40 μm, more preferably 7 μm to 35 μm, and further preferably 9 μm to 30 μm.

[0161] <I-3. Negative electrode and negative electrode current collector>

[0162] Figure 1 , 2 The negative electrode 160 shown is composed of a negative electrode active material, a conductive auxiliary agent as needed, a binder, and a negative electrode current collector. The negative electrode 160 can function as a negative electrode of a non-aqueous secondary battery.

[0163] Preferably, the negative electrode active material layer is disposed on one or both sides of the negative electrode collector, and the negative electrode active material layer contains a negative electrode active material and, as required, contains a conductive aid and a binder. As described above, the non-aqueous lithium ion secondary battery of the first embodiment is preferably a structure capable of containing a non-aqueous electrolyte of X mass % relative to the mass of the negative electrode excluding the negative electrode collector.

[0164] As the negative electrode active material, for example, in addition to carbon materials represented by amorphous carbon (hard carbon), graphite (for example, artificial graphite, natural graphite, etc.), pyrolytic carbon, coke, glassy carbon, sintered bodies of organic polymer compounds, mesophase carbon microspheres, carbon fibers, activated carbon, carbon colloids, and carbon black, metallic lithium, metal oxides, metal nitrides, lithium alloys, tin alloys, silicon alloys, intermetallic compounds, organic compounds, inorganic compounds, metal complexes, organic polymer compounds, etc. can be cited. The negative electrode active material can be used alone or in combination of two or more. As the negative electrode active material, graphite is preferred from the viewpoint of the use of the non-aqueous electrolyte of the first embodiment.

[0165] From the viewpoint of increasing the battery voltage, it is preferred that the negative electrode active material layer contain a negative electrode active material capable of reacting at a ratio of 0.4 V (vs. Li / Li + ) Materials that absorb lithium ions at a lower potential.

[0166] Examples of the conductive aid include carbon black represented by graphite, acetylene black and Ketjen black, and carbon fiber. The content of the conductive aid is preferably 20 parts by mass or less, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the negative electrode active material.

[0167] Examples of the binder include carboxymethyl cellulose, PVDF, PTFE, polyacrylic acid, and fluororubber. In addition, diene rubbers such as styrene butadiene rubber may also be mentioned. The binder content is preferably 10 parts by mass or less, more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the negative electrode active material.

[0168] The negative electrode active material and the negative electrode mixture formed by mixing the conductive aid and the binder as needed are dispersed in a solvent to form a slurry containing the negative electrode mixture, and the slurry containing the negative electrode mixture is applied to the negative electrode collector and dried (removing the solvent), and pressed as needed to form a negative electrode active material layer. As such a solvent, there is no particular limitation, and a conventionally known solvent can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be cited.

[0169] The negative electrode current collector is composed of metal foil such as copper foil, nickel foil, stainless steel foil, etc. In addition, the negative electrode current collector may be carbon-coated on the surface or processed into a mesh shape. The thickness of the negative electrode current collector is preferably 5 μm to 40 μm, more preferably 6 μm to 35 μm, and further preferably 7 μm to 30 μm.

[0170] <I-4. Spacer>

[0171] like Figure 2As shown, for the non-aqueous secondary battery 100 in the first embodiment, from the viewpoint of providing safety such as preventing a short circuit and shutdown of the positive electrode 150 and the negative electrode 160, it is preferred to have a separator 170 between the positive electrode 150 and the negative electrode 160. As the separator 170, there is no limitation, and the same separator as the separator provided in the known non-aqueous secondary battery can be used, and an insulating film with large ion permeability and excellent mechanical strength is preferred. As the separator 170, for example, woven fabrics, non-woven fabrics, synthetic resin microporous films, etc. can be cited, among which synthetic resin microporous films are preferred.

[0172] As the synthetic resin microporous membrane, for example, a polyolefin-based microporous membrane such as a microporous membrane containing polyethylene or polypropylene as the main component or a microporous membrane containing both of these polyolefins is preferably used. As the nonwoven fabric, for example, a porous membrane made of heat-resistant resins such as glass, ceramic, polyolefin, polyester, polyamide, liquid crystal polyester, and aromatic polyamide can be cited.

[0173] The spacer 170 may be a single layer or multiple layers of a microporous film, or a structure of two or more microporous films stacked together. The spacer 170 may also be a single layer or multiple layers of a mixed resin material obtained by melt-kneading two or more resin materials.

[0174] For the purpose of imparting functions, inorganic particles may be present on the surface or inside of the spacer, and other organic layers may be further coated or laminated. In addition, a cross-linked structure may also be included. In order to improve the safety performance of the non-aqueous secondary battery, these methods may be combined as needed.

[0175] By using such a separator 170 , it is possible to realize good input-output characteristics and low self-discharge characteristics required of lithium-ion batteries for high-output applications.

[0176] The thickness of the microporous film that can be used as a separator is not particularly limited. From the viewpoint of film strength, it is preferably 1 μm or more, and from the viewpoint of permeability, it is preferably 500 μm or less. From the viewpoint of high output uses such as safety tests that have high heat release and require self-discharge characteristics above the past, and from the viewpoint of windability in large battery winding machines, the thickness of the microporous film is preferably 5 μm or more and 30 μm or less, more preferably 10 μm or more and 25 μm or less. It should be noted that in the case of taking into account both short-circuit resistance and output performance, the thickness of the microporous film is further preferably 15 μm or more and 25 μm or less, and in the case of taking into account both high energy density and output performance, the thickness of the microporous film is further preferably 10 μm or more and less than 15 μm.

[0177] From the viewpoint of following the rapid movement of lithium ions during high output, the porosity of the microporous film that can be used as a separator is preferably 30% or more and 90% or less, more preferably 35% or more and 80% or less, and further preferably 40% or more and 70% or less. It should be noted that, in the case of giving priority to improving output performance while ensuring safety, the porosity of the microporous film is particularly preferably 50% or more and 70% or less, and in the case of paying attention to both short-circuit resistance and output performance, it is particularly preferably 40% or more and less than 50%.

[0178] The air permeability of the microporous membrane that can be used as a separator is preferably 1 sec / 100 cm from the viewpoint of the balance between membrane thickness and porosity. 3 Above and 400 seconds / 100cm 3 Less than 100 sec / 100 cm 3 Above and 350 / 100cm 3 It should be noted that, when emphasizing both short-circuit resistance and output performance, the air permeability of the microporous membrane is particularly preferably 150 sec / 100 cm 3 Above and 350 seconds / 100cm 3 Below, when giving priority to improving output performance while ensuring safety, 100 / 100cm is particularly preferred. 3 More than 1 second and less than 150 seconds / 100cm 3 . On the other hand, when a non-aqueous electrolyte with low ion conductivity is combined with a separator within the above range, the speed of movement of lithium ions is not limited by the structure of the separator but by the high ion conductivity of the non-aqueous electrolyte, and there is a tendency that the expected input-output characteristics cannot be obtained. Therefore, the ion conductivity of the non-aqueous electrolyte is preferably 10mS / cm or more, more preferably 15mS / cm, and further preferably 20mS / cm. However, the film thickness, air permeability and porosity of the separator and the ion conductivity of the non-aqueous electrolyte are not limited to the above examples.

[0179] <I-5. Battery exterior>

[0180] Figure 1 , 2 The structure of the battery outer package 110 of the non-aqueous secondary battery 100 shown is not particularly limited, and for example, any one of a battery can and a laminated film outer package can be used. As a battery can, for example, a square, square-shaped, cylindrical, oval, flat, coin-shaped or button-shaped metal can made of steel, stainless steel, aluminum or a cladding material can be used. As a laminated film outer package, for example, a laminated film composed of a three-layer structure of hot melt resin / metal film / resin can be used.

[0181] The laminated film outer casing can overlap two pieces with the hot melt resin side facing inward, or be bent into a state with the hot melt resin side facing inward, so that it can be used as an outer casing in a state where the ends are sealed by heat sealing. When a laminated film outer casing is used, the positive lead 130 (or the positive terminal and the lead tab connected to the positive terminal) can be connected to the positive electrode collector, and the negative lead 140 (or the negative terminal and the lead tab connected to the negative terminal) can be connected to the negative electrode collector. In this case, the laminated film outer casing can be packaged in a state where the ends of the positive lead 130 and the negative lead 140 (or the lead tabs connected to the positive terminal and the negative terminal, respectively) are led out to the outside of the outer casing.

[0182] <I-6. Battery manufacturing method>

[0183] The nonaqueous secondary battery 100 in the first embodiment can be manufactured by a known method using the above-mentioned nonaqueous electrolyte, for example, a positive electrode 150 having a positive electrode active material layer on one or both sides of a current collector, a negative electrode 160 having a negative electrode active material layer on one or both sides of a current collector, a battery casing 110, and a separator 170 as required.

[0184] First, a laminated body consisting of the positive electrode 150 and the negative electrode 160 and the separator 170 as required is formed. For example, the laminated body may be formed by winding the long positive electrode 150 and the negative electrode 160 in a stacked state with the long separator sandwiched between the positive electrode 150 and the negative electrode 160; the laminated body may be formed by cutting the positive electrode 150 and the negative electrode 160 into a plurality of sheets having a predetermined area and shape to obtain positive electrode sheets and negative electrode sheets, and alternately stacking the obtained positive electrode sheets and negative electrode sheets via separator sheets; the laminated body may be formed by bending the long separator and alternately inserting the positive electrode body sheets and the negative electrode body sheets between the bent separators, etc., but the present invention is not limited thereto.

[0185] Then, the above-mentioned stacked body can be housed in a battery exterior 110 (battery case), and the nonaqueous electrolyte solution of the first embodiment can be sealed inside the battery case, thereby manufacturing the nonaqueous secondary battery of the first embodiment.

[0186] Alternatively, the non-aqueous secondary battery 100 can be manufactured by impregnating a substrate composed of a polymer material with a non-aqueous electrolyte to pre-prepare a gel-state electrolyte membrane, forming a stacked structure using a sheet-like positive electrode 150, a negative electrode 160, an electrolyte membrane, and a separator 170 as required, and then housing the stacked structure in a battery casing 110.

[0187] It should be noted that when the configuration of the electrode is designed to have a portion where the peripheral end of the negative electrode active material layer overlaps with the peripheral end of the positive electrode active material layer, or when there is a portion with too small a width in the non-opposite portion of the negative electrode active material layer, the position of the electrode is offset when the battery is assembled, so that the charge and discharge cycle characteristics in the non-aqueous secondary battery may be reduced. Therefore, for the electrode body used in the non-aqueous secondary battery, it is preferred that the position of the electrode is fixed in advance with a tape such as a polyimide tape, a polyphenylene sulfide tape, a polypropylene (PP) tape, an adhesive, etc.

[0188] In the first embodiment, when a non-aqueous electrolyte using acetonitrile is used, due to its high ionic conductivity, the lithium ions released from the positive electrode during the initial charge of the non-aqueous secondary battery are likely to diffuse to the entire negative electrode. In a non-aqueous secondary battery, the area of ​​the negative electrode active material layer is usually made larger than the positive electrode active material layer. However, if the lithium ions diffuse to the position in the negative electrode active material layer that is not opposite to the positive electrode active material layer and are retained, the lithium ions will not be released during the initial discharge and will remain on the negative electrode. Therefore, the contribution of the lithium ions that have not been released becomes the irreversible capacity. For such reasons, in a non-aqueous secondary battery using a non-aqueous electrolyte containing acetonitrile, the initial charge and discharge efficiency is sometimes reduced.

[0189] On the other hand, when the area of ​​the positive electrode active material layer is larger than that of the negative electrode active material layer, or both are equal, current concentration is likely to occur at the edge of the negative electrode active material layer during charging, and lithium dendrites are likely to form.

[0190] Due to the above reasons, the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion where the positive electrode active material layer and the negative electrode active material layer are opposite is not particularly limited, but is preferably greater than 1.0 and less than 1.1, more preferably greater than 1.002 and less than 1.09, further preferably greater than 1.005 and less than 1.08, and particularly preferably greater than 1.01 and less than 1.08. In a non-aqueous secondary battery using a non-aqueous electrolyte containing acetonitrile, the initial charge and discharge efficiency can be improved by reducing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion where the positive electrode active material layer and the negative electrode active material layer are opposite.

[0191] Reducing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion of the positive electrode active material layer opposite to the negative electrode active material layer refers to limiting the ratio of the area of ​​the portion of the negative electrode active material layer that is not opposite to the positive electrode active material layer. Thus, the amount of lithium ions released from the positive electrode during the initial charge that are retained in the portion of the negative electrode active material layer that is not opposite to the positive electrode active material layer (i.e., the amount of lithium ions that are not released from the negative electrode during the initial discharge and become irreversible capacity) can be reduced as much as possible. Therefore, by designing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion of the positive electrode active material layer opposite to the negative electrode active material layer within the above range, the initial charge and discharge efficiency of the battery can be improved while achieving an improvement in the load characteristics of the battery caused by the use of acetonitrile, and further the formation of lithium dendrites can be suppressed.

[0192] The non-aqueous secondary battery 100 in the first embodiment can function as a battery through the initial charge, and a part of the non-aqueous electrolyte is decomposed and stabilized during the initial charge. There is no particular limitation on the method of the initial charge, and the initial charge is preferably performed at 0.001C to 0.3C, more preferably at 0.002C to 0.25C, and further preferably at 0.003C to 0.2C. It is also preferred that the initial charge is performed via constant voltage charging on the way. By setting the voltage range in which the lithium salt participates in the electrochemical reaction to be longer, a stable and strong SEI is formed on the surface of the electrode (negative electrode 160), which has the effect of suppressing the increase of internal resistance. In addition, the reaction product will not be firmly fixed only to the negative electrode 160, and in some form, it also gives a good effect to the components other than the negative electrode 160 such as the positive electrode 150 and the separator 170. Therefore, it is very effective to consider the electrochemical reaction of the lithium salt dissolved in the non-aqueous electrolyte for the initial charge. In addition, it is preferred that the capacity that the negative electrode can absorb is greater than the charge capacity taken out from the positive electrode during charging, so that lithium can be prevented from being precipitated at the negative electrode. The charge capacity at an ambient temperature of 23 to 30° C. is preferably 70% or more and 99% or less relative to the capacity of the negative electrode active material. When the capacity relationship is satisfied, there is no concern about lithium electrolysis on the negative electrode, and since no unnecessary negative electrode capacity remains, the energy density per unit weight and the energy density per unit volume are improved.

[0193] The nonaqueous secondary battery 100 of the first embodiment can also be used as a battery pack in which a plurality of nonaqueous secondary batteries 100 are connected in series or in parallel. From the viewpoint of managing the charge and discharge state of the battery pack, it is preferable that each battery be used in a voltage range of 2 to 5V.

[0194] As mentioned above, although the 1st embodiment of this invention was demonstrated, this invention is not limited to the said embodiment. This invention can be variously modified in the range which does not deviate from the summary.

[0195] <II. Second embodiment>

[0196] The second embodiment of the present invention is described in detail below. In the second embodiment, a non-aqueous secondary battery is provided. The non-aqueous secondary battery of the second embodiment is not limited and may include Figure 1 , 2 The structure of the lithium-ion battery 100 is shown.

[0197] <II-1. Non-aqueous secondary battery>

[0198] The non-aqueous secondary battery of the second embodiment has a negative electrode, a positive electrode, a separator and a non-aqueous electrolyte, and the non-aqueous secondary battery is charged more than once. The negative electrode contains one or more inorganic lithium compounds and organic lithium compounds that can be extracted by immersion in an extraction solvent. Preferably, the positive electrode contains one or more positive electrode active materials that can occlude and release lithium ions, and preferably the negative electrode contains a negative electrode active material containing graphite. In addition, the non-aqueous electrolyte contains acetonitrile and cyclic carbonate as non-aqueous solvents.

[0199] The negative electrode preferably contains a component that can be extracted from the negative electrode by using water as an extraction solvent, and more preferably contains at least one of the following (a) to (d) as a component of the negative electrode coating.

[0200] (a) LiF.

[0201] (b) LiOCOOCH2CH2OCOOLi.

[0202] (c) CH3CH2OCOOLi.

[0203] (d) CH3OCOOLi.

[0204] Here, the negative electrode coating includes a product of a non-aqueous solvent and a decomposition product of an additive that is accompanied by a reduction reaction in the negative electrode when the non-aqueous secondary battery is charged one or more times. The components of the negative electrode coating in the second embodiment can be extracted with an extraction solvent, for example, by immersing in heavy water for more than 72 hours, and the extraction method is not limited to this. In addition, for the quantification of the extracted components, from the perspective of detection sensitivity, for example, for the component (a), it is preferably performed by ion chromatography, and for the components (b) to (d), it is preferably performed by NMR, etc., but it is not particularly limited to this.

[0205] In the second embodiment, the component of (a) can be classified as an inorganic lithium compound, and the components of (b) to (d) can be classified as an organic lithium compound. From the viewpoint of preventing the reduction and decomposition of acetonitrile, the rapid stabilization of the initial battery capacity, and improving the efficiency of the manufacturing process, the negative electrode of the second embodiment preferably comprises at least one of the components of (a) and (b) to (d), or comprises the components of (a) and all of the components of (b) to (d).

[0206] Each of the components is mainly generated on the surface of the negative electrode active material through the reduction reaction of the cyclic carbonate, becoming SEI (Solid Electrolyte Interface). Through SEI, a film that conducts Li ions and does not conduct electrons is formed to prevent further reduction reactions in other solvents. On the other hand, the non-aqueous secondary battery of the second embodiment contains acetonitrile as a non-aqueous solvent for the non-aqueous electrolyte. Acetonitrile has low viscosity and a high dielectric constant, and is coordinated with Li ions so that it is easy to move near the electrode active material during charge and discharge. Therefore, it can be considered that due to this characteristic, the input-output characteristics are easily improved, and further, the stabilization of the electrode capacity ends quickly. On the other hand, acetonitrile can be reduced and decomposed on the surface of the negative electrode active material. The negative electrode coating component in the second embodiment containing acetonitrile includes the components (a) to (d), and the molar ratios of the components relative to the total amount (i.e., total content) of (a) to (d) are as follows: component (a) is preferably 20 mol% to 70 mol%, component (b) is preferably 20 mol% to 70 mol%, component (c) is preferably 1 mol% to 20 mol%, component (d) is preferably 1 mol% to 20 mol%, component (a) is more preferably 20 mol% to 65 mol%, component (b) is more preferably 25 mol% to 65 mol%, component (c) is more preferably 5 mol% to 20 mol%, and component (d) is more preferably 5 to 20 mol%. As described above, a battery in which the coating is formed by containing more (a) and (b) and less (c) and (d) in a composition ratio has a tendency to rapidly stabilize the discharge capacity.

[0207] At this time, the negative electrode may contain PF6 anions, and may also contain N(SO2F)2 anions and / or N(SO2CF3)2 anions. That is, the electrolyte may contain at least one anion selected from the group consisting of PF6 anions, N(SO2CF3)2 or N(SO2F)2 anions. Since the anions promote the formation of a protective film and form a non-conductor film on the surface of the surface foil as the positive electrode collector, it is preferred from the viewpoint of suppressing the increase of internal resistance.

[0208] Specifically, the nonaqueous secondary battery of the second embodiment may be Figure 1 and 2 The non-aqueous secondary battery shown. Here, Figure 1 is a top view schematically showing a non-aqueous secondary battery, Figure 2 is along Figure 1 Cross-sectional view along line AA.

[0209] Figure 1 , Figure 2 The non-aqueous secondary battery 100 shown is composed of a pouch-type battery cell. The non-aqueous secondary battery 100 contains a stacked electrode body (not shown) formed by stacking a positive electrode 150 and a negative electrode 160 via a separator 170 in a space 120 of a battery outer package 110 composed of two sheets of aluminum laminate films, and a non-aqueous electrolyte. The battery outer package 110 is sealed by heat-melting the upper and lower aluminum laminate films at its outer periphery. The stacked body formed by stacking the positive electrode 150, the separator 170, and the negative electrode 160 in sequence is impregnated with a non-aqueous electrolyte.

[0210] The aluminum laminate film constituting the battery exterior 110 is preferably an aluminum laminate film obtained by coating both surfaces of an aluminum foil with a polyolefin-based resin.

[0211] The positive electrode 150 is connected to the positive electrode lead 130 in the non-aqueous secondary battery 100. Although not shown, the negative electrode 160 is also connected to the negative electrode lead 140 in the non-aqueous secondary battery 100. One end of each of the positive electrode lead 130 and the negative electrode lead 140 is led out to the outside of the battery casing 110 so as to be connected to external equipment, etc., and their ionomer parts are thermally welded together with one side of the battery casing 110.

[0212] Figure 1 and 2 The non-aqueous secondary battery 100 shown has a stacked electrode body with one positive electrode 150 and one negative electrode 160, respectively. However, the number of stacked positive electrodes 150 and negative electrodes 160 can be appropriately increased by capacity design. In the case of a stacked electrode body having a plurality of positive electrodes 150 and negative electrodes 160, the tabs of the same pole can be joined to each other by welding, etc., and then joined to a lead body by welding and taken out of the battery. As the tab of the same pole, it can be a method of being composed of an exposed portion of a collector or a method of welding a metal sheet to an exposed portion of a collector.

[0213] The positive electrode 150 is composed of a positive electrode active material layer and a positive electrode current collector, and the positive electrode active material layer is made of a positive electrode mixture. The negative electrode 160 is composed of a negative electrode active material layer and a negative electrode current collector, and the negative electrode active material layer is made of a negative electrode mixture. The positive electrode 150 and the negative electrode 160 are arranged so that the positive electrode active material layer and the negative electrode active material layer face each other via a separator 170.

[0214] There are no particular limitations on these components, and materials used in conventional lithium-ion batteries can be used. Hereinafter, each component of the nonaqueous secondary battery will be described in more detail.

[0215] <II-2. Non-aqueous electrolyte>

[0216] The nonaqueous electrolyte of the second embodiment can have the structure of the nonaqueous electrolyte of the first embodiment shown above. In addition, for the nonaqueous electrolyte, materials used for nonaqueous electrolytes of conventional lithium ion batteries can be applied within the range that does not impair the effects of the present invention.

[0217] The "non-aqueous electrolyte" in the second embodiment refers to an electrolyte containing a non-aqueous solvent and a lithium salt, and having a water content of 1% by mass or less relative to the total amount of the non-aqueous electrolyte. The proportion of water is preferably 300 ppm or less, and more preferably 200 ppm or less. The non-aqueous electrolyte may also contain additives.

[0218] (Non-aqueous solvent)

[0219] Here, the non-aqueous solvent is described. In the second embodiment, the "non-aqueous solvent" refers to the elements other than the lithium salt in the electrolyte. In the second embodiment, when the electrolyte contains an additive, the "non-aqueous solvent" refers to the elements other than the lithium salt and the additive in the electrolyte.

[0220] The non-aqueous solvent of the second embodiment includes acetonitrile as an essential component. Moreover, relative to the total amount of the non-aqueous electrolyte, the content of acetonitrile is preferably 1% by mass or more and 60% by mass or less, more preferably 3% by mass or more and 50% by mass or less, and further preferably 5% by mass or more and 40% by mass or less. By including a specified amount of acetonitrile, the non-aqueous secondary battery in the second embodiment has a tendency to have excellent input and output performance. However, in addition to acetonitrile, the non-aqueous solvent may also contain other non-aqueous solvents. As non-aqueous solvents other than acetonitrile, for example, alcohols such as methanol and ethanol can be cited; aprotic solvents, etc. Among them, aprotic polar solvents are preferred.

[0221] Specific examples of the aprotic solvent in the non-aqueous solvent include, for example, cyclic carbonates represented by ethylene carbonate, propylene carbonate, 1,2-butenyl carbonate, trans-2,3-butenyl carbonate, cis-2,3-butenyl carbonate, 1,2-pentenyl carbonate, trans-2,3-pentenyl carbonate, cis-2,3-pentenyl carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinyl carbonate; 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, Fluorinated ethylene carbonates represented by 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one; lactones represented by γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone; ethylene sulfite, propylene sulfite, butylene sulfite, pentylene sulfite, cyclopentane sulfone, 3-cyclobutene sulfone, 3-methylcyclopentane sulfone, 1,3-propane sultone, 1,4-butane sultone, 1-propylene-1,3-sultone, dimethyl sulfoxide, tetramethylene sulfoxide, and ethylene glycol sulfite as represented The sulfur compounds of the table; cyclic ethers represented by tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and 1,3-dioxane; chain carbonates represented by ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, ethyl propyl carbonate, and methyl trifluoroethyl carbonate; chain fluorinated carbonates represented by dimethyl trifluorocarbonate, diethyl trifluorocarbonate, and methyl ethyl trifluorocarbonate; mononitriles represented by propionitrile, butyronitrile, valeronitrile, benzonitrile, and acrylonitrile; alkoxy-substituted nitriles represented by methoxyacetonitrile and 3-methoxypropionitrile; malononitrile, succinonitrile, glutaronitrile, adiponitrile, 1,4- dinitriles represented by dicyanoheptane, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 2,6-dicyanoheptane, 1,8-dicyanooctane, 2,7-dicyanooctane, 1,9-dicyanononane, 2,8-dicyanononane, 1,10-dicyanodecane, 1,6-dicyanodecane, and 2,4-dimethylglutaronitrile; cyclic nitriles represented by benzonitrile; chain esters represented by methyl propionate; chain ethers represented by dimethoxyethane, ethyl ether, 1,3-dioxolane, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), and tetraethylene glycol dimethyl ether (tetraglyme); 4 -OR 5 (wherein, Rf4 is an alkyl group containing a fluorine atom, R5 In addition to fluorinated ethers represented by acetone, methyl ethyl ketone, and methyl isobutyl ketone, halides represented by their fluorides can be cited. They can be used alone or in combination of two or more.

[0222] In addition, in these other non-aqueous solvents, it is preferred to use one or more of cyclic carbonates and chain carbonates. The non-aqueous secondary battery of the second embodiment more preferably contains cyclic carbonates in non-aqueous electrolytes, and particularly preferably contains ethylene carbonate and vinylene carbonate as cyclic carbonates. It is possible to choose to use only one of other cyclic carbonates and chain carbonates in the aforementioned materials for example, or two or more (for example, two or more of the cyclic carbonates for the aforementioned examples, two or more of the chain carbonates for the aforementioned examples, or two or more of the cyclic carbonates for the aforementioned examples and the chain carbonates for the aforementioned examples). Wherein, as cyclic carbonates, more preferably propylene carbonate or fluoroethylene carbonate, as chain carbonates, more preferably ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate.

[0223] The vinyl carbonate has high reactivity and is consumed according to the amount of the negative electrode during the initial charge, promoting the formation of SEI. In the second embodiment, it can be considered that in order to form a good SEI, by fully adding before the initial charge of the battery so that ethylene carbonate and vinyl carbonate remain in a specified amount after forming the coating, the formation of SEI is carried out faster than the reduction reaction of acetonitrile on the surface of the negative electrode active material. It can be considered that this rapid SEI formation reaction is achieved by the competitive reaction of ethylene carbonate and vinyl carbonate, and preferably both are contained in a specified ratio. After the SEI formation reaction is carried out by the initial charge, the molar ratio of the residual vinyl carbonate is preferably 0.01mol% to 30mol%, more preferably 0.1mol% to 30mol%, further preferably 0.3mol% to 25mol%, and particularly preferably 1mol% to 20mol% relative to the ethylene carbonate contained in the non-aqueous electrolyte of the second embodiment.

[0224] As mentioned above, in order to make the vinylene carbonate residual predetermined amount relative to ethylene carbonate, the non-aqueous secondary battery in the second embodiment only needs to contain an appropriate non-aqueous electrolyte before the initial charge. Relative to the total amount of the non-aqueous electrolyte, the content of vinylene carbonate is preferably 0.1 mass % or more and 10 mass % or less to keep good reactivity. On the other hand, in the case where the residual vinylene carbonate disappears after the initial charge, it is necessary to adjust the addition amount at any time according to the content in the battery of the non-aqueous electrolyte, the content of acetonitrile and the negative electrode amount of the battery to make the initial charge and discharge stable. From this viewpoint, in order to manufacture the non-aqueous secondary battery in the second embodiment, the non-aqueous electrolyte enclosed in the battery can also have the structure of the first embodiment. In addition, vinylene carbonate not only contributes to the reaction formation of SEI, but also is a solvent suitable for dissolving lithium salts, therefore, relative to the total amount of the non-aqueous electrolyte, the content of vinylene carbonate is preferably 5 mass % or more and 35 mass % or less, and further preferably 10 mass % or more and 30 mass % or less.

[0225] (Lithium Salt)

[0226] The lithium salt is not particularly limited within the range not impairing the effects of the present invention. For example, in the second embodiment, the lithium salt may include a fluorine-containing inorganic lithium salt and / or an imide salt.

[0227] Imidate salt refers to LiN(SO2C m F 2m+1 )2〔wherein m is an integer from 0 to 8〕a lithium salt represented by, specifically, preferably comprising LiN(SO2F)2 and / or LiN(SO2CF3)2. Since the decomposition temperature of the imide salt itself is high, the increase in resistance during high-temperature storage is suppressed. In addition, since the viscosity as a non-aqueous electrolyte is suppressed to a low level, it is possible to exert excellent output performance, especially in low-temperature regions. Relative to the total amount of the non-aqueous electrolyte of the second embodiment, the content of the imide salt is preferably in the range of 0.1 mass % to 40 mass %, more preferably in the range of 0.2 mass % to 30 mass %, and further preferably in the range of 0.5 mass % to 20 mass %. By being within this range, the performance under low-temperature conditions can be improved without reducing the ion conductivity of the non-aqueous electrolyte.

[0228] A typical fluorine-containing inorganic lithium salt is LiPF6 which dissolves and releases PF6 anions. However, the non-aqueous electrolyte may also contain fluorine-containing inorganic lithium salts other than LiPF6. Examples of such fluorine-containing inorganic lithium salts include LiBF4, LiAsF6, Li2SiF6, LiSbF6, Li2B 12 F b H 12-b[wherein b is an integer of 0 to 3], etc. In the second embodiment, the "fluorine-containing inorganic lithium salt" refers to a lithium salt that does not contain carbon atoms in the anion but contains fluorine atoms in the anion. The fluorine-containing inorganic lithium salt forms a passivation film on the surface of the metal foil as the positive electrode collector and is excellent in suppressing corrosion of the positive electrode collector. These fluorine-containing inorganic lithium salts are used alone or in combination of two or more.

[0229] The content of the fluorine-containing inorganic lithium salt in the non-aqueous electrolyte of the second embodiment is not particularly limited, but is preferably 0.1 mol or more, more preferably 0.2 mol or more, and further preferably 0.25 mol or more relative to 1 L of the non-aqueous solvent. When the content of the fluorine-containing inorganic lithium salt is within the above range, there is a tendency that the ion conductivity increases and high output characteristics can be exhibited.

[0230] The non-aqueous electrolyte solution of the second embodiment may further contain an organic lithium salt. In the second embodiment, the "organic lithium salt" refers to a lithium salt containing a carbon atom in the anion.

[0231] As the organic lithium salt, an organic lithium salt having an oxalic acid group can be cited. As a specific example of the organic lithium salt having an oxalic acid group, for example, organic lithium salts represented by LiB(C2O4)2, LiBF2(C2O4), LiPF4(C2O4), and LiPF2(C2O4)2 can be cited, among which at least one lithium salt selected from the lithium salts represented by LiB(C2O4)2 and LiBF2(C2O4) is preferred. In addition, it is more preferred to use one or more of them together with a fluorine-containing inorganic lithium salt.

[0232] From the viewpoint of better ensuring the effect of its use, the amount of the organic lithium salt with oxalic acid group added in the non-aqueous electrolyte is preferably 0.005 moles or more, more preferably 0.02 moles or more, and further preferably 0.05 moles or more relative to the amount of 1L of the non-aqueous solvent of the non-aqueous electrolyte. However, when the amount of the organic lithium salt with oxalic acid group in the non-aqueous electrolyte is too much, it is possible to precipitate. Therefore, based on the amount of 1L of the non-aqueous solvent of the non-aqueous electrolyte, the amount of the organic lithium salt with oxalic acid group added in the non-aqueous electrolyte is preferably less than 1.0 moles, more preferably less than 0.5 moles, and further preferably less than 0.2 moles.

[0233] It is known that organic lithium salts having oxalate groups are poorly soluble in organic solvents with low polarity, especially in linear carbonates. Organic lithium salts having oxalate groups sometimes contain trace amounts of lithium oxalate, and further, when mixed as a non-aqueous electrolyte, sometimes react with trace amounts of water contained in other raw materials to produce new white precipitates of lithium oxalate. Therefore, the content of lithium oxalate in the non-aqueous electrolyte of the second embodiment is not particularly limited, and is preferably 0 to 500 ppm.

[0234] As the lithium salt in the second embodiment, in addition to the above, other lithium salts commonly used in non-aqueous secondary batteries may be added as an auxiliary. Specific examples of other lithium salts include LiClO4, LiAlO4, LiAlCl4, LiB 10 Cl 10 , inorganic lithium salts containing no fluorine atoms in anions such as lithium borochloride; LiCF3SO3, LiCF3CO2, Li2C2F4(SO3)2, LiC(CF3SO2)3, LiC n F 2n+1 SO3 (where n≥2), organic lithium salts such as lower aliphatic carboxylic acid Li, tetraphenylborate Li, etc.; LiPF5 (CF3) and other organic lithium salts made from LiPF n (C p F 2p+1 ) 6-n [wherein n is an integer of 1 to 5, and p is an integer of 1 to 8] an organic lithium salt represented by LiBF3(CF3) or the like q (C s F 2s+1 ) 4-q [wherein q is an integer of 1 to 3 and s is an integer of 1 to 8]; a lithium salt bonded to a polyvalent anion; an organic lithium salt represented by the following formulae (7a), (7b) and (7c), etc.

[0235] LiC(SO2R 6 )(SO2R 7 )(SO2R 8 )(7a)

[0236] LiN(SO2OR 9 )(SO2OR 10 )(7b)

[0237] LiN(SO2R 11 )(SO2OR 12 )(7c)

[0238] {In the formula, R 6 , R 7 , R 8 , R 9 , R 10 , R 11 and R 12 They may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms.

[0239] At least one selected from the group consisting of fluorine-containing inorganic lithium salts, imide salts, and organic lithium salts can be used together with one or more of them.

[0240] (additive)

[0241] In the second embodiment, for example, the non-aqueous electrolyte may appropriately contain any additive selected from anhydrides, sulfonates, diphenyl disulfide, cyclohexylbenzene, biphenyl, fluorobenzene, tert-butylbenzene, phosphates [ethyl diethylphosphonoacetate (EDPA): (C2H5O)2(P=O)-CH2(C=O)OC2H5; tris(trifluoroethyl) phosphate (TFEP): (CF3CH2O)3P=O; triphenyl phosphate (TPP): (C6H5O)3P=O; triallyl phosphate: (CH2=CHCH2O)3P=O, etc.] and derivatives of these compounds. In particular, the phosphates are effective in inhibiting side reactions during storage.

[0242] (Other optional additives)

[0243] In the second embodiment, for the purpose of improving the high-temperature storage property and safety of the non-aqueous secondary battery, the non-aqueous electrolyte may appropriately contain any additive selected from, for example, sulfonates, diphenyl disulfide, cyclohexylbenzene, biphenyl, fluorobenzene, tert-butylbenzene, phosphates [ethyl diethylphosphonoacetate (EDPA): (C2H5O)2(P=O)-CH2(C=O)OC2H5; tris(trifluoroethyl) phosphate (TFEP): (CF3CH2O)3P=O; triphenyl phosphate (TPP): (C6H5O)3P=O; triallyl phosphate: (CH2=CHCH2O)3P=O, etc.], nitrogen-containing cyclic compounds having no steric hindrance around non-covalent electron pairs [pyridine, 1-methyl-1H-benzotriazole, 1-methylpyrazole, etc.], and derivatives of these compounds. In particular, the phosphoric acid esters are effective in suppressing side reactions during high-temperature storage.

[0244] The content of other arbitrary additives is calculated by the mass percentage relative to the total mass of all components constituting the non-aqueous electrolyte. The content of other arbitrary additives is not particularly limited, and relative to the total amount of the non-aqueous electrolyte, it is preferably in the range of 0.01 mass % or more and 10 mass % or less, more preferably 0.02 mass % or more and 5 mass % or less, and further preferably 0.05 mass % to 3 mass %. By adjusting the content of other arbitrary additives within the above range, there is a tendency to be able to add better battery characteristics without damaging the basic function as a non-aqueous secondary battery.

[0245] <II-3. Positive electrode>

[0246] The positive electrode 150 is composed of a positive electrode active material layer made of a positive electrode mixture and a positive electrode current collector. The positive electrode 150 is not particularly limited as long as it functions as a positive electrode of a non-aqueous secondary battery within the scope of the present invention.

[0247] The positive electrode active material layer contains a positive electrode active material and may further contain a conductive auxiliary agent and a binder.

[0248] Preferably, the positive electrode active material layer contains a material capable of absorbing and releasing lithium ions as the positive electrode active material. Preferably, the positive electrode active material layer contains the positive electrode active material and a conductive aid and a binder as required. When such a material is used, it tends to be able to obtain a high voltage and a high energy density, so it is preferred.

[0249] Examples of the positive electrode active material include lithium-containing compounds represented by the following formulae (8a) and (8b), and other lithium-containing compounds.

[0250] Li x MO2(8a)

[0251] Li y M2O4(8b)

[0252] {In the formula, M represents one or more metal elements including at least one transition metal element, x represents a number of 0 to 1.1, and y represents a number of 0 to 2.}

[0253] As lithium-containing compounds represented by formula (8a) and (8b), for example, lithium cobalt oxide represented by LiCoO2; lithium manganese oxide represented by LiMnO2, LiMn2O4 and Li2Mn2O4; lithium nickel oxide represented by LiNiO2; z Lithium-containing composite metal oxides represented by MO2 (wherein M includes at least one transition metal element selected from the group consisting of Ni, Mn and Co, and represents two or more metal elements selected from the group consisting of Ni, Mn, Co, Al and Mg, and z represents a number greater than 0.9 and less than 1.2).

[0254] The lithium-containing compound other than the lithium-containing compound represented by formula (8a) and (8b) is not particularly limited as long as it contains lithium. Examples of such lithium-containing compounds include composite oxides containing lithium and transition metal elements, metal sulfides containing lithium, metal phosphate compounds containing lithium and transition metal elements, and metal silicate compounds containing lithium and transition metal elements (e.g., Li t M uSiO4, M have the same meanings as in formula (8a), t represents a number from 0 to 1, and u represents a number from 0 to 2). From the viewpoint of obtaining a higher voltage, the lithium-containing compound is preferably a composite oxide and a metal phosphate compound containing lithium and at least one transition metal element selected from the group consisting of cobalt (Co), nickel (Ni), manganese (Mn), iron (Fe), copper (Cu), zinc (Zn), chromium (Cr), vanadium (V) and titanium (Ti).

[0255] More specifically, lithium-containing compounds are preferably composite oxides containing lithium and transition metal elements or metal chalcogenides containing lithium and transition metal elements, and metal phosphate compounds containing lithium. Examples thereof include compounds represented by the following formulae (9a) and (9b), respectively.

[0256] Li v M I D2(9a)

[0257] Li w M II PO4(9b)

[0258] {wherein, D represents oxygen or a chalcogen element, M I and M II Respectively represent one or more transition metal elements, v and w values ​​are determined by the charge and discharge state of the battery, v represents 0.05 to 1.10, and w represents a number from 0.05 to 1.10.}

[0259] The lithium-containing compound represented by the above formula (9a) has a layered structure, and the compound represented by the above formula (9b) has an olivine structure. For the purpose of stabilizing the structure, these lithium-containing compounds can be compounds in which a part of the transition metal elements is replaced by Al, Mg or other transition metal elements, compounds in which these metal elements are contained in the grain boundaries, compounds in which a part of the oxygen atoms are replaced by fluorine atoms, compounds in which other positive electrode active materials are coated on at least a part of the surface of the positive electrode active material, etc.

[0260] As the positive electrode active material in the second embodiment, only the above-mentioned lithium-containing compound may be used, or other positive electrode active materials may be used in combination with the lithium-containing compound.

[0261] As such other positive electrode active materials, for example, metal oxides or metal chalcogenides having a tunnel structure and a layered structure; sulfur; conductive polymers, etc. As metal oxides or metal chalcogenides having a tunnel structure and a layered structure, for example, MnO2, FeO2, FeS2, V2O5, V6O 13Oxides, sulfides, selenides, etc. of metals other than lithium represented by TiO2, TiS2, MoS2, and NbSe2. As conductive polymers, for example, conductive polymers represented by polyaniline, polythiophene, polyacetylene, and polypyrrole can be cited.

[0262] The above-mentioned other positive electrode active materials can be used alone or in combination of two or more, without particular limitation. However, since lithium ions can be reversibly and stably absorbed and released, and high energy density can be achieved, the preferred positive electrode active material layer contains at least one transition metal element selected from Ni, Mn and Co.

[0263] When a lithium-containing compound and other positive electrode active materials are used together as positive electrode active materials, the ratio of the two, as well as the ratio of the lithium-containing compound to the total positive electrode active materials, is preferably 80% by mass or more, more preferably 85% by mass or more.

[0264] Examples of the conductive aid include carbon black represented by graphite, acetylene black and Ketjen black, and carbon fiber. The conductive aid content is preferably 10 parts by mass or less, more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the positive electrode active material.

[0265] Examples of the binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid, styrene butadiene rubber, and fluororubber. The binder content is preferably 6 parts by mass or less, more preferably 0.5 to 4 parts by mass, relative to 100 parts by mass of the positive electrode active material.

[0266] The positive electrode mixture formed by mixing the positive active material, the conductive aid as needed and the binder is dispersed in a solvent to form a slurry containing the positive electrode mixture, and the slurry containing the positive electrode mixture is applied to the positive electrode collector and dried (removing the solvent), and pressed as needed to form a positive electrode active material layer. As such a solvent, it is not particularly limited, and known solvents can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be cited.

[0267] The positive electrode current collector is composed of metal foil such as aluminum foil, nickel foil, stainless steel foil, etc. The positive electrode current collector may be carbon-coated on the surface or processed into a mesh shape. The thickness of the positive electrode current collector is preferably 5 μm to 40 μm, more preferably 7 μm to 35 μm, and further preferably 9 μm to 30 μm.

[0268] <II-4. Negative electrode>

[0269] The negative electrode 160 is composed of a negative electrode active material layer made of a negative electrode mixture and a negative electrode current collector. The negative electrode 160 is not particularly limited as long as it functions as a negative electrode of a non-aqueous secondary battery within the scope of the present invention.

[0270] In order to increase the battery voltage, the negative electrode active material layer preferably contains a negative electrode active material capable of reacting at a ratio of 0.4 V (vs. Li / Li + ) A material that absorbs lithium ions at a lower potential. Preferably, the negative electrode active material layer contains a negative electrode active material and additives, a conductive aid, and a binder as required. Here, the negative electrode active material layer contains a decomposition product of a cyclic carbonate such as an inorganic lithium compound and an organic lithium compound as described above.

[0271] As negative electrode active materials, for example, in addition to carbon materials represented by amorphous carbon (hard carbon), artificial graphite, natural graphite, graphite, pyrolytic carbon, coke, glassy carbon, sintered bodies of organic polymer compounds, mesophase carbon microbeads, carbon fibers, activated carbon, carbon colloids and carbon black, metallic lithium, metal oxides, metal nitrides, lithium alloys, tin alloys, silicon alloys, intermetallic compounds, organic compounds, inorganic compounds, metal complexes, organic polymer compounds, etc. can be cited.

[0272] In the second embodiment, the negative electrode active material may contain SiOx (0.5≤x≤1.5) or an element capable of forming an alloy with lithium, such element being, for example, silicon. Silicon may be in any form of a crystalline, low-crystalline, or amorphous body. In addition, it is preferred to increase the conductivity between particles by coating the surface of the active material with a conductive material. In particular, the working potential of silicon is about 0.5 V (relative to Li / Li + ), the working potential relative to graphite is about 0.05V (relative to Li / Li + ) is slightly higher, thus reducing the danger of lithium electrolysis. Acetonitrile, the non-aqueous solvent used in the second embodiment, undergoes a reduction reaction with lithium metal, causing gas generation. Therefore, a negative electrode active material that is difficult to undergo lithium electrolysis is preferred in combination with a nitrile electrolyte. On the other hand, a negative electrode active material with an excessively high working potential will reduce the energy density of the battery. Therefore, from the viewpoint of improving energy density, it is preferred that the negative electrode active material be at a working potential of less than 0.4V (relative to Li / Li + ) works at lower potentials.

[0273] The content of silicon is preferably in the range of 0.1 mass % to 100 mass % relative to the total amount of the negative electrode mixture of the second embodiment, more preferably in the range of 1 mass % to 80 mass %, and further preferably in the range of 3 mass % to 60 mass %. By adjusting the content of silicon within the above range, the balance between the high capacity and the charge and discharge cycle performance of the non-aqueous secondary battery can be ensured.

[0274] The negative electrode active material may be used alone or in combination of two or more.

[0275] Examples of the conductive aid include carbon black represented by graphite, acetylene black and Ketjen black, and carbon fiber. The content of the conductive aid is preferably 20 parts by mass or less, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the negative electrode active material.

[0276] Examples of the binder include carboxymethyl cellulose, PVDF, PTFE, polyacrylic acid, styrene butadiene rubber, polyimide, polyamide imide, and fluororubber. The binder content is preferably 10 parts by mass or less, more preferably 0.5 to 6 parts by mass, relative to 100 parts by mass of the negative electrode active material.

[0277] The negative electrode active material and the negative electrode mixture formed by mixing the conductive aid and the binder as needed are dispersed in a solvent to form a slurry containing the negative electrode mixture, and the slurry containing the negative electrode mixture is applied to the negative electrode collector and dried (removing the solvent), and pressed as needed to form a negative electrode active material layer. As such a solvent, there is no particular limitation, and known solvents can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be cited.

[0278] The negative electrode current collector is composed of metal foil such as copper foil, nickel foil, stainless steel foil, etc. In addition, the negative electrode current collector may be carbon-coated on the surface or processed into a mesh shape. The thickness of the negative electrode current collector is preferably 5 μm to 40 μm, more preferably 6 μm to 35 μm, and further preferably 7 μm to 30 μm.

[0279] <II-5. Spacer>

[0280] For the non-aqueous secondary battery 100 in the second embodiment, from the viewpoint of providing safety such as preventing short circuit and shutdown of the positive electrode 150 and the negative electrode 160, it is preferred to have a separator 170 between the positive electrode 150 and the negative electrode 160. As the separator 170, there is no limitation, and the same separator as the separator provided in the known non-aqueous secondary battery can be used, preferably an insulating film with large ion permeability and excellent mechanical strength. As the separator 170, for example, woven fabric, non-woven fabric, synthetic resin microporous film, etc. can be cited, among which synthetic resin microporous film is preferred.

[0281] As the synthetic resin microporous membrane, for example, a polyolefin-based microporous membrane such as a microporous membrane containing polyethylene or polypropylene as the main component or a microporous membrane containing both of these polyolefins is preferably used. As the nonwoven fabric, for example, a porous membrane made of heat-resistant resins such as glass, ceramic, polyolefin, polyester, polyamide, liquid crystal polyester, and aromatic polyamide can be cited.

[0282] The spacer 170 may be a single layer or multiple layers of a microporous film, or a structure of two or more microporous films stacked together. The spacer 170 may also be a single layer or multiple layers of a mixed resin material obtained by melt-kneading two or more resin materials.

[0283] By using such a separator 170, it is particularly possible to achieve the good input-output characteristics and low self-discharge characteristics required by the lithium-ion secondary battery for the above-mentioned high-output purpose. The film thickness of the microporous membrane is not particularly limited. From the perspective of membrane strength, it is preferably 1 μm or more, and from the perspective of permeability, it is preferably 500 μm or less. From the perspective of high-output uses such as safety tests that have a high heat release and require self-discharge characteristics that are higher than before, and from the perspective of windability in large battery winding machines, the film thickness is preferably 5 μm or more and 30 μm or less, and more preferably 10 μm or more and 25 μm or less. It should be noted that in the case of taking into account both short-circuit resistance and output performance, the film thickness is further preferably 15 μm or more and 25 μm or less, and in the case of taking into account both high energy density and output performance, it is further preferably 10 μm or more and less than 15 μm. From the viewpoint of following the rapid movement of lithium ions at high output, the porosity of the membrane is preferably 30% or more and 90% or less, more preferably 35% or more and 80% or less, and further preferably 40% or more and 70% or less. It should be noted that, in the case of giving priority to improving output performance while ensuring safety, the porosity of the membrane is particularly preferably 50% or more and 70% or less. In the case of emphasizing both short-circuit resistance and output performance, it is particularly preferably 40% or more and less than 50%. From the viewpoint of balancing the membrane thickness and porosity, the air permeability of the membrane is preferably 1 second / 100cm 3 Above and 400 seconds / 100cm 3 Less than 100 sec / 100 cm 3 Above and 350 / 100cm 3 It should be noted that, when emphasizing both short-circuit resistance and output performance, the air permeability of the film is particularly preferably 150 sec / 100 cm 3 Above and 350 seconds / 100cm 3Below, when giving priority to improving output performance while ensuring safety, 100 / 100cm is particularly preferred. 3 More than 1 second and less than 150 seconds / 100cm 3 .

[0284] <II-6. Battery packaging>

[0285] The structure of the battery exterior 110 of the non-aqueous secondary battery 100 in the second embodiment is not particularly limited. For example, any one of a battery can and a laminated film exterior can be used. As a battery can, for example, a metal can made of steel or aluminum can be used. As a laminated film exterior, for example, a laminated film composed of a three-layer structure of hot melt resin / metal film / resin can be used.

[0286] The laminated film outer casing can overlap two pieces with the hot melt resin side facing inward, or be bent into a state with the hot melt resin side facing inward, so that it can be used as an outer casing in a state where the ends are sealed by heat sealing. When a laminated film outer casing is used, the positive lead 130 (or the positive terminal and the lead tab connected to the positive terminal) can be connected to the positive electrode collector, and the negative lead 140 (or the negative terminal and the lead tab connected to the negative terminal) can be connected to the negative electrode collector. In this case, the laminated film outer casing can be packaged in a state where the ends of the positive lead 130 and the negative lead 140 (or the lead tabs connected to the positive terminal and the negative terminal, respectively) are led out to the outside of the outer casing.

[0287] <II-7. Method for producing non-aqueous electrolyte solution>

[0288] The nonaqueous electrolyte solution of the second embodiment can be produced by mixing a nonaqueous solvent containing acetonitrile and a cyclic carbonate with a lithium salt by any method. Furthermore, the nonaqueous electrolyte solution can be produced by mixing an additive in addition to vinylene carbonate by any method.

[0289] <II-8. Method for manufacturing battery>

[0290] The nonaqueous secondary battery 100 in the second embodiment is manufactured by a known method using the above-mentioned nonaqueous electrolyte, a positive electrode 150 having a positive electrode active material layer on one or both sides of a current collector, a negative electrode 160 having a negative electrode active material layer on one or both sides of a current collector, a battery casing 110, and a separator 170 as required.

[0291] First, a laminated body consisting of a positive electrode 150 and a negative electrode 160 and a separator 170 as required is formed. For example, a method of winding a laminated body of a wound structure by winding a long positive electrode 150 and a negative electrode 160 in a stacked state with the long separator sandwiched between the positive electrode 150 and the negative electrode 160; a method of cutting the positive electrode 150 and the negative electrode 160 into a plurality of sheets having a predetermined area and shape to obtain positive electrode sheets and negative electrode sheets, and forming a laminated body of a laminated structure in which the obtained positive electrode sheets and negative electrode sheets are alternately stacked via separator sheets; a method of bending a long separator to form a laminated body of a laminated structure in which positive electrode sheets and negative electrode sheets are alternately inserted between the bent separators; etc.

[0292] Then, the stack is housed in a battery case 110 (battery box) and the nonaqueous electrolyte of the second embodiment is sealed inside the battery box, thereby producing the nonaqueous secondary battery of the second embodiment. The nonaqueous electrolyte may have the structure of the first embodiment.

[0293] Alternatively, a non-aqueous secondary battery 100 can be manufactured by impregnating a substrate made of a polymer material with an electrolyte solution to prepare a gel-state electrolyte membrane in advance, forming a stacked structure using a sheet-like positive electrode 150, a negative electrode 160, an electrolyte membrane, and a separator 170 as required, and housing the stacked structure in a battery casing 110.

[0294] The shape of the nonaqueous secondary battery 100 in the second embodiment is not particularly limited, and may be, for example, cylindrical, oval, rectangular, button, coin, flat, or laminated. In the second embodiment, a laminated type is particularly preferred.

[0295] It should be noted that when the configuration of the electrode is designed to have a portion where the outer peripheral end of the negative electrode active material layer overlaps with the outer peripheral end of the positive electrode active material layer, or when there is a portion with too small a width in the non-opposite portion of the negative electrode active material layer, the position of the electrode is offset when the battery is assembled, so that the charge and discharge cycle characteristics in the non-aqueous secondary battery may be reduced. Therefore, for the electrode body used in the non-aqueous secondary battery, it is preferred to fix the position of the electrode in advance with a tape such as a polyimide tape, a polyphenylene sulfide tape, a PP tape, an adhesive, etc.

[0296] The non-aqueous secondary battery 100 in the second embodiment can function as a battery by the initial charge, and is stabilized by the decomposition of a portion of the electrolyte during the initial charge. There is no particular limitation on the method of the initial charge, and the initial charge is preferably performed at 0.001C to 0.3C, more preferably at 0.002C to 0.25C, and further preferably at 0.003C to 0.2C. The initial charge can also obtain a preferred result by performing constant voltage charging during the initial charge. By setting the voltage range in which the lithium salt participates in the electrochemical reaction to be longer, SEI is formed on the electrode surface, which has the effect of suppressing the increase of the internal resistance including the positive electrode 150. In addition, the reaction product will not be firmly fixed only to the negative electrode 160, and in some form, it also gives a good effect to the components other than the negative electrode 160 such as the positive electrode 150 and the separator 170. Therefore, it is very effective to consider the electrochemical reaction of the lithium salt dissolved in the non-aqueous electrolyte for the initial charge.

[0297] The nonaqueous secondary battery 100 in the second embodiment can also be used as a battery cell group formed by connecting a plurality of nonaqueous secondary batteries 100 in series or in parallel. From the perspective of managing the charge and discharge state of the battery cell group, the operating voltage range of each nonaqueous secondary battery is preferably 2 to 5V, more preferably 2 to 4.5V, and particularly preferably 2V to 4V.

[0298] As mentioned above, although the 2nd embodiment of this invention was demonstrated, this invention is not limited to the said embodiment. This invention can be variously modified in the range which does not deviate from the summary.

[0299] <III. Third embodiment>

[0300] The third embodiment of the present invention is described in detail below. In the third embodiment, a non-aqueous secondary battery or a method for manufacturing the same and a secondary battery manufacturing process are provided. The non-aqueous secondary battery of the third embodiment is not limited and may include Figure 1 , 2 The structure of the lithium-ion battery 100 is shown.

[0301] <III-1. Non-aqueous electrolyte>

[0302] The "non-aqueous electrolyte" in the third embodiment refers to a non-aqueous electrolyte in which water is less than 1% by mass relative to the total amount of the non-aqueous electrolyte and contains a non-aqueous solvent and LiPF6. The non-aqueous electrolyte of the third embodiment preferably contains no water as much as possible, and may contain a very small amount of water as long as it does not hinder the solution of the problem of the present invention. As an amount relative to the total amount of the non-aqueous electrolyte, such a moisture content is less than 300 mass ppm, preferably less than 200 mass ppm. For the non-aqueous electrolyte, as long as it has a structure for achieving the solution of the problem of the present invention, regarding other constituent elements, the constituent materials in the known non-aqueous electrolyte for lithium-ion batteries can be appropriately selected for application.

[0303] <III-1-1. Non-aqueous solvent>

[0304] In the third embodiment, the "non-aqueous solvent" refers to the elements other than lithium salts and various additives removed from the non-aqueous electrolyte. In the third embodiment, when the non-aqueous electrolyte contains an electrode protection additive, the "non-aqueous solvent" refers to the elements other than lithium salts and additives other than the electrode protection additive removed from the non-aqueous electrolyte. As the non-aqueous solvent, for example, alcohols such as methanol and ethanol; aprotic solvents, etc. can be cited. Among them, as the non-aqueous solvent, aprotic solvents are preferred. The non-aqueous solvent may also include solvents other than non-protonic solvents as long as it does not hinder the solution of the subject of the present invention.

[0305] The non-aqueous solvent of the non-aqueous electrolyte of the third embodiment contains acetonitrile as a non-protonic solvent. By containing acetonitrile in the non-aqueous solvent, since the ion conductivity of the non-aqueous electrolyte is improved, the diffusivity of the lithium ions in the battery can be improved. Therefore, when the non-aqueous electrolyte contains acetonitrile, especially in the positive electrode in which the filling amount of the positive electrode active material is increased by thickening the positive electrode active material layer, the lithium ions can also be well diffused to the area near the collector that is difficult for the lithium ions to reach during high-load discharge. Thus, sufficient capacity can also be derived during high-load discharge, and a non-aqueous secondary battery with excellent load characteristics can be obtained.

[0306] In addition, by including acetonitrile in the non-aqueous solvent, the rapid charging characteristics of the non-aqueous secondary battery can be improved. In the constant current (CC)-constant voltage (CV) charging of the non-aqueous secondary battery, the capacity per unit time during the CC charging period is greater than the charging capacity per unit time during the CV charging period. When acetonitrile is used in the non-aqueous solvent of the non-aqueous electrolyte, in addition to increasing the area where CC charging can be performed (extending the time of CC charging), the charging current can also be increased, and therefore, the time from the start of charging of the non-aqueous secondary battery to the fully charged state can be significantly shortened.

[0307] It should be noted that acetonitrile is easily decomposed by electrochemical reduction. Therefore, when using acetonitrile, preferably, as a non-aqueous solvent, other solvents (for example, aprotic solvents except acetonitrile) are used together with acetonitrile, and / or an electrode protection additive for forming a protective coating to an electrode is added.

[0308] Relative to the total amount of non-aqueous solvent, the content of acetonitrile in the non-aqueous solvent is preferably 5 volume % to 60 volume %. Relative to the total amount of non-aqueous solvent, the lower limit of the content of acetonitrile is preferably more than 5 volume %, more preferably more than 10 volume %. Relative to the total amount of non-aqueous solvent, the upper limit of the content of acetonitrile is more preferably less than 60 volume %, more preferably less than 50 volume %. In addition, when the content of acetonitrile in the non-aqueous solvent is within the above-mentioned range, there is a tendency to keep the excellent performance of acetonitrile and to make the high temperature cycle characteristics of the non-aqueous secondary battery and other battery characteristics better.

[0309] As the aprotic solvent other than acetonitrile, for example, cyclic carbonates, fluoroethylene carbonates, lactones, organic compounds having sulfur atoms, chain fluorinated carbonates, cyclic ethers, mononitriles other than acetonitrile, alkoxy-substituted nitriles, dinitriles, cyclic nitriles, short-chain fatty acid esters, chain ethers, fluorinated ethers, ketones, compounds in which a part or all of the H atoms of the aprotic solvent are substituted with halogen atoms, etc. can be cited.

[0310] Since acetonitrile, which is a component of the non-aqueous solvent, is easily decomposed by electrochemical reduction, the non-aqueous electrolyte solution of the third embodiment adds vinylene carbonate, thereby stabilizing the charge and discharge capacity of the battery when used in a non-aqueous secondary battery.

[0311] The nonaqueous electrolyte solution of the third embodiment, in which the nonaqueous solvent includes acetonitrile, vinylene carbonate as a cyclic carbonate, and vinyl sulfite as an organic compound having a sulfur atom, can operate the battery at a high current density when used in a nonaqueous secondary battery.

[0312] Due to the high resistance of the negative electrode protection coating from vinyl carbonate, therefore, there is a tendency that the performance in fast charging, low temperature environment is degraded and gas is produced during decomposition to cause battery expansion. Compared with other oxygen-containing / sulfur compounds, the lowest unoccupied molecular orbital (LUMO) energy level of vinyl sulfite is low, and it can be reduced and decomposed with a higher potential than vinyl carbonate to form a negative electrode protection coating, and the addition amount of vinyl carbonate can be reduced to solve the problem brought by the negative electrode protection coating from vinyl carbonate. In addition, the negative electrode protection coating from vinyl sulfite has a small resistance in a wide range of temperature regions, and further, promotes the formation of a negative electrode SEI (Solid Electrolyte Interface) with high durability for acetonitrile and its decomposition products, thereby providing a non-aqueous electrolyte and a non-aqueous secondary battery that can stably work with a high current density.

[0313] From the viewpoint of suppressing an increase in internal resistance, the total content of vinylene carbonate and vinyl sulfite in the nonaqueous electrolyte solution of the third embodiment is preferably 0.1 volume % or more and less than 15 volume % relative to the total amount of the nonaqueous solvent.

[0314] Examples of the cyclic carbonate include ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, trans-2,3-butylene carbonate, cis-2,3-butylene carbonate, 1,2-pentenyl carbonate, trans-2,3-pentenyl carbonate, cis-2,3-pentenyl carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinyl ethylene carbonate.

[0315] Examples of the fluoroethylene carbonate include 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one.

[0316] Examples of the lactone include γ-butyrolactone, α-methyl-γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone.

[0317] Examples of the organic compound having a sulfur atom include ethylene sulfite, propylene sulfite, butylene sulfite, pentenyl sulfite, sulfolane, 3-sulfolane, 3-methylsulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propylene-1,3-sultone, dimethyl sulfoxide, tetramethylene sulfoxide, and ethylene glycol sulfite.

[0318] Examples of the chain carbonate include ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, ethyl propyl carbonate, and diisobutyl carbonate.

[0319] Examples of the cyclic ether include tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and 1,3-dioxane.

[0320] Examples of the mononitriles other than acetonitrile include propionitrile, butyronitrile, valeronitrile, benzonitrile, and acrylonitrile.

[0321] Examples of the alkoxy-substituted nitrile include methoxyacetonitrile and 3-methoxypropionitrile.

[0322] Examples of the dinitriles include malononitrile, succinonitrile, glutaronitrile, adiponitrile, 1,4-dicyanoheptane, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 2,6-dicyanoheptane, 1,8-dicyanooctane, 2,7-dicyanooctane, 1,9-dicyanononane, 2,8-dicyanononane, 1,10-dicyanodecane, 1,6-dicyanodecane, and 2,4-dimethylglutaronitrile.

[0323] Examples of the cyclic nitrile include benzonitrile.

[0324] Examples of the short-chain fatty acid esters include methyl acetate, methyl propionate, methyl isobutyrate, methyl butyrate, methyl isovalerate, methyl valerate, methyl pivalate, methyl 2-methylbutyrate, methyl hexanoate, ethyl acetate, ethyl propionate, ethyl isobutyrate, ethyl butyrate, ethyl isovalerate, ethyl valerate, ethyl pivalate, ethyl 2-methylbutyrate, ethyl hexanoate, propyl acetate, propyl propionate, propyl isobutyrate, propyl butyrate, propyl isovalerate, propyl valerate, propyl pivalate, propyl 2-methylbutyrate, propyl hexanoate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, propyl valerate, propyl pivalate, propyl 2-methylbutyrate, propyl hexanoate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, isopropyl valerate, isopropyl pivalate, isopropyl 2-methylbutyrate, isopropyl hexanoate, butyl acetate, butyl propionate, butyl isobutyrate, butyl butyrate, butyl isovalerate, butyl valerate, butyl pivalate, butyl 2-methylbutyrate, butyl hexanoate, isobutyl acetate, isobutyl propionate, isobutyl isobutyrate, isobutyl butyrate, isobutyl isovalerate, isobutyl valerate, isobutyl pivalate, isobutyl 2-methylbutyrate, isobutyl hexanoate, tert-butyl acetate, tert-butyl propionate, tert-butyl isobutyrate, tert-butyl butyrate, tert-butyl isovalerate, tert-butyl valerate, tert-butyl pivalate, tert-butyl 2-methylbutyrate, and tert-butyl hexanoate.

[0325] Examples of the chain ether include dimethoxyethane, diethyl ether, 1,3-dioxolane, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), and tetraethylene glycol dimethyl ether (tetraglyme).

[0326] Examples of the fluorinated ether include Rf 20 -OR 21 (Where Rf 20 represents an alkyl group containing a fluorine atom, and R 7 represents a monovalent organic group which may contain a fluorine atom).

[0327] Examples of the ketone include acetone, methyl ethyl ketone, and methyl isobutyl ketone.

[0328] Examples of the compound in which a part or all of the H atoms of the aprotic solvent are substituted with halogen atoms include compounds in which the halogen atom is fluorine.

[0329] Here, as the fluoride of linear carbonate, for example, can enumerate methyl trifluoroethyl carbonate, dimethyl trifluorocarbonate, diethyl trifluorocarbonate, methyl ethyl trifluorocarbonate, methyl 2,2-difluoroethyl carbonate, methyl 2,2,2-trifluoroethyl carbonate, methyl 2,2,3,3-tetrafluoropropyl carbonate.Above-mentioned fluorinated linear carbonate can be represented by following general formula.

[0330] R 1 -OC(O)OR 2

[0331] {In the formula, R 1 and R 2 It is composed of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2 and CH2Rf 3 At least one selected from the group consisting of 3 is an alkyl group having 1 to 3 carbon atoms in which at least one fluorine atom replaces a hydrogen atom, and R 1 and / or R 2 Contains at least one fluorine atom.}

[0332] Examples of the fluorinated short-chain fatty acid ester include fluorinated short-chain fatty acid esters represented by 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, and 2,2,3,3-tetrafluoropropyl acetate. The fluorinated short-chain fatty acid ester can be represented by the following general formula.

[0333] R 10 -C(O)OR 11

[0334] {In the formula, R 10 It is made of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, CF3CF2H, CFH2, CF2Rf 12 CFHRf 12 and CH2Rf 13 At least one selected from the group consisting of 11 It is composed of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2 and CH2Rf 13 At least one selected from the group consisting of 12 is an alkyl group having 1 to 3 carbon atoms which may be formed by replacing a hydrogen atom with at least one fluorine atom, Rf 13 is an alkyl group having 1 to 3 carbon atoms in which at least one fluorine atom replaces a hydrogen atom, and R 10 and / or R 11 Contains at least one fluorine atom, when R 10 When it is CF2H, R 11 Not CH3.}

[0335] The aprotic solvent other than acetonitrile in the third embodiment may be used alone or in combination of two or more.

[0336] From the viewpoint that improves the stability of nonaqueous electrolyte, the nonaqueous solvent in the preferred 3rd embodiment uses more than one in cyclic carbonate and the linear carbonate and acetonitrile.From this viewpoint, the nonaqueous solvent in the 3rd embodiment more preferably uses cyclic carbonate and acetonitrile, further preferably uses cyclic carbonate and linear carbonate together with acetonitrile.

[0337] When a cyclic carbonate other than vinylene carbonate is used together with acetonitrile, it is particularly preferred that the cyclic carbonate contains ethylene carbonate and / or fluoroethylene carbonate.

[0338] <III-1-2. Electrolyte salt>

[0339] The non-aqueous electrolyte solution of the third embodiment only needs to contain LiPF6, and other electrolyte salts are not particularly limited. For example, in the third embodiment, as lithium salts, LiPF6 and lithium-containing imide salts are included.

[0340] Lithium imide salt is LiN(SO2C m F 2m+1 )2〔wherein m is an integer of 0 to 8〕, specifically, preferably including at least one of LiN(SO2F)2 and LiN(SO2CF3)2. It may include only one of these imide salts, or two of them. Alternatively, it may include imide salts other than these imide salts.

[0341] When acetonitrile is contained in the non-aqueous solvent, since the saturation concentration of the lithium imide salt relative to acetonitrile is higher than the saturation concentration of LiPF6, it is preferred to contain the lithium imide salt in a molar concentration of LiPF6≤lithium imide salt, which can inhibit the association and precipitation of lithium salt and acetonitrile under low temperature conditions. In addition, from the perspective of ion supply, it is preferred that the content of lithium imide salt is 0.5 mol or more and 3 mol or less relative to 1L of non-aqueous solvent. According to the non-aqueous electrolyte containing acetonitrile containing at least one of LiN(SO2F)2 and LiN(SO2CF3)2, the decrease in ion conductivity in a low temperature region such as -10°C or -30°C can be effectively suppressed, and excellent low temperature characteristics can be obtained. As described above, by limiting the content, the increase in resistance during high temperature heating can also be more effectively suppressed.

[0342] In addition, as a lithium salt, a fluorine-containing inorganic lithium salt other than LiPF6 may be included, for example, LiBF4, LiAsF6, Li2SiF6, LiSbF6, Li2B 12 F b H 12-b[wherein b is an integer of 0 to 3] and the like. In the third embodiment, the "inorganic lithium salt" refers to a lithium salt that does not contain carbon atoms in the anion and is soluble in acetonitrile. In addition, in the third embodiment, the "fluorine-containing inorganic lithium salt" refers to a lithium salt that does not contain carbon atoms in the anion, contains fluorine atoms in the anion and is soluble in acetonitrile. The fluorine-containing inorganic lithium salt forms a passivation film on the surface of the metal foil serving as the positive electrode collector, and is excellent in inhibiting the corrosion of the positive electrode collector. These fluorine-containing inorganic lithium salts are used alone or in combination of two or more. As the fluorine-containing inorganic lithium salt, a compound that is a complex salt of LiF and a Lewis acid is preferred, among which, if a fluorine-containing inorganic lithium salt having a phosphorus atom is used, free fluorine atoms are easily released, and therefore it is more preferred. A representative fluorine-containing inorganic lithium salt is LiPF6 that dissolves and releases PF6 anions. When a fluorine-containing inorganic lithium salt having a boron atom is used as the fluorine-containing inorganic lithium salt, it is preferred because it is easy to capture excess free acid components that may cause battery degradation. From this viewpoint, LiBF 4 is particularly preferred.

[0343] The content of the fluorine-containing inorganic lithium salt in the non-aqueous electrolyte of the third embodiment is not particularly limited, and is preferably 0.01 mol or more, more preferably 0.02 mol or more, and further preferably 0.03 mol or more relative to 1L of the non-aqueous solvent. When the content of the fluorine-containing inorganic lithium salt is within the above-mentioned range of 0.01 mol or more, the ion conductivity increases, and there is a tendency to be able to exhibit high output characteristics. In addition, relative to 1L of the non-aqueous solvent, the content of the fluorine-containing inorganic lithium salt is preferably less than 1.5 mol, more preferably less than 0.5 mol, and further preferably less than 0.1 mol. When the content of the fluorine-containing inorganic lithium salt is within the range of less than 1.5 mol, the ion conductivity increases, and there is a tendency to be able to exhibit high output characteristics and to suppress the decrease in ion conductivity associated with the increase in viscosity under low temperature conditions, and there is a tendency to be able to maintain the excellent performance of the non-aqueous electrolyte and to make the high temperature cycle characteristics and other battery characteristics of the non-aqueous secondary battery better.

[0344] The non-aqueous electrolyte solution of the third embodiment may further contain an organic lithium salt. In the third embodiment, the "organic lithium salt" refers to a lithium salt having a carbon atom in its anion and being soluble in acetonitrile.

[0345] As an organic lithium salt, an organic lithium salt having an oxalic acid group can be cited. As a specific example of an organic lithium salt having an oxalic acid group, for example, organic lithium salts represented by LiB(C2O4)2, LiBF2(C2O4), LiPF4(C2O4) and LiPF2(C2O4)2 can be cited, among which at least one lithium salt selected from the lithium salts represented by LiB(C2O4)2 and LiBF2(C2O4) is preferred. In addition, it is more preferred to use one or more of them together with a fluorine-containing inorganic lithium salt. In addition to being added to a non-aqueous electrolyte, the organic lithium salt having an oxalic acid group can also be included in the negative electrode (negative electrode active material layer).

[0346] From the viewpoint of better ensuring the effect of its use, the amount of the organic lithium salt with oxalate group added in the non-aqueous electrolyte is preferably 0.005 moles or more, more preferably 0.02 moles or more, and further preferably 0.05 moles or more, relative to the amount of 1L of the non-aqueous solvent of the non-aqueous electrolyte. However, when the amount of the above-mentioned organic lithium salt with oxalate group in the non-aqueous electrolyte is too much, it is possible to precipitate. Therefore, based on the amount of 1L of the non-aqueous solvent of the non-aqueous electrolyte, the amount of the above-mentioned organic lithium salt with oxalate group added in the non-aqueous electrolyte is preferably less than 1.0 moles, more preferably less than 0.5 moles, and further preferably less than 0.2 moles.

[0347] It is known that organic lithium salts having oxalate groups are poorly soluble in organic solvents with low polarity, especially in linear carbonates. Organic lithium salts having oxalate groups sometimes contain trace amounts of lithium oxalate, and further, when mixed as a non-aqueous electrolyte, sometimes react with trace amounts of water contained in other raw materials to produce new white precipitates of lithium oxalate. Therefore, the content of lithium oxalate in the non-aqueous electrolyte of the third embodiment is not particularly limited, and is preferably 0 to 500 ppm.

[0348] As the lithium salt in the third embodiment, in addition to the substances listed above, lithium salts commonly used in non-aqueous secondary batteries may be added as an auxiliary. Specific examples of other lithium salts include LiClO4, LiAlO4, LiAlCl4, LiB 10 Cl 10 , inorganic lithium salts containing no fluorine atoms in anions such as lithium borochloride; LiCF3SO3, LiCF3CO2, Li2C2F4(SO3)2, LiC(CF3SO2)3, LiC n F (2n+1) SO3{where n≥2}, organic lithium salts such as lower aliphatic carboxylic acid Li, tetraphenylborate Li, LiB(C3O4H2)2, etc.; LiPF5(CF3) etc. n (C p F 2p+1 )6-n [wherein n is an integer of 1 to 5, and p is an integer of 1 to 8] an organic lithium salt represented by LiBF3(CF3) or the like q (C s F 2s+1 ) 4-q [wherein q is an integer of 1 to 3 and s is an integer of 1 to 8] an organic lithium salt represented by; a lithium salt bonded to a polyvalent anion; an organic lithium salt represented by the following formula (sa), the following formula (sb) and the following formula (sc), etc.

[0349] LiC(SO2R A )(SO2R B )(SO2R C )(sa)

[0350] {In the formula, R A , R B and R C They may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms.

[0351] LiN(SO2OR D )(SO2OR E )(sb)

[0352] {In the formula, R D and R E They may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms.

[0353] LiN(SO2R F )(SO2OR G )(sc)

[0354] {In the formula, R F and R G They may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms.

[0355] One or two or more of these can be used together with the fluorine-containing inorganic lithium salt.

[0356] <III-1-3. Additives>

[0357] The nonaqueous electrolyte solution of the third embodiment may contain additives in addition to the nonaqueous solvent and electrolyte salt described above.

[0358] <Vinylene carbonate>

[0359] The non-aqueous electrolyte in the preferred third embodiment contains vinylene carbonate (VC). Vinylene carbonate undergoes reduction reaction on the surface of the negative electrode active material to form a coating, therefore, an addition amount commensurate with the mass of the negative electrode active material is required. From the viewpoint of forming a coating, relative to the total amount of the non-aqueous solvent, the vinylene carbonate concentration in the non-aqueous electrolyte is preferably more than 0.1 volume %. In addition, the addition of excessive vinylene carbonate may lead to a decrease in the viscosity of the electrolyte, a decrease in low-temperature characteristics, and the generation of excessive gas, therefore, relative to the total amount of the non-aqueous solvent, the addition amount of vinylene carbonate is preferably less than 10 volume %, preferably less than 8 volume %, more preferably less than 6 volume %. In the case of multi-stage injection in the manufacturing process of the non-aqueous secondary battery, the VC concentration is preferably within the above range in the final composition of the non-aqueous electrolyte contained in the battery.

[0360] <Vinyl sulfite>

[0361] The non-aqueous electrolyte in the third embodiment contains vinyl sulfite (ES). Vinyl sulfite decomposes at a higher potential than vinylene carbonate, and a reduction reaction occurs on the surface of the negative electrode active material to form a coating, so an amount of addition commensurate with the mass of the negative electrode active material is required. From the viewpoint of forming a coating, the ES concentration in the non-aqueous electrolyte is preferably 0.01 volume % or more relative to the total amount of the non-aqueous solvent. On the other hand, the addition of excessive vinyl sulfite is likely to result in the generation of excessive gas, impurity byproducts accompanied by excessive reduction reactions, so the ES concentration in the non-aqueous electrolyte is preferably 4 volume % or less relative to the total amount of the non-aqueous solvent. In the case of multi-stage injection in the manufacturing process of the non-aqueous secondary battery, the ES concentration is preferably within the above range in the final composition of the non-aqueous electrolyte contained in the battery.

[0362] <Inorganic sulfur compounds>

[0363] The non-aqueous secondary battery in the third embodiment can be manufactured by the following method: having at least two electrolyte injection steps of injecting a non-aqueous electrolyte into the battery outer package, having at least one charging step after the initial electrolyte injection step and before the final electrolyte injection step, and in the electrolyte injection step after the initial time, injecting an electrolyte having a higher volume ratio of acetonitrile to the total electrolyte than the electrolyte used in the initial electrolyte injection step into the battery outer package. In addition, an inorganic sulfur compound containing sulfur atoms with a valence of more than -2 and less than 0, such as sulfur and copper sulfide, is included on the negative electrode coating after the initial charge and discharge. The sulfur described here can be, for example, a solid, crystal, semi-solid, gel, liquid, vapor, or a combination thereof that is substantially composed of sulfur (S) atoms except for unavoidable impurities. In the X-ray photoelectron spectroscopy (XPS) measurement, the compound is a compound observed in the region of binding energy of 160 to 165 eV. A non-aqueous secondary battery using a non-aqueous electrolyte can function as a battery through the initial charge. It is assumed that when the acetonitrile concentration is high during the initial charge, defects are generated in the negative electrode coating. In addition to the excessive reduction and decomposition reaction of ES in the defects, it reacts with copper ions dissolved from the collector after the reduction reaction to form these compounds.

[0364] These compounds have low ion conductivity and accumulate in large quantities on the negative electrode, which may cause a decrease in output performance or a decrease in cycle life performance. Therefore, compared with the amount of the compound containing lithium (Li) atoms, the amount of the compound containing sulfur atoms with a valence of -2 or more and less than 0 in the negative electrode coating is preferably 3.80% or less, and more preferably 3.00% or less. On the other hand, from the perspective of battery stability or controlling the reduction reaction of the negative electrode, in the negative electrode coating, compared with the amount of the compound containing Li atoms, the amount of the compound containing sulfur atoms with a valence of -2 or more and less than 0 is preferably 0.1% or more. The amount of substance described here may be, for example, a value based on a molecular weight.

[0365] <Other electrode protection additives>

[0366] As other electrode protection additives, there is no particular limitation as long as it does not hinder the problem solving of the present invention, and it can be substantially repeated with the substance that acts as a solvent for dissolving lithium salts (i.e., the above-mentioned non-aqueous solvent) (wherein, acetonitrile and vinylene carbonate are excluded). The electrode protection additive is preferably a substance that helps to improve the performance of the non-aqueous electrolyte and non-aqueous secondary battery in the third embodiment, but also includes substances that do not directly participate in the electrochemical reaction.

[0367] Specific examples of other electrode protection additives include fluoroethylene carbonates represented by 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one; cyclic carbonates containing unsaturated bonds represented by 4,5-dimethylvinyl carbonate and vinyl carbonate; and γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ- The present invention also includes lactones represented by caprolactone, and ε-caprolactone; cyclic ethers represented by 1,4-dioxane; cyclic sulfur compounds represented by propylene sulfite, butylene sulfite, pentenyl sulfite, cyclopentane sulfone, 3-cyclobutene sulfone, 3-methylcyclopentane sulfone, 1,3-propane sultone, 1,4-butane sultone, 1-propylene-1,3-sultone, and tetramethylene sulfoxide; chain acid anhydrides represented by acetic anhydride, propionic anhydride, and benzoic anhydride; cyclic acid anhydrides represented by malonic anhydride, succinic anhydride, glutaric anhydride, maleic anhydride, phthalic anhydride, 1,2-cyclohexane dicarboxylic anhydride, 2,3-naphthalene dicarboxylic anhydride, or naphthalene-1,4,5,8-tetracarboxylic dianhydride; mixed acid anhydrides having a structure formed by dehydration condensation of two different carboxylic acids or different types of acids such as carboxylic acid and sulfonic acid. These can be used alone or in combination of two or more.

[0368] There is no particular limitation on the content of the electrode protection additive in the non-aqueous electrolyte in the third embodiment. The content of the electrode protection additive relative to the total amount of the non-aqueous solvent is preferably 0.1 volume % to 30 volume %, more preferably 0.3 volume % to 15 volume %, and further preferably 0.5 volume % to 4 volume %.

[0369] In the third embodiment, the more the content of the electrode protection additive is, the more the degradation of the non-aqueous electrolyte is suppressed. However, the less the content of the electrode protection additive is, the more the high output characteristics of the non-aqueous secondary battery in a low temperature environment are improved. Therefore, by adjusting the content of the electrode protection additive within the above range, there is a tendency to maximize the excellent performance based on the high ion conductivity of the non-aqueous electrolyte without damaging the basic function of the non-aqueous secondary battery. By preparing the non-aqueous electrolyte with such a composition, there is a tendency to make the cycle performance of the non-aqueous secondary battery, the high output performance in a low temperature environment and other battery characteristics all better.

[0370] <Other optional additives>

[0371] In the third embodiment, for the purpose of improving the charge and discharge cycle characteristics of the non-aqueous secondary battery, improving the high-temperature storage property, safety (for example, preventing overcharging, etc.), etc., the non-aqueous electrolyte can also appropriately contain any additive selected from, for example, sulfonates, diphenyl disulfide, cyclohexylbenzene, biphenyl, fluorobenzene, tert-butylbenzene, phosphates [ethyl diethylphosphonoacetate (EDPA): (C2H5O)2(P=O)-CH2(C=O)OC2H5; tris(trifluoroethyl) phosphate (TFEP): (CF3CH2O)3P=O; triphenyl phosphate (TPP): (C6H5O)3P=O; triallyl phosphate: (CH2=CHCH2O)3P=O, etc.], nitrogen-containing cyclic compounds having no steric hindrance around non-covalent electron pairs [pyridine, 1-methyl-1H-benzotriazole, 1-methylpyrazole, etc.], and derivatives of these compounds. In particular, phosphoric acid esters are effective in suppressing side reactions during storage.

[0372] The content of other arbitrary additives in the third embodiment is calculated by the mass percentage relative to the total mass of all components constituting the non-aqueous electrolyte. The content of other arbitrary additives is not particularly limited, and relative to the total amount of the non-aqueous electrolyte, it is preferably in the range of 0.01 mass % or more and 10 mass % or less, more preferably 0.02 mass % or more and 5 mass % or less, and further preferably 0.05 mass % or more and 3 mass % or less. By adjusting the content of other arbitrary additives to the above range, there is a tendency to be able to add better battery characteristics without damaging the basic function as a non-aqueous secondary battery.

[0373] <III-2. Positive Electrode and Positive Electrode Collector>

[0374] Figure 1 , 2 The positive electrode 150 shown is composed of a positive electrode active material layer and a positive electrode current collector, and the positive electrode active material layer is made of a positive electrode mixture. The positive electrode 150 is not particularly limited as long as it functions as a positive electrode of a non-aqueous secondary battery, and may also be a known positive electrode. The positive electrode in the third embodiment contains a lithium-containing compound containing Fe, and preferably also contains nickel (Ni) at a relatively high ratio.

[0375] The positive electrode active material layer contains a positive electrode active material, and preferably further contains a conductive auxiliary agent and a binder as necessary.

[0376] The positive electrode active material layer preferably contains a material capable of absorbing and releasing lithium ions as the positive electrode active material. When such a material is used, high voltage and high energy density tend to be obtained, which is preferred.

[0377] As the positive electrode active material, it is preferred that at least one lithium-containing compound having an olivine structure represented by the following general formula (1) be selected from at least one lithium-containing compound, or a lithium (Li)-containing metal oxide represented by the following general formula (2) containing at least one transition metal element selected from the group consisting of Ni, Mn and Co.

[0378] Li w MPO4(1)

[0379] {In the formula, M represents at least one transition metal element, and the w value is determined by the charge and discharge state of the battery and represents a number between 0 and 1.2.}

[0380] Li p Ni q Co r Mn s M t O u (2)

[0381] {Wherein, M is at least one metal selected from the group consisting of aluminum (Al), tin (Sn), indium (In), iron (Fe), vanadium (V), copper (Cu), magnesium (Mg), titanium (Ti), zinc (Zn), molybdenum (Mo), zirconium (Zr), strontium (Sr) and barium (Ba), and is in the range of 0<p<1.3, 0<q<1.2, 0<r<1.2, 0≤s<0.5, 0≤t<0.3, 0.7≤q+r+s+t≤1.2, 1.8<u<2.2, and p is a value determined by the charge and discharge state of the battery.}

[0382] The lithium-containing compound represented by the general formula (1) is preferably a metal phosphate compound containing lithium and a transition metal element. In the formula (1), the w value is preferably determined by the charge and discharge state of the battery and represents a number of 0.05 to 1.10.

[0383] Specific examples of the positive electrode active material include Li w Li compounds such as FePO4 or lithium cobalt oxides represented by LiCoO2; lithium manganese oxides represented by LiMnO2, LiMn2O4 and Li2Mn2O4; lithium nickel oxides represented by LiNiO2; 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.2 Li represented by O2 zLithium-containing composite metal oxides represented by MO2 (wherein M includes at least one transition metal element selected from the group consisting of Ni, Mn and Co, and represents two or more metal elements selected from the group consisting of Ni, Mn, Co, Al and Mg, and z represents a number greater than 0.9 and less than 1.2).

[0384] In particular, when the Ni content ratio q of the Li-containing metal oxide represented by the general formula (2) is 0.5<q<1.2, it is preferred because both the amount of Co used as a rare metal and the high energy density can be achieved. As such a positive electrode active material, for example, LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.75 Co 0.15 Mn 0.15 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.85 Co 0.075 Mn 0.075 O2、LiNi 0.8 Co 0.15 Al 0.05 O2、LiNi 0.81 Co 0.1 Al 0.09 O2、LiNi 0.85 Co 0.1 Al 0.05 Lithium-containing composite metal oxides represented by O2, etc.

[0385] On the other hand, the higher the Ni content ratio in the positive electrode active material layer, the more it tends to degrade at a low voltage. In the positive electrode active material containing Li metal oxide represented by the general formula (2), there are actually active sites that cause oxidation degradation of the non-aqueous electrolyte, but the active sites sometimes unintentionally consume the compounds added to protect the negative electrode on the positive electrode side. Among them, acid anhydrides have a tendency to be easily affected by them. In particular, in the case of containing acetonitrile as a non-aqueous solvent, the addition effect of acid anhydrides is huge, and therefore, the consumption of acid anhydrides on the positive electrode side is a fatal issue.

[0386] In addition, these additive decomposition products that enter the positive electrode side and accumulate will not only become the main cause of the increase in the internal resistance of the non-aqueous secondary battery, but also accelerate the degradation of the lithium salt. Furthermore, the protection of the negative electrode surface, which is the original purpose, becomes insufficient. In order to deactivate the active sites that substantially oxidize and degrade the non-aqueous electrolyte, it is important to coexist with components that act as a control or neutralizer for the Jahn-Teller distortion. Therefore, it is preferred that the positive electrode active material contains at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba.

[0387] For the same reason, it is preferred that the surface of the positive electrode active material is coated with a compound containing at least one metal element selected from the group consisting of Zr, Ti, Al and Nb. In addition, it is more preferred that the surface of the positive electrode active material is coated with an oxide containing at least one metal element selected from the group consisting of Zr, Ti, Al and Nb. Furthermore, since it will not hinder the permeation of lithium ions, it is particularly preferred that the surface of the positive electrode active material is coated with at least one oxide selected from the group consisting of ZrO2, TiO2, Al2O3, NbO3 and LiNbO2.

[0388] The positive electrode active material may be a lithium-containing compound other than the Li-containing metal oxide represented by the above general formula (1) and (2), and is not particularly limited as long as it contains lithium. As such a lithium-containing compound, for example, a composite oxide containing lithium and a transition metal element, a metal sulfide having lithium, and a metal silicate compound containing lithium and a transition metal element may be cited. From the viewpoint of obtaining a higher voltage, as a lithium-containing compound, in particular, a metal phosphate compound containing lithium and at least one transition metal element selected from the group consisting of Co, Ni, Mn, Fe, Cu, Zn, Cr, V and Ti is preferred.

[0389] More specifically, the lithium-containing compound includes compounds represented by the following formula (Xa) and the following formula (Xb).

[0390] Li v M I D2(Xa)

[0391] {wherein, D represents a chalcogen element, M I Represents at least one transition metal element, and the v value is determined by the charge and discharge state of the battery, and represents a number between 0.05 and 1.10.}

[0392] Li t M II uSiO4(Xb)

[0393] {In the formula, M II represents at least one transition metal element, the t value is determined by the charge and discharge state of the battery and represents a number from 0.05 to 1.10, and u represents a number from 0 to 2.}

[0394] The lithium-containing compound represented by the above formula (Xa) has a layered structure, and the compounds represented by the above formula (1) and the above formula (Xb) have an olivine structure. For the purpose of stabilizing the structure, these lithium-containing compounds can be compounds in which a part of the transition metal elements are replaced by Al, Mg or other transition metal elements, compounds in which these metal elements are contained in the grain boundaries, compounds in which a part of the oxygen atoms are replaced by fluorine atoms, compounds in which other positive electrode active materials are coated on at least a part of the surface of the positive electrode active material, etc.

[0395] As the positive electrode active material in the third embodiment, only the above-mentioned lithium-containing compound may be used, or other positive electrode active materials may be used in combination with the lithium-containing compound.

[0396] As such other positive electrode active materials, for example, metal oxides or metal chalcogenides having a tunnel structure and a layered structure; sulfur; conductive polymers, etc. As metal oxides or metal chalcogenides having a tunnel structure and a layered structure, for example, MnO2, FeO2, FeS2, V2O5, V6O 13 Oxides, sulfides, selenides, etc. of metals other than lithium represented by TiO2, TiS2, MoS2, and NbSe2. As conductive polymers, for example, conductive polymers represented by polyaniline, polythiophene, polyacetylene, and polypyrrole can be cited.

[0397] The above-mentioned other positive electrode active materials can be used alone or in combination of two or more, without particular limitation. However, since lithium ions can be reversibly and stably absorbed and released, and high energy density can be achieved, it is preferred that the positive electrode active material layer contains at least one transition metal element selected from Ni, Mn and Co.

[0398] When a lithium-containing compound and other positive electrode active materials are used together as positive electrode active materials, the ratio of the two, as well as the ratio of the lithium-containing compound to the total positive electrode active materials, is preferably 80% by mass or more, more preferably 85% by mass or more.

[0399] Examples of the conductive aid include carbon black represented by graphite, acetylene black and Ketjen black, and carbon fiber. The conductive aid content is preferably 10 parts by mass or less, more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the positive electrode active material.

[0400] Examples of the binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid, styrene butadiene rubber, and fluororubber. The binder content is preferably 10 parts by mass or less, more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the positive electrode active material.

[0401] The positive electrode mixture formed by mixing the positive active material, the conductive aid as needed and the binder is dispersed in a solvent to form a slurry containing the positive electrode mixture, the slurry containing the positive electrode mixture is applied to the positive electrode collector and dried (removing the solvent), and pressed as needed to form a positive electrode active material layer. As such solvent, it is not particularly limited, and a conventionally known solvent can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be cited.

[0402] The positive electrode current collector is composed of metal foil such as aluminum foil, nickel foil, stainless steel foil, etc. The positive electrode current collector may be carbon-coated on the surface or processed into a mesh shape. The thickness of the positive electrode current collector is preferably 5 μm to 40 μm, more preferably 7 μm to 35 μm, and further preferably 9 μm to 30 μm.

[0403] <III-3. Negative Electrode and Negative Electrode Collector>

[0404] Figure 1 , 2 The negative electrode 160 shown is composed of a negative electrode active material layer made of a negative electrode mixture and a negative electrode current collector. The negative electrode 160 can function as a negative electrode of a non-aqueous secondary battery.

[0405] The negative electrode active material layer preferably contains a negative electrode active material and, if necessary, contains a conductive aid and a binder.

[0406] As negative electrode active materials, for example, in addition to carbon materials represented by amorphous carbon (hard carbon), graphite (for example, artificial graphite, natural graphite, etc.), pyrolytic carbon, coke, glassy carbon, sintered bodies of organic polymer compounds, mesophase carbon microspheres, carbon fibers, activated carbon, carbon colloids, and carbon black, metal lithium, metal oxides, metal nitrides, lithium alloys, tin alloys, silicon alloys, intermetallic compounds, organic compounds, inorganic compounds, metal complexes, organic polymer compounds, etc. The negative electrode active materials may be used alone or in combination of two or more.

[0407] In order to increase the battery voltage, the negative electrode active material layer preferably contains a negative electrode active material capable of reacting at a ratio of 0.4 V (vs. Li / Li + ) Materials that absorb lithium ions at a lower potential.

[0408] Examples of the conductive aid include carbon black represented by graphite, acetylene black and Ketjen black, and carbon fiber. The content of the conductive aid is preferably 20 parts by mass or less, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the negative electrode active material.

[0409] Examples of the binder include carboxymethyl cellulose, PVDF, PTFE, polyacrylic acid, and fluororubber. In addition, diene rubbers such as styrene butadiene rubber may also be mentioned. The binder content is preferably 10 parts by mass or less, more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the negative electrode active material.

[0410] The negative electrode active material and the negative electrode mixture formed by mixing the conductive aid and the binder as needed are dispersed in a solvent to form a slurry containing the negative electrode mixture, and the slurry containing the negative electrode mixture is applied to the negative electrode collector and dried (removing the solvent), and pressed as needed to form a negative electrode active material layer. As such a solvent, there is no particular limitation, and a conventionally known solvent can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be cited.

[0411] The negative electrode current collector is composed of metal foil such as copper foil, nickel foil, stainless steel foil, etc. In addition, the negative electrode current collector may be carbon-coated on the surface or processed into a mesh shape. The thickness of the negative electrode current collector is preferably 5 μm to 40 μm, more preferably 6 μm to 35 μm, and further preferably 7 μm to 30 μm.

[0412] <III-4. Spacer>

[0413] like Figure 2 As shown, for the non-aqueous secondary battery 100 in the third embodiment, from the viewpoint of providing safety such as preventing a short circuit and shutdown of the positive electrode 150 and the negative electrode 160, it is preferred to have a separator 170 between the positive electrode 150 and the negative electrode 160. As the separator 170, there is no limitation, and the same separator as the separator provided in the known non-aqueous secondary battery can be used, and an insulating film with large ion permeability and excellent mechanical strength is preferred. As the separator 170, for example, woven fabrics, non-woven fabrics, synthetic resin microporous films, etc. can be cited, among which synthetic resin microporous films are preferred.

[0414] As the synthetic resin microporous membrane, for example, a polyolefin-based microporous membrane such as a microporous membrane containing polyethylene or polypropylene as the main component or a microporous membrane containing both of these polyolefins is preferably used. As the nonwoven fabric, for example, a porous membrane made of heat-resistant resins such as glass, ceramic, polyolefin, polyester, polyamide, liquid crystal polyester, and aromatic polyamide can be cited.

[0415] The spacer 170 may be a single layer or multiple layers of a microporous film, or a structure of two or more microporous films stacked together. The spacer 170 may also be a single layer or multiple layers of a mixed resin material obtained by melt-kneading two or more resin materials.

[0416] For the purpose of imparting functions, inorganic particles may be present on the surface or inside of the spacer, and other organic layers may be further coated or laminated. In addition, a cross-linked structure may also be included. In order to improve the safety performance of the non-aqueous secondary battery, these methods may be combined as needed.

[0417] By using such a separator 170 , it is possible to realize good input-output characteristics and low self-discharge characteristics required of lithium-ion batteries for high-output applications.

[0418] The thickness of the microporous film that can be used as a separator is not particularly limited. From the viewpoint of film strength, it is preferably 1 μm or more, and from the viewpoint of permeability, it is preferably 500 μm or less. From the viewpoint of high output uses such as safety tests that have high heat release and require self-discharge characteristics above the past, and from the viewpoint of windability in large battery winding machines, the thickness of the microporous film is preferably 5 μm or more and 30 μm or less, more preferably 10 μm or more and 25 μm or less. It should be noted that in the case of taking into account both short-circuit resistance and output performance, the thickness of the microporous film is further preferably 15 μm or more and 25 μm or less, and in the case of taking into account both high energy density and output performance, it is further preferably 10 μm or more and less than 15 μm.

[0419] From the viewpoint of following the rapid movement of lithium ions during high output, the porosity of the microporous film that can be used as a separator is preferably 30% or more and 90% or less, more preferably 35% or more and 80% or less, and further preferably 40% or more and 70% or less. It should be noted that, in the case of giving priority to improving output performance while ensuring safety, the porosity of the microporous film is particularly preferably 50% or more and 70% or less, and in the case of paying attention to both short-circuit resistance and output performance, it is particularly preferably 40% or more and less than 50%.

[0420] The air permeability of the microporous membrane that can be used as a separator is preferably 1 sec / 100 cm from the viewpoint of the balance between membrane thickness and porosity. 3 Above and 400 seconds / 100cm 3 Less than 100 sec / 100 cm 3 Above and 350 / 100cm 3It should be noted that, when emphasizing both short-circuit resistance and output performance, the air permeability of the microporous membrane is particularly preferably 150 sec / 100 cm 3 Above and 350 seconds / 100cm 3 Below, when giving priority to improving output performance while ensuring safety, 100 / 100cm is particularly preferred. 3 More than 1 second and less than 150 seconds / 100cm 3 . On the other hand, when a non-aqueous electrolyte with low ion conductivity is combined with a separator having an air permeability and porosity within the above range, the speed of movement of lithium ions is not limited by the structure of the separator but by the high ion conductivity of the non-aqueous electrolyte, and there is a tendency that the expected input-output characteristics cannot be obtained. Therefore, the ion conductivity of the non-aqueous electrolyte is preferably 10mS / cm or more, more preferably 15mS / cm, and further preferably 20mS / cm. However, the film thickness, air permeability and porosity of the separator and the ion conductivity of the non-aqueous electrolyte are not limited to the above examples.

[0421] <III-5. Battery packaging>

[0422] Figure 1 , 2 The structure of the battery outer package 110 of the non-aqueous secondary battery 100 shown is not particularly limited, and for example, any one of a battery can and a laminated film outer package can be used. As a battery can, for example, a square, square-shaped, cylindrical, oval, flat, coin-shaped or button-shaped metal can made of steel, stainless steel, aluminum or a cladding material can be used. As a laminated film outer package, for example, a laminated film composed of a three-layer structure of hot melt resin / metal film / resin can be used.

[0423] The laminated film outer casing can overlap two pieces with the hot melt resin side facing inward, or be bent into a state with the hot melt resin side facing inward, so that it can be used as an outer casing in a state where the ends are sealed by heat sealing. When a laminated film outer casing is used, the positive lead 130 (or the positive terminal and the lead tab connected to the positive terminal) can be connected to the positive electrode collector, and the negative lead 140 (or the negative terminal and the lead tab connected to the negative terminal) can be connected to the negative electrode collector. In this case, the laminated film outer casing can be packaged in a state where the ends of the positive lead 130 and the negative lead 140 (or the lead tabs connected to the positive terminal and the negative terminal, respectively) are led out to the outside of the outer casing.

[0424] <III-6. Method for manufacturing battery>

[0425] The nonaqueous secondary battery 100 according to the third embodiment can be manufactured using the above-mentioned nonaqueous electrolyte, a positive electrode 150 having a positive electrode active material layer on one or both sides of a current collector, a negative electrode 160 having a negative electrode active material layer on one or both sides of a current collector, a battery casing 110, and a separator 170 as required. The method for manufacturing a nonaqueous secondary battery according to the third embodiment includes at least two electrolyte injection steps (hereinafter sometimes referred to as "two-stage injection") of injecting a nonaqueous electrolyte into a battery casing, at least one charging step after the initial electrolyte injection step and before the final electrolyte injection step, and in the electrolyte injection step after the initial step, an electrolyte having a higher volume ratio of acetonitrile to the entire electrolyte than the electrolyte used in the initial electrolyte injection step can be injected.

[0426] First, a stacked body consisting of the positive electrode 150 and the negative electrode 160 and the separator 170 as required is formed. For example, the stacked body may be formed by winding the long positive electrode 150 and the negative electrode 160 in a stacked state with the long separator sandwiched between the positive electrode 150 and the negative electrode 160 to form a stacked body with a wound structure; the stacked body may be formed by cutting the positive electrode 150 and the negative electrode 160 into a plurality of sheets having a predetermined area and shape to obtain positive electrode sheets and negative electrode sheets, and alternately stacking the obtained positive electrode sheets and negative electrode sheets via separator sheets; the stacked body may be formed by bending the long separator to alternately insert positive electrode sheets and negative electrode sheets between the bent separators; etc.

[0427] Then, the above-mentioned stack is housed in a battery exterior 110 (battery case), the non-aqueous electrolyte of the third embodiment is injected into the battery case, and the stack is immersed in the non-aqueous electrolyte and sealed, thereby manufacturing the non-aqueous secondary battery of the third embodiment.

[0428] Alternatively, the non-aqueous secondary battery 100 can be manufactured by impregnating a substrate made of a polymer material with a non-aqueous electrolyte to pre-prepare a gel-state electrolyte membrane, forming a stacked structure using a sheet-like positive electrode 150, a negative electrode 160, an electrolyte membrane, and a separator 170 as required, and then housing the stacked structure in a battery casing 110.

[0429] It should be noted that when the configuration of the electrode is designed to have a portion where the peripheral end of the negative electrode active material layer overlaps with the peripheral end of the positive electrode active material layer, or when there is a portion with too small a width in the non-opposite portion of the negative electrode active material layer, the position of the electrode is offset when the battery is assembled, so that the charge and discharge cycle characteristics in the non-aqueous secondary battery may be reduced. Therefore, for the electrode body used in the non-aqueous secondary battery, it is preferred that the position of the electrode is fixed in advance with a tape such as a polyimide tape, a polyphenylene sulfide tape, a polypropylene (PP) tape, an adhesive, etc.

[0430] In the third embodiment, when a non-aqueous electrolyte using acetonitrile is used, due to its high ionic conductivity, the lithium ions released from the positive electrode during the initial charge of the non-aqueous secondary battery are likely to diffuse to the entire negative electrode. In a non-aqueous secondary battery, the area of ​​the negative electrode active material layer is usually made larger than the positive electrode active material layer. However, if the lithium ions diffuse to the position in the negative electrode active material layer that is not opposite to the positive electrode active material layer and are retained, the lithium ions will not be released during the initial discharge and will remain on the negative electrode. Therefore, the contribution of the lithium ions that have not been released becomes the irreversible capacity. For such reasons, in a non-aqueous secondary battery using a non-aqueous electrolyte containing acetonitrile, the initial charge and discharge efficiency is sometimes reduced.

[0431] On the other hand, when the area of ​​the positive electrode active material layer is larger than that of the negative electrode active material layer, or both are equal, current concentration is likely to occur at the edge of the negative electrode active material layer during charging, and lithium dendrites are likely to form.

[0432] Due to the above reasons, the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion where the positive electrode active material layer and the negative electrode active material layer are opposite is not particularly limited, but is preferably greater than 1.0 and less than 1.1, more preferably greater than 1.002 and less than 1.09, further preferably greater than 1.005 and less than 1.08, and particularly preferably greater than 1.01 and less than 1.08. In a non-aqueous secondary battery using a non-aqueous electrolyte containing acetonitrile, the initial charge and discharge efficiency can be improved by reducing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion where the positive electrode active material layer and the negative electrode active material layer are opposite.

[0433] Reducing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion of the positive electrode active material layer opposite to the negative electrode active material layer refers to limiting the ratio of the area of ​​the portion of the negative electrode active material layer that is not opposite to the positive electrode active material layer. Thus, the amount of lithium ions released from the positive electrode during the initial charge that are retained in the portion of the negative electrode active material layer that is not opposite to the positive electrode active material layer (i.e., the amount of lithium ions that are not released from the negative electrode during the initial discharge and become irreversible capacity) can be reduced as much as possible. Therefore, by designing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion of the positive electrode active material layer opposite to the negative electrode active material layer within the above range, the initial charge and discharge efficiency of the battery can be improved while achieving an improvement in the load characteristics of the battery caused by the use of acetonitrile, and further the formation of lithium dendrites can be suppressed.

[0434] The non-aqueous secondary battery 100 in the third embodiment can function as a battery through the initial charge, and a part of the non-aqueous electrolyte is decomposed and stabilized during the initial charge. There is no particular limitation on the method of the initial charge, and the initial charge is preferably performed at 0.001C to 0.3C, more preferably at 0.002C to 0.25C, and further preferably at 0.003C to 0.2C. It is also preferred that the initial charge is performed via constant voltage charging on the way. By setting the voltage range in which the lithium salt participates in the electrochemical reaction to be longer, a stable and strong SEI is formed on the surface of the electrode (negative electrode 160), which has the effect of suppressing the increase of internal resistance. In addition, the reaction product will not be firmly fixed only to the negative electrode 160, and in some form, it also gives a good effect to the components other than the negative electrode 160 such as the positive electrode 150 and the separator 170. Therefore, it is very effective to consider the electrochemical reaction of the lithium salt dissolved in the non-aqueous electrolyte for the initial charge. It should be noted that the initial discharge is not particularly limited either, but is preferably performed at 0.002C to 1.0C.

[0435] For the non-aqueous secondary battery 100 in the third embodiment, during the initial charge and aging treatment, the electrolyte can be impregnated into the separator and the electrode and the gas present in the battery cell for the purpose of removing the gas, which can be carried out under reduced pressure. From the viewpoint of electrolyte impregnation, the temperature under reduced pressure is preferably above 15°C, more preferably above 20°C, and further preferably above 25°C. As for the degree of reduced pressure, from the viewpoint of electrolyte impregnation and gas removal, the degree of reduced pressure is also preferably below 900hPa, more preferably 800hPa. It should be noted that for manufacturing under such reduced pressure conditions, usually, the volatilization of the electrolyte may become a problem, but by applying the two-stage injection in the third embodiment of the present invention, the volatilization of the electrolyte is reduced, so the manufacturing problem can also be solved.

[0436] The nonaqueous secondary battery 100 of the third embodiment can also be used as a battery pack in which a plurality of nonaqueous secondary batteries 100 are connected in series or in parallel. From the viewpoint of managing the charge and discharge state of the battery pack, the operating voltage range of each battery is preferably 2 to 5V.

[0437] In the manufacturing process of the non-aqueous secondary battery 100 in the third embodiment, there may be two or more electrolyte injection steps for injecting a non-aqueous electrolyte into the battery exterior. When there are multiple electrolyte injection steps, there is at least one charging step after the initial electrolyte injection step and before the final electrolyte injection step, and the composition of the electrolyte injected in each electrolyte injection step may be different.

[0438] From the viewpoint of forming the negative electrode coating, the electrolyte used in the initial electrolyte injection process (hereinafter, sometimes referred to as "initial electrolyte injection") preferably contains a higher concentration of VC and ES than the electrolyte used in the electrolyte injection process after the initial injection. From the same viewpoint, the initial electrolyte injection preferably contains 0.1 volume % or more of VC, more preferably contains 2 volume % or more, and further preferably contains 4 volume % or more. In addition, the initial electrolyte injection preferably contains 0.1 volume % or more of ES, more preferably contains 2 volume % or more.

[0439] From the viewpoint of reducing the volatilization of electrolyte, the electrolyte used in the electrolyte injection process after the first time preferably contains acetonitrile (AcN) with higher concentration than the first injection electrolyte, and more preferably the volume ratio of AcN relative to whole electrolytes is higher than the first injection electrolyte. From the same viewpoint, the first injection electrolyte preferably contains less than 50 volume % AcN, more preferably contains less than 35 volume %, and further preferably contains less than 20 volume %. In addition, from the viewpoint of improving the ionic conductivity of electrolyte, the electrolyte used in the electrolyte injection process after the first time preferably contains more than 20 volume % AcN, more preferably contains more than 35 volume %, and further preferably contains more than 50 volume %. In addition, the electrolyte used in the electrolyte injection process after the first time, for example, can contain less than 100 volume % AcN.

[0440] Although the third embodiment of the present invention has been described above, the present invention is not limited to the above embodiment and can be modified in various ways without departing from the gist of the present invention.

[0441] Example

[0442] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.

[0443] <Examples, Comparative Examples, and Reference Examples of the First Embodiment>

[0444] (1) Preparation of non-aqueous electrolyte

[0445] Various non-aqueous solvents and various additives are mixed in an inactive environment to achieve a predetermined concentration, and various lithium salts are added to achieve a predetermined volume molar concentration (M), thereby preparing non-aqueous electrolytes (1-S1) to (1-S20). The abbreviations of the non-aqueous solvents, lithium salts, and additives in Table 1-1 have the following meanings.

[0446] (Lithium Salt)

[0447] LiFSI: lithium bis(fluorosulfonyl)imide. LiPF6: lithium hexafluorophosphate.

[0448] (Non-aqueous solvent)

[0449] AcN: acetonitrile.

[0450] EMC: Ethyl methyl carbonate.

[0451] EC: Ethylene carbonate.

[0452] ES: Ethylene sulfite.

[0453] Table 1-1

[0454] Electrolyte No. Li salt Electrolyte composition (volume ratio) 1-S1 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 35AcN / 41EMC / 20EC / 4ES 1-S2 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 20AcN / 56EMC / 20EC / 4ES 1-S3 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 5AcN / 71EMC / 20EC / 4ES 1-S4 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 47AcN / 29.2EMC / 20EC / 3.8ES 1-S5 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 60AcN / 16.2EMC / 20EC / 3.8ES 1-S6 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 10AcN / 66EMC / 20EC / 4ES 1-S7 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 8AcN / 68.2EMC / 20EC / 3.8ES 1-S8 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 16AcN / 64EMC / 20EC 1-S9 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 16AcN / 61.9EMC / 19.4EC / 2.7ES 1-S10 <![CDATA[LiFSI 0.6M+LiPF6 0.7M]]> 17AcN / 59EMC / 20EC / 4ES 1-S11 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 20AcN / 57EMC / 20EC / 3ES 1-S12 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 20AcN / 56.2EMC / 20EC / 3.8ES 1-S13 <![CDATA[LiFSI 0.6M+LiPF6 0.7M]]> 25AcN / 51EMC / 20EC / 4ES 1-S14 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 29AcN / 47EMC / 20EC / 4ES 1-S15 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 30AcN / 50EMC / 20EC 1-S16 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 30AcN / 48.1EMC / 19.2EC / 2.7ES 1-S17 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 35AcN / 41.2EMC / 20EC / 3.8ES 1-S18 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 42AcN / 34.2EMC / 20EC / 3.8ES 1-S19 <![CDATA[LiFSI 1M+LiPF6 0.3M]]> 45AcN / 35EMC / 20EC 1-S20 <![CDATA[LiPF6 1.1M]]> 80EMC / 20EC

[0455] (2) Fabrication of non-aqueous secondary batteries

[0456] (2-1) Preparation of positive electrode

[0457] (A) LiFePO4 as a positive electrode active material, (B) acetylene black powder as a conductive aid, and (C) polyvinylidene fluoride (PVDF) and / or carbon nanotubes (CNT) as a binder are mixed in a specific mass ratio shown in Table 1-2 to obtain a positive electrode mixture.

[0458] N-methyl-2-pyrrolidone as a solvent was added to the obtained positive electrode mixture, and the mixture was further mixed to prepare a slurry containing the positive electrode mixture. The slurry containing the positive electrode mixture was coated on one or both sides of a 15 μm thick aluminum foil as a positive electrode collector while adjusting the unit area weight, and the solvent was dried and removed in a hot air drying furnace. Then, the positive electrode active material layer was rolled by a roller press to a density of 1.9 g / cm 3 , a positive electrode (1-C1 to C3) consisting of a positive electrode active material layer and a positive electrode current collector corresponding to the positive electrode mixture composition of 1-C1 to C3 in Table 2 is obtained. In addition, while adjusting the unit area weight of the slurry containing the positive electrode mixture, it is applied to one or both sides of the aluminum foil as the positive electrode current collector foil, and the solvent is dried and removed in a hot air drying furnace. Then, it is rolled with a roller press so that the density of the positive electrode active material layer becomes 2.2 g / cm 3 , thereby obtaining a positive electrode (1-C4, 1-C5) consisting of a positive electrode active material layer and a positive electrode collector corresponding to the positive electrode mixture composition of 1-C4, 1-C5 in Table 1-2. In addition, a lead is welded to positive electrodes 1-C3 to C5. Then, vacuum drying is performed at 120°C for more than 12 hours to obtain a positive electrode. The unit area weight of each positive electrode except the positive electrode collector is shown in Table 1-2.

[0459] (2-2) Preparation of negative electrode

[0460] As (a) a negative electrode active material, graphite, (b) a conductive aid, and (c) a binder were mixed in the mass ratio shown in Table 1-2 to obtain a negative electrode mixture.

[0461] Water as a solvent was added to the obtained negative electrode mixture, and the mixture was further mixed to prepare a slurry containing the negative electrode mixture. The mixture was applied to one or both sides of a copper foil with a thickness of 10 μm as a negative electrode current collector, and the solvent was dried and removed in a hot air drying furnace. Then, the negative electrode active material layer was rolled using a roller press so that the density of the negative electrode active material layer became 1.4 g / cm 3 , a negative electrode (1-A1 to A3) consisting of a negative electrode active material layer and a negative electrode current collector is obtained. In addition, the slurry containing the negative electrode mixture is applied to one or both sides of a copper foil with a thickness of 10 μm as the negative electrode current collector, and the solvent is dried and removed in a hot air drying furnace. Then, the negative electrode active material layer is rolled with a roller press to a density of 1.6 g / cm 3 , a negative electrode (1-A4, 1-A5) consisting of a negative electrode active material layer and a negative electrode current collector corresponding to the negative electrode mixture of 1-A4, 1-A5 in Table 1-2 is obtained. In addition, a lead is welded to the negative electrodes 1-A3 to A5. Then, vacuum drying is performed at 80°C for more than 12 hours to obtain a negative electrode. The unit area weight of the negative electrode active material layer is shown in Table 1-2.

[0462] In the following Table 1-2, among the types of binders, PVDF is polyethylene vinylidene fluoride, CMC is carboxymethyl cellulose, and SBR is styrene butadiene rubber.

[0463] Table 1-2

[0464]

[0465] (2-3) Assembly of non-aqueous secondary battery (coin type)

[0466] In a nitrogen glove box with a dew point temperature of -60 to -20°C, a polypropylene gasket was placed in a CR2032 battery box (SUS304 / Al cladding), and an object obtained by punching the positive electrode (1-C1, 1-C2) obtained as described above into a disc-shaped object with a diameter of 15.958 mm was placed in the center so that the positive electrode active material layer was facing upward. An object obtained by punching a glass fiber filter paper (GA-100 made by ADVANTEC CO., LTD.) into a disc-shaped object with a diameter of 16.156 mm was placed thereon, and the amount of non-aqueous electrolyte was set to 150 μL, and the weight of the non-aqueous electrolyte was calculated according to the specific gravity of the non-aqueous electrolyte. An object obtained by punching the negative electrode (1-A1, 1-A2) obtained as described above into a disc-shaped object with a diameter of 16.156 mm was placed so that the negative electrode active material layer was facing downward, forming a laminate consisting of an electrode and a separator. Furthermore, after setting the spacer and the spring, the battery cover is embedded. Rivet with a riveting machine. Maintain at 25°C for 12 hours to fully fuse the non-aqueous electrolyte and the laminate, thereby obtaining a coin-type non-aqueous secondary battery (hereinafter, also referred to as a "coin-type battery"). Here, the battery composed of electrodes 1-C1 and 1-A1 is coin 1, and the battery composed of 1-C2 and 1-A2 is coin 2. The design capacity of coin 1 is 3.0 mAh, and the design capacity of coin 2 is 6.0 mAh.

[0467] (2-4) Assembly of non-aqueous secondary battery (laminated type)

[0468] The cut positive electrode with lead (1-C3) and the negative electrode with lead (1-A3) were stacked via a polyethylene microporous film separator (thickness 20 μm) in a dry room with a dew point temperature of -80°C to -20°C to form a laminate, and the laminate was housed in an aluminum laminate sheet outer casing. Then, the outer casing was sealed with a non-aqueous electrolyte solution contained in the outer casing. Figure 1 The appearance shown is produced Figure 2The laminated non-aqueous secondary battery with the cross-sectional structure shown. Maintain at 25°C for 48 hours to allow the non-aqueous electrolyte to fully fuse with the laminate, thereby obtaining a laminated sheet type (bag type) non-aqueous secondary battery (hereinafter, also referred to as a "laminated battery"). Here, the area of ​​the electrode, the number of laminated sheets, the area of ​​the laminated sheet, and the amount of non-aqueous electrolyte are changed according to the designed capacity of the battery. In a 30mAh single-layer battery cell (hereinafter, referred to as laminate 1), the positive electrode is set to 30mm square, the negative electrode is set to 32mm square, the laminated sheet is set to 55mm×70mm, and the electrolyte is set to 0.522g. In addition, in a 1Ah wound battery cell (hereinafter referred to as lamination 2), the positive electrode is set to 56mm wide × 378mm long and 56mm wide × 304mm long, and the negative electrode is set to 58mm wide × 401mm long and 58mm wide × 342mm long, and they are alternately stacked and wound in a manner of clamping a separator. In addition, the laminate sheet is set to 60mm × 75mm, and the electrolyte is set to 7.0g. In addition, in a 5Ah stacked battery cell (hereinafter referred to as lamination 3), 6 double-sided coated positive electrodes 94mm wide × 174mm long and 7 double-sided coated negative electrodes 100mm wide × 180mm long are alternately stacked in a manner of clamping a separator, the laminate sheet is set to 150mm × 220mm, and the electrolyte is set to 18.5~21.0g. In addition, Figure 1 , Figure 2 This is the general appearance of the laminated battery. Laminates 1 to 3 do not necessarily have the same appearance.

[0469] The cut positive electrode with lead (1-C4) and the negative electrode with lead (1-A4) were stacked with six positive electrodes and six negative electrodes via a polyethylene microporous film separator (thickness 12 μm) in a dry room with a dew point temperature of -80°C to -20°C to form a laminate, and the laminate was placed in an aluminum laminate sheet outer casing. Then, the outer casing was sealed in a state where a non-aqueous electrolyte was contained in a predetermined amount in the outer casing, so as to Figure 1 The appearance shown is produced Figure 2 A laminated non-aqueous secondary battery having the cross-sectional structure shown. Maintain at 25°C for 12 hours to allow the non-aqueous electrolyte to fully fuse with the laminate, thereby obtaining a laminated sheet-type (bag-type) non-aqueous secondary battery (hereinafter referred to as laminate A). Here, the amount of the non-aqueous electrolyte is set to 0.22g, 0.44g or 0.50g. In addition, in a dry room with a dew point temperature of -80°C to -20°C, the cut positive electrode with a lead (1-C5) and the negative electrode with a lead (1-A5) are overlapped with 8 positive electrodes and negative electrodes via a polyethylene microporous film separator (thickness 12μm) to form a laminate, and the laminate is housed in an aluminum laminate sheet outer casing. Then, the outer casing is sealed in a state where a specified amount of the non-aqueous electrolyte is contained in the outer casing, so as to Figure 1 The appearance shown is produced Figure 2The laminated non-aqueous secondary battery having the cross-sectional structure shown in FIG. was kept at 25° C. for 12 hours to allow the non-aqueous electrolyte to fully fuse with the laminate, thereby obtaining a laminated sheet type non-aqueous secondary battery (hereinafter referred to as laminate B). Here, the amount of the non-aqueous electrolyte was set to 0.84 g or 0.90 g.

[0470] (3) Evaluation of non-aqueous secondary batteries

[0471] For the coin-type batteries and laminated batteries obtained as described above, first, the initial charging treatment and the initial charge and discharge capacity were measured according to the following steps (3-1). Then, each coin-type battery and laminated battery were evaluated according to the steps (3-2). It should be noted that the charging and discharging of the coin-type battery was carried out using the charging and discharging device ACD-M01A (trade name) manufactured by ASKAElectronic Co., Ltd. and the program thermostatic bath IN804 (trade name) manufactured by Yamato Science Co., Ltd., and the charging and discharging of the laminated battery was carried out using TOSCAT-300 (trade name) manufactured by Toyo Systems Co., Ltd. and LU-123 (trade name) or BTS-408C (trade name) manufactured by ESPEC.

[0472] In the first embodiment, 1C refers to a current value at which a fully charged battery is discharged at a constant current and the discharge is expected to be completed in 1 hour. In addition, when a non-aqueous secondary battery is simply referred to, both the above-mentioned coin-type battery and laminated battery are included.

[0473] (3-1a) Initial charge and discharge treatment of non-aqueous secondary batteries (coin-type batteries and laminated batteries 1 to 3)

[0474] The ambient temperature of the non-aqueous secondary battery was set to 25°C, and the coin-type battery was charged at a constant current equivalent to 0.1C, and the laminated batteries 1 to 3 were charged at a constant current equivalent to 0.025C until the battery voltage reached 3.5V. Then, the constant voltage charging was continued for 2 hours while the current was decayed while the battery voltage was maintained at 3.5V, or the constant voltage charging was continued until the charge capacity reached 90% of the designed capacity. After charging, the coin-type battery was rested for 10 minutes, and the laminated battery was rested for 20 minutes, and then discharged at a constant current of 0.1C to 2.0V.

[0475] (3-2a) Fine charge and discharge processing (coin-type battery and laminated battery 1 to 3)

[0476] After treatment (3-1a), the ambient temperature of the non-aqueous secondary battery is set to 25°C and charged to 3.5V at a constant current of 0.2C. Then, the constant voltage charging is continued for 2 hours while the current is decayed while the voltage is maintained at 3.5V, or the constant voltage charging is continued until the current value decays to 0.05C. After charging, the coin-type battery takes a 10-minute rest time, and the laminated batteries 1 to 3 take a 20-minute rest time. Then, discharge is performed at a constant current of 0.2C until 2.0V. The ratio of the discharge capacity to the charge capacity in this operation is calculated as the capacity efficiency (%) of charge and discharge. In addition, the irreversible rate (%) of the charge and discharge capacity is also calculated by subtracting the capacity efficiency of the charge and discharge from 100.

[0477] (3-1b) Initial charge and discharge treatment of non-aqueous secondary batteries (laminated batteries A and B)

[0478] The ambient temperature of the prepared non-aqueous secondary battery was set to 25°C, and the laminated batteries A and B were charged at a constant current equivalent to 0.025C until the battery voltage reached 3.6V. Then, constant voltage charging was continued while maintaining the battery voltage at 3.6V until the current decayed to 0.02C. After charging, a rest time of 20 minutes was taken, and then, discharge was performed at a constant current of 0.1C until 2.0V.

[0479] (3-2b) Fine charge and discharge treatment (laminated batteries A and B)

[0480] After treatment (3-1b), the ambient temperature of the non-aqueous secondary battery is set to 25°C and charged to 3.6V at a constant current of 0.2C. Then, while maintaining the voltage at 3.6V, the constant voltage charging is continued for 2 hours while the current is decayed, or the constant voltage charging is continued until the current value decays to 0.05C. After charging, a 20-minute rest time is taken. Then, the battery is discharged at a constant current of 0.2C until 2.0V. The ratio of the discharge capacity to the charge capacity in this operation is calculated as the capacity efficiency (%) of charge and discharge. In addition, the irreversible rate (%) of the charge and discharge capacity is also calculated by subtracting the capacity efficiency from 100.

[0481] (3-3a) Charge and discharge cycle test of non-aqueous secondary batteries (coin-type batteries and laminated batteries 1 to 3)

[0482] The ambient temperature of the prepared non-aqueous secondary batteries (coin-type batteries 1, 2, laminated batteries 1 to 3) was set to 50°C, and the batteries were charged at a constant current equivalent to 1C until the battery voltage reached 3.5V. Then, constant voltage charging was continued while maintaining the battery voltage at 3.5V until the current decayed to 0.05C. After charging, a 10-minute rest time was taken, and then the batteries were discharged at a constant current of 1C until 2.0V. The above charging and discharging operations were repeated 50 times. In addition, the ratio of the discharge capacity to the charging capacity in each charging and discharging operation was calculated, the average value of 50 times was calculated, and the cycle average capacity efficiency was calculated. The cycle average irreversibility rate (%) was calculated by subtracting the cycle average capacity efficiency from 100.

[0483] (3-3b) Charge and discharge cycle test of non-aqueous secondary batteries (laminated batteries A and B)

[0484] The ambient temperature of the prepared non-aqueous secondary batteries (laminated batteries A and B) was set to 50°C, and they were charged at a constant current equivalent to 1C until the battery voltage reached 3.6V. Then, constant voltage charging was continued while maintaining the battery voltage at 3.6V until the current decayed to 0.05C. After charging, a 10-minute rest time was taken, and then the battery was discharged at a constant current of 1C until it reached 2.0V. The above charging and discharging operations were repeated 50 times. In addition, the ratio of the discharge capacity to the charging capacity in each charging and discharging operation was calculated, the average value of 50 times was calculated, and the cycle average capacity efficiency was calculated, and the cycle average irreversibility rate (%) was calculated by subtracting the cycle average capacity efficiency from 100.

[0485] (3-4) Output test of non-aqueous secondary battery (laminated battery A)

[0486] For the battery with an electrolyte amount of 0.5g in the laminated battery A, the ambient temperature is set to 25°C and charged at a constant current equivalent to 0.3C until the battery voltage reaches 3.6V. Then, constant voltage charging is continued while maintaining the battery voltage at 3.6V until the current decays to 0.05C. After charging, a 10-minute rest time is taken, and then the battery is discharged at a constant current of 0.3C until 2.0V. The discharge current is set to 2C, and the same charge and discharge operation is performed again. Calculate the ratio of the discharge capacity in 0.3C discharge to the discharge capacity in 2C discharge, and calculate the output performance (2C capacity / 0.3C capacity).

[0487] (3-5) Non-aqueous secondary batteries

[0488] [Examples 1-1 to 1-42 and Comparative Examples 1-1 to 1-5]

[0489] To each non-aqueous electrolyte prepared as shown in Table 1-1, vinylene carbonate (VC) and sulfate ions (SO4) in the amounts shown in Table 1-3 or Table 1-4 were added. 2- ), sulfite ion (SO3 2- ), assemble the non-aqueous secondary battery as described above and perform the initial charge and discharge treatment and the fine charge and discharge, and calculate the charge and discharge efficiency and the irreversible rate of the charge and discharge capacity in the fine charge and discharge. Here, the liquid ratio X (mass %) is the ratio of the mass of the non-aqueous electrolyte to the mass of the negative electrode excluding the negative electrode collector, and A (volume %) is the content of acetonitrile relative to the volume of the non-aqueous solvent. The interpretation of each test result is explained.

[0490]

[0491]

[0492] Preferably, the capacity efficiency of the capacity efficiency in the above-mentioned fine charge and discharge is higher than 97.5%, and as the irreversible capacity rate, it is lower than 2.5%. In Examples 1-1 to 1-42, the irreversible rate of capacity is lower than 2.5%, and the stabilizing effect of the performance brought by the additive is observed. On the other hand, in Comparative Examples 1-1 to 1-5, irreversible reactions inevitably occur during charging, and the capacity efficiency is significantly low, or the irreversible capacity is higher than 2.5%, or significant poor charging is caused, resulting in inability to discharge. It can be seen from this that by adding vinylene carbonate and sulfate ions or sulfite ions to the non-aqueous electrolyte so that they are within the specified range, the battery tends to be stably driven.

[0493] The cycle average irreversibility rate is preferably 0.19% or less, and more preferably 0.17% or less. As in Examples 1-37 to 1-42, in batteries where X is 200% or less, within the prescribed range where the content of acetonitrile is 35% by volume or less and the amount of vinylene carbonate added is 15×A / X or more, a tendency of the irreversibility rate being less than 0.19% is observed. It can be considered that in these batteries, the effect of forming a negative electrode coating is improved, and the battery is also stably driven for a long time under a high temperature environment.

[0494] [Examples 1-43 to 54 and Reference Example 1-1]

[0495] To each non-aqueous electrolyte prepared as shown in Table 1-5, vinylene carbonate (VC) and sulfate ions (SO4) in the amounts shown in Table 1-5 were added. 2-), after assembling the non-aqueous secondary battery as described above and performing the initial charge and discharge treatment and the fine charge and discharge, the output test of the laminated battery A was carried out according to the steps described in (3-4) above. In addition, a cycle test was carried out separately according to the steps shown in (3-3). Here, the liquid content ratio X (mass %) is the ratio of the mass of the non-aqueous electrolyte contained in the battery to the mass of the negative electrode excluding the negative electrode collector. In this output test, the amount of electrolyte is made the same in each electrolyte, and X=98. In addition, A (volume %) is the content of acetonitrile relative to the volume of the non-aqueous solvent. The following is an explanation of the test results of the output test and the cycle test.

[0496]

[0497] Examples 1-43 to 54 contain a specified amount of vinylene carbonate, and the capacity efficiency in the cycle test is 0.19% or less. In addition, it is more preferably 0.17% or less, and in batteries containing vinyl sulfite or sulfate ions, there is a tendency to show better capacity efficiency. On the other hand, the ratio of 2C capacity / 0.3C capacity representing output performance is preferably 83% or more, more preferably 84% or more. The more acetonitrile content there is, the higher the 2C capacity / 0.3C capacity tends to be, and both cycle performance and output performance can be taken into account. In addition, it can be seen that when an electrolyte not containing acetonitrile is used as Reference Example 1-1, the long-term stability of the capacity efficiency and the output performance cannot be taken into account.

[0498] (4-1) Preparation of nickel-containing electrodes and non-aqueous secondary batteries

[0499] The composite oxide of lithium, nickel, manganese and cobalt (LiNi 0.8 Mn 0.1 Co 0.1 O2), carbon black powder as a conductive aid, and polyvinylidene fluoride (PVDF) as a binder were mixed in a mass ratio of 94:3:3 to obtain a positive electrode mixture. N-methyl-2-pyrrolidone as a solvent was added to the obtained positive electrode mixture and further mixed to prepare a slurry containing the positive electrode mixture. The slurry containing the positive electrode mixture was mixed with a unit area weight of 8.4 mg / cm 2 or 16.6 mg / cm 2 The positive electrode active material layer was coated on one side of a 20 μm thick aluminum foil as a positive electrode current collector in a manner of adjustment, and the solvent was dried and removed. Then, the positive electrode active material layer was rolled using a roll press so that the density of the positive electrode active material layer became 2.91 g / cm 3 , a positive electrode (1-C6, 1-C7) consisting of a positive electrode active material layer and a positive electrode current collector was obtained. However, the unit area weight of 1-C6 was 8.4 mg / cm 2 , the unit area weight of 1-C7 is 16.6 mg / cm2 .

[0500] Following the manufacturing steps of the aforementioned coin-type battery, a battery (coin 4) was manufactured by combining the positive electrode 1-C6 and the negative electrode 1-A1, and a battery (coin 5) was manufactured by combining the positive electrode 1-C7 and the negative electrode 1-A2.

[0501] (4-2) Initial charge and discharge treatment of non-aqueous secondary batteries containing nickel electrodes

[0502] The small non-aqueous secondary battery was set to an ambient temperature of 25°C, and charged at a constant current equivalent to 0.025C to 3.1V, and then charged at a constant voltage of 3.1V for 1.5 hours. After a 3-hour pause, the battery was charged at a constant current equivalent to 0.05C to 4.2V, and then charged at a constant voltage of 4.2V for 1.5 hours. Then, the battery was discharged to 3.0V at a constant current equivalent to 0.15C.

[0503] (4-3) Fine charge and discharge treatment

[0504] After treatment (4-1), the ambient temperature of the non-aqueous secondary battery is set to 25°C and charged to 4.2V at a constant current of 0.2C. Then, the constant voltage charging is continued for 2 hours while maintaining the voltage at 4.2V, or the constant voltage charging is continued until the current value decays to 0.05C. A 10-minute rest time is taken after charging. Then, the battery is discharged to 3.0V at a constant current of 0.2C. The ratio of the discharge capacity to the charge capacity in this operation is calculated as the capacity efficiency (%) of charge and discharge. In addition, the irreversible rate (%) of the charge and discharge capacity is also calculated by subtracting the charge and discharge efficiency from 100.

[0505] (4-4) Non-aqueous Secondary Batteries

[0506] [Examples 1-55 to 57]

[0507] To each electrolyte prepared in Table 1-1, add the amount of vinylene carbonate and sulfate ion shown in Table 1-6, assemble the non-aqueous secondary battery as described above, perform the initial charge and discharge treatment and the fine charge and discharge, and calculate the charge and discharge efficiency and the irreversible rate of the charge and discharge capacity in the fine charge and discharge. Here, the liquid ratio X (mass %) is the ratio of the mass of the non-aqueous electrolyte to the mass of the negative electrode excluding the negative electrode collector, and A (volume %) is the content of acetonitrile relative to the volume of the non-aqueous solvent.

[0508]

[0509] When nickel is contained in the positive electrode, the capacity efficiency is preferably 97.0% or more, and more preferably 97.3% or more. In addition, the irreversible capacity rate of the capacity is preferably 3% or less, and more preferably 2.7% or less. In Examples 1-55 to 1-57, the irreversible capacity rate is 2.7% or less, confirming the stable driving of the battery.

[0510] <Examples and Comparative Examples of Second Embodiment>

[0511] (Examples 2-1 to 2-3 and Comparative Examples 2-1 and 2-2)

[0512] Examples 2-1 to 2-3 and Comparative Examples 2-1 and 2-2 are described below.

[0513] [Production of positive electrode]

[0514] LiFePO4 as a positive electrode active material, acetylene black powder as a conductive aid, carbon nanotubes, and polyvinylidene fluoride (PVDF) as a binder were mixed in a mass ratio of 94:2:1:3 to obtain a positive electrode mixture. N-methyl-2-pyrrolidone as a solvent was added to the obtained positive electrode mixture, and the mixture was further mixed to prepare a slurry containing the positive electrode mixture. The slurry containing the positive electrode mixture was mixed with a unit area weight of about 9.9 mg / cm 2 The positive electrode active material layer was coated on one side of a 15 μm thick aluminum foil as a positive electrode current collector in a manner of adjusting the thickness of the positive electrode active material layer. When the slurry containing the positive electrode mixture was coated on the aluminum foil, a portion of the aluminum foil was exposed to form an uncoated area. Then, the positive electrode active material layer was rolled using a roller press to a density of 2.2 g / cm 3 , a positive electrode consisting of a positive electrode active material layer and a positive electrode collector is obtained.

[0515] Then, the positive electrode was cut so that the area of ​​the positive electrode mixture layer was 30 mm×50 mm and included the exposed portion of the aluminum foil. Then, an aluminum lead piece for extracting current was welded to the exposed portion of the aluminum foil and vacuum dried at 120° C. for 12 hours to obtain a positive electrode with a lead.

[0516] [Production of negative electrode]

[0517] Graphite as a negative electrode active material, carboxymethyl cellulose as a binder, and styrene butadiene rubber latex as a binder were mixed at a mass ratio of 100:1.1:1.5 to obtain a negative electrode mixture. An appropriate amount of water was added to the obtained negative electrode mixture and mixed thoroughly to prepare a slurry containing the negative electrode mixture. The slurry was mixed with a unit area weight of about 5.1 mg / cm 2The negative electrode active material layer was coated on one side of a copper foil having a thickness of 10 μm in a predetermined thickness while being adjusted in a manner. When the slurry containing the negative electrode mixture was coated on the copper foil, an uncoated area was formed in such a manner that a portion of the copper foil was exposed. Then, the negative electrode active material layer was rolled using a roller press so that the density of the negative electrode active material layer became 1.60 g / cm 3 , thereby obtaining a negative electrode consisting of a negative electrode active material layer and a negative electrode collector.

[0518] Then, the negative electrode was cut so that the area of ​​the negative electrode mixture layer was 32 mm×52 mm and included the exposed portion of the copper foil. Then, a nickel lead for extracting current was welded to the exposed portion of the copper foil and vacuum dried at 80° C. for 12 hours to obtain a negative electrode with a lead.

[0519] 〔Battery Manufacturing〕

[0520] [Assembly of single-layer laminated batteries]

[0521] The positive electrode with a lead and the negative electrode with a lead are overlapped via a polyethylene microporous film separator (film thickness 12 μm) in a manner that the mixture coating surface of each pole is opposite to each other to produce a stacked electrode body. The stacked electrode body is housed in a 90 mm × 80 mm aluminum laminate outer body and vacuum dried at 80 ° C for 5 hours to remove moisture. Then, after 0.4 g of each electrolyte shown in Table 2-1 is injected into the outer body, the outer body is encapsulated to produce a single-layer laminated (bag-type) non-aqueous secondary battery (hereinafter, also referred to as "single-layer laminated battery" or "single-layer laminated").

[0522] The nonaqueous electrolyte solution was obtained by mixing the materials in an argon glove box at a dew point temperature of -110° C. to -70° C. In Table 2-1, the abbreviations of the materials of the nonaqueous electrolyte solution injected into the secondary battery before the initial charge have the following meanings.

[0523] LiFSI: lithium bis(fluorosulfonyl)imide.

[0524] AcN: acetonitrile.

[0525] EC: Ethylene carbonate.

[0526] VC: vinylene carbonate.

[0527] ES: Ethylene sulfite.

[0528] EMC: Ethyl methyl carbonate.

[0529] Table 2-1 Non-aqueous electrolyte composition ratio (mass %)

[0530] Electrolyte LiFSI <![CDATA[LiPF6]]> AHr EC VC ES EMC 2-S1 16.2 3.8 20.9 21.9 2 4.5 31.4 2-S2 16.1 3.8 20.9 22 4.5 4.6 28.8 2-S3 14.5 3.5 12.1 20.5 3.9 4.2 41.3 2-S4 15.5 0 0 26.4 1.6 0 56.5 2-S5 16.2 3.8 20.8 22 0.7 4.6 31.9

[0531] [Evaluation of single-layer laminated batteries]

[0532] First, the evaluation battery obtained as described above was subjected to the initial charging treatment according to the following step (1-1). Then, each battery was evaluated according to the following step (1-2) and the analysis of the negative electrode protective film components. It should be noted that the charging and discharging was performed using a charging and discharging device ACD-01 (trade name) manufactured by ASKA Electronic Co., Ltd. and a thermostatic bath PLM-63S (trade name) manufactured by Futaba Science Co., Ltd.

[0533] In the second embodiment, 1C refers to a current value at which a fully charged battery is discharged at a constant current and the discharge is expected to be completed in 1 hour.

[0534] (1-1) Initial charge and discharge treatment of single-layer laminated batteries

[0535] The battery was set at an ambient temperature of 25°C, and charged to 3.6V at a constant current of 2.1mA (0.1C), then charged at a constant voltage of 3.6V until the charge capacity reached 1.8mAh. Then, the battery was discharged to 2V at a constant current of 2.1mA (0.1C).

[0536] (1-2) Room temperature cycling of single-layer laminated batteries

[0537] For the battery that has been initially charged and discharged by the method described in (1-1) above, the ambient temperature of the battery is set to 25°C, and after charging to 3.6V at a constant current of 23mA equivalent to 1C, it is charged at a constant voltage of 3.6V until the charging current decays to 0.05C. Then, it is discharged to 2V at a constant current of 21mA. This process of charging and discharging once each is considered as a cycle, and 100 cycles of charging and discharging are performed. The rate of change of capacity when the increase in discharge capacity ends and the capacity reaches the specified value is calculated based on the initial discharge capacity of the test.

[0538] (Examples 2-4, 2-5)

[0539] Embodiment 2-4 and embodiment 2-5 are described below.

[0540] [Production of positive electrode]

[0541] LiFePO4 as a positive electrode active material, acetylene black powder as a conductive aid, and polyvinylidene fluoride (PVDF) as a binder were mixed in a mass ratio of 87:8:5 to obtain a positive electrode mixture. N-methyl-2-pyrrolidone as a solvent was added to the obtained positive electrode mixture, and further mixed to prepare a slurry containing the positive electrode mixture. The slurry containing the positive electrode mixture was mixed with a unit area weight of about 20.7 mg / cm 2The positive electrode active material layer was coated on one side of a 15 μm thick aluminum foil as a positive electrode current collector in a manner of adjusting the thickness of the positive electrode active material layer. When the slurry containing the positive electrode mixture was coated on the aluminum foil, a portion of the aluminum foil was exposed to form an uncoated area. Then, the positive electrode active material layer was rolled using a roller press to a density of 1.9 g / cm 3 , thereby obtaining a positive electrode consisting of a positive electrode active material layer and a positive electrode collector.

[0542] Then, the positive electrode was cut so that the area of ​​the positive electrode mixture layer was 29 mm×56 mm and included the exposed portion of the aluminum foil. Then, an aluminum lead piece for extracting current was welded to the exposed portion of the aluminum foil and vacuum dried at 120° C. for 12 hours to obtain a positive electrode with a lead.

[0543] [Production of negative electrode]

[0544] Graphite as a negative electrode active material, carboxymethyl cellulose as a binder, and styrene butadiene rubber latex as a binder were mixed at a mass ratio of 100:1.1:1.5 to obtain a negative electrode mixture. An appropriate amount of water was added to the obtained negative electrode mixture and mixed thoroughly to prepare a slurry containing the negative electrode mixture. The slurry was mixed with a unit area weight of about 8.8 mg / m 2 The negative electrode active material layer was coated on one side of a copper foil having a thickness of 10 μm in a predetermined thickness while being adjusted in a manner. When the slurry containing the negative electrode mixture was coated on the copper foil, an uncoated area was formed in such a manner that a portion of the copper foil was exposed. Then, the negative electrode active material layer was rolled using a roller press so that the density of the negative electrode active material layer became 1.60 g / cm 3 , thereby obtaining a negative electrode consisting of a negative electrode active material layer and a negative electrode collector.

[0545] Then, the negative electrode was cut so that the area of ​​the negative electrode mixture layer was 31 mm×58 mm and included the exposed portion of the copper foil. Then, a nickel lead for extracting current was welded to the exposed portion of the copper foil and vacuum dried at 80° C. for 12 hours to obtain a negative electrode with a lead.

[0546] [Assembly of laminated batteries]

[0547] The positive electrode with a lead and the negative electrode with a lead are overlapped via a polyethylene microporous film separator (film thickness 20 μm) in a manner that the mixture coating surfaces of each pole are opposite to each other to produce a stacked electrode body. The stacked electrode body is housed in a 90 mm × 80 mm aluminum laminate outer body and vacuum dried at 80 ° C for 5 hours to remove moisture. Then, after 5.6 g of the electrolyte 2-S2 and 2-S3 shown in Table 2-1 above are respectively injected into the outer body, the outer body is encapsulated to produce a stacked laminated (bag type) non-aqueous secondary battery (hereinafter, also referred to as "stacked laminated battery" or "stacked laminated").

[0548] [Evaluation of laminated batteries]

[0549] First, the evaluation battery obtained as described above was subjected to the initial charging treatment according to the following step (1-1). Then, each battery was evaluated according to the following step (1-2) and the analysis of the negative electrode protective film components. It should be noted that the charging and discharging was performed using a charging and discharging device ACD-01 (trade name) manufactured by ASKA Electronic Co., Ltd. and a thermostatic bath PLM-63S (trade name) manufactured by Futaba Science Co., Ltd.

[0550] Here, 1C, as described in the above-mentioned [Evaluation of Single-Layer Laminated Batteries], refers to a current value at which a fully charged battery is discharged at a constant current and the discharge is expected to be completed in 1 hour.

[0551] (1-1) Initial charge and discharge treatment of laminated batteries

[0552] The battery was set at an ambient temperature of 25°C, charged at a constant current of 23 mA (0.025C) to 3.5 V, then charged at a constant voltage of 3.5 V until the charge capacity reached 800 mAh, and then discharged at a constant current of 91 mA (0.1C) to 2 V.

[0553] (1-2) Room temperature cycling of laminated batteries

[0554] The ambient temperature of the battery was set to 25°C, and after charging to 3.5V at a constant current of 182mA equivalent to 1C, it was charged at a constant voltage of 3.5V until the current decayed to 0.05C. Then, it was discharged to 2V at a constant current of 182mA equivalent to 1C. After performing this operation 10 times, stabilization of the discharge capacity was observed until this moment. The rate of change of capacity when the increase of the discharge capacity ended and the capacity reached the specified value was calculated based on the discharge capacity at the beginning of the test.

[0555] [Analysis of negative electrode protective film components]

[0556] Since the negative electrode protective coating of the example of the second embodiment is poorly soluble in non-aqueous electrolyte, its solubility in organic solvents is also low. Therefore, heavy water is used to extract the negative electrode protective coating. In addition, as an analysis method for the components of the negative electrode protective coating, the compound represented by the general formula (a) is measured using IC, and the compound represented by the general formula (b) to (d) is measured using NMR. The molar mass of each compound is (a) 25.94g / mol, (b) 161.95g / mol, (c) 96.01g / mol and (d) 81.98g / mol, respectively, and the molar ratio of each compound relative to the total content of (a) to (d) is calculated.

[0557] (Extraction of negative electrode coating components)

[0558] Under an argon environment, take out the negative electrode of a single-layer laminated battery or a stacked laminated battery after the above test, cut a 3 mm square negative electrode sheet (including the collector), put it into a glass threaded tube, inject 1.5 mL of heavy water with a syringe, and seal it with a cap. After standing for 72 hours to extract the electrode coating, use a Pasteur pipette filled with glass wool to filter the cotton plug to obtain an extract.

[0559] (IC determination)

[0560] The extract was diluted 1000 times with distilled water, and 30 μL of the dilution was injected into the column for IC measurement. The measuring device used was IC-2010 manufactured by TOSOH CORPORATION, the column used was TSKgel-Super IC-AZ manufactured by TOSOH CORPORATION, the column temperature was 40°C, and the flow rate was 0.8 mL / min.

[0561] (NMR measurement)

[0562] The obtained extract was placed in a 3 mm diameter NMR tube and sealed. In addition, tetrafluorobenzene (manufactured by Tokyo Chemical Industry Co., Ltd.) as a standard substance was dissolved in deuterated chloroform (manufactured by Sigma-Aldrich) containing tetramethylsilane as a chemical shift standard and placed in a 5 mm diameter NMR tube. The above 3 mm diameter NMR tube was inserted into the NMR tube and the double tube method was used for the measurement. 1 H NMR measurement. In addition, a heavy aqueous solution of dimethyl sulfoxide (concentration 0.398 mg / mL) was prepared as a quantitative standard substance and the same measurement was performed. 1 H NMR determination.

[0563] The measuring device used was a JNM-ECS-400 FT NMR device manufactured by JEOL Resonance Inc. Deuterated chloroform was used as the lock solvent, the cumulative number was 256 times, and tetramethylsilane (0 ppm) was used as the chemical shift standard. For quantitative calculation, the integral value of the peak attributed to the proton of tetrafluorobenzene was set to 2000, and the integral value equivalent to one proton per unit concentration was obtained from the integral value of the signal of dimethyl sulfoxide as the reference substance, and this value was used to calculate from the integral value of each peak.

[0564] [Analysis of non-aqueous electrolyte components]

[0565] In an argon environment, an incision is made in the laminated outer package of the single-layer laminated battery or the laminated laminated battery after the test, and a non-aqueous electrolyte is collected from the inside with a syringe, placed in an NMR tube with a diameter of 3 mm, and diluted with dimethoxyethane. In addition, tetrafluorobenzene (manufactured by Tokyo Chemical Industry Co., Ltd.) as a standard substance is dissolved in deuterated chloroform (manufactured by Sigma-Aldrich) containing tetramethylsilane as a chemical shift standard, and placed in an NMR tube with a diameter of 5 mm. The above-mentioned NMR tube with a diameter of 3 mm is inserted into the NMR tube, and the double tube method is used for the measurement. 1 H NMR measurement. In addition, a heavy aqueous solution of dimethyl sulfoxide (concentration 0.398 mg / mL) was prepared as a quantitative standard substance and the same measurement was performed. 1 H NMR measurement: The weight ratio of each component was calculated from the integrated value of the signal of each component standardized with the standard substance.

[0566] The following is an evaluation result of each example of the second embodiment. Table 2-2 records the ratio of the initial discharge capacity to the design capacity in the cycle test of the single-layer laminated battery. Here, when calculating the design capacity, if 170 mAh of capacity is theoretically taken out per 1 g of positive electrode active material, namely lithium iron phosphate, according to the active material ratio in the positive electrode (94%) and the coating area (15 cm 2 ), the design capacity of the single-layer laminated battery was calculated to be 23.7 mAh. In addition, the results of calculating the rate of change of capacity when the increase of discharge capacity was completed and the capacity reached the specified value based on the initial discharge capacity of the test were recorded.

[0567] Table 2-2

[0568]

[0569] In a secondary battery containing acetonitrile in a non-aqueous electrolyte and having a coating component with a prescribed composition ratio after the test, in the initial discharge, a capacity of more than 77% relative to the designed capacity is obtained, and in addition, the rate of change of the capacity until the discharge capacity stabilizes to a prescribed value is small, limited to less than 2.1%. On the other hand, in Comparative Example 2-1, which does not contain acetonitrile and in which (c) and (d) are greater than 20 mol%, only a capacity of less than 73% relative to the designed capacity is obtained, and the rate of change of the capacity until the discharge capacity stabilizes to a prescribed value is 5.6%, and the capacity is unstable. In addition, in Comparative Example 2-2, in which no vinylene carbonate is left in the battery when SEI is formed, the initial charge and discharge cannot be performed. In this way, after the coating is formed, the prescribed vinylene carbonate is also left in the battery, thereby having a tendency to form a good coating relative to the electrolyte containing acetonitrile and the capacity of the battery is rapidly stabilized.

[0570] Table 2-3 below shows the ratio of the initial discharge capacity to the design capacity in the cycle test of the stacked laminated battery. Here, when calculating the design capacity, if 170 mAh of capacity is theoretically taken out per 1 g of positive electrode active material, namely lithium iron phosphate, then according to the active material ratio in the positive electrode (87%) and the coating area (16.24 cm 2 ) and the number of electrode stacks (24), the design capacity of the stacked laminated battery was calculated to be 1193 mAh. In addition, the results of calculating the rate of change of capacity when the increase of discharge capacity ends and the capacity reaches the specified value based on the initial discharge capacity of the test are recorded.

[0571] Table 2-3

[0572]

[0573] In Examples 2-4 and 2-5, a predetermined coating was formed to obtain a capacity of 75% or more of the designed capacity, and the rate of change until the capacity stabilized was 1.1% or less, which was sufficiently small, and relatively fast capacity stabilization was observed.

[0574] <Example III and Comparative Example III of the Third Embodiment>

[0575] (1) Preparation of non-aqueous electrolyte

[0576] In an inactive environment, various non-aqueous solvents and various additives are mixed in a manner of respectively prescribed concentrations, and further, various lithium salts are added in a manner of respectively prescribed concentrations to prepare non-aqueous electrolytes (3-S1) to (3-S14). The abbreviations of the non-aqueous solvents, lithium salts, and additives in Table 3-1 have the following meanings.

[0577] (Lithium Salt)

[0578] LiFSI: lithium bis(fluorosulfonyl)imide.

[0579] LiPF6: lithium hexafluorophosphate.

[0580] (Non-aqueous solvents or additives).

[0581] AcN: acetonitrile.

[0582] EMC: Ethyl methyl carbonate.

[0583] EC: Ethylene carbonate.

[0584] ES: Ethylene sulfite.

[0585] VC: vinylene carbonate.

[0586] Table 3-1

[0587]

[0588] (2) Fabrication of non-aqueous secondary batteries

[0589] (2-1) Preparation of positive electrode

[0590] LiNi as the positive electrode active material (A) 0.5 Co 0.2 Mn 0.3 O2 (NCM523) or LiFePO4 (LFP), carbon black powder as (B) a conductive aid, and polyvinylidene fluoride (PVDF) as (C) a binder are mixed in a specific mass ratio shown in Table 3-2 to obtain a positive electrode mixture.

[0591] N-methyl-2-pyrrolidone as a solvent was added to the obtained positive electrode mixture, and the mixture was further mixed to prepare a slurry containing the positive electrode mixture. The slurry containing the positive electrode mixture was coated on one or both sides of a 15 μm thick aluminum foil as a positive electrode collector while adjusting the unit area weight, and the solvent was dried and removed in a hot air drying furnace. Then, the positive electrode active material layer was rolled by a roller press to a density of 1.9 g / cm 3 , thereby obtaining a positive electrode (3-C1, 3-C2) consisting of a positive electrode active material layer and a positive electrode collector. Then, vacuum drying was performed at 80°C for more than 12 hours to obtain a positive electrode. The unit area weight excluding the positive electrode collector is shown in Table 3-2.

[0592] (2-2) Preparation of negative electrode

[0593] (a) Graphite as a negative electrode active material, (b) a conductive aid (carbon black), and (c) a binder were mixed in the mass ratio shown in Table 2 to obtain a negative electrode mixture.

[0594] Water as a solvent was added to the obtained negative electrode mixture, and the mixture was further mixed to prepare a slurry containing the negative electrode mixture. The slurry was applied to one or both sides of a copper foil with a thickness of 10 μm as a negative electrode current collector, and the solvent was dried and removed in a hot air drying furnace. Then, the negative electrode active material layer was rolled using a roller press so that the density of the negative electrode active material layer became 1.4 g / cm 3 , a negative electrode (3-A1) consisting of a negative electrode active material layer and a negative electrode current collector was obtained. Then, vacuum drying was performed at 80° C. for more than 12 hours to obtain a negative electrode. The unit area weight of the negative electrode active material layer is shown in Table 3-2.

[0595] Table 3-2

[0596]

[0597] (2-3) Preparation of spacer

[0598] <Preparation of polypropylene resin composition>

[0599] Ultra-high molecular weight polypropylene resin (PP, MFR = 0.25) and ethylene / 1-butene copolymer (C2 / C4: density = 0.893 g / cm 2 , melting point = 80°C, MFR = 6.7) were dry-blended at a mass ratio of PP: C2 / C4 = 50:50 (mass %), and then melt-kneaded using ZSK40 (manufactured by Coperion, L / D = 46). In order to suppress the decomposition and modification of the resin as much as possible, the area from the resin feeding hopper port to the raw material tank is completely sealed and nitrogen is continuously introduced from the lower part of the hopper to control the oxygen concentration near the raw material feeding port to be below 50 ppm. In addition, the exhaust section is completely sealed to eliminate the air leakage into the barrel. Due to the effect of reducing the oxygen concentration, the decomposition and modification of the polymer are significantly suppressed under high temperature conditions, and further, the ethylene / 1-butene copolymer can be finely dispersed. After melt-kneading, the strands are pulled out from the die (8 holes) and the molten kneaded product is cooled in a water cooling bath, and then cut using a pelletizer to obtain pellets.

[0600] <Production of microporous membrane (single layer)>

[0601] Ultrahigh molecular weight polypropylene resin (PP, MFR = 0.25) and the above pellets were dry-blended at a mass ratio of PP: pellets = 90:10 (mass %), melted using a 2.5-inch extruder, and supplied to an annular die using a gear pump. Thus, the feed ratio of the resins fed was PP: C2 / C4 = 95:5 (mass %).

[0602] The temperature of the mold was set to 230°C, and the molten polymer was cooled by blowing air and then wound on a roll. The extruded precursor (roll film) had a thickness of 15 μm, and then the roll film was annealed at 130°C for 15 minutes. Then, the annealed film was cold stretched to 21% at room temperature, then hot stretched to 156% at 120°C, and relaxed to 126% at 125°C, thereby forming a spacer (F1) having a structure of a microporous film. After the above stretching and opening, the physical properties of the microporous film were measured.

[0603] (2-4) Assembly of small non-aqueous secondary batteries

[0604] The positive electrode (3-C1) obtained as described above was punched into a disk with a diameter of 15.958 mm and the negative electrode (3-A1) obtained as described above was punched into a disk with a diameter of 16.156 mm. The separator (F1) obtained as described above (aperture ratio 8.1, film thickness 25 μm, air permeability resistance 217 sec / 100 cm) was superimposed. 3 , porosity 55%) on both sides to obtain a laminate. The laminate was inserted into a disc-shaped battery box made of SUS. Then, a prescribed amount of non-aqueous electrolyte was injected into the battery box, and after the laminate was immersed in the non-aqueous electrolyte, the battery box was sealed to fully fuse the non-aqueous electrolyte and the laminate, thereby obtaining a small non-aqueous secondary battery (3-C1 / F1 / 3-A1).

[0605] Following the same steps, 3-C2 was used as the positive electrode, 3-A1 was used as the negative electrode, and the separator F1 (aperture ratio 8.1, film thickness 25 μm, air permeability resistance 217 sec / 100 cm) was obtained. 3 and a porosity of 55%).

[0606] (3) Evaluation of small non-aqueous secondary batteries

[0607] First, the small non-aqueous secondary battery obtained as described above was subjected to initial charging treatment and initial charge-discharge capacity measurement according to the following step (3-1). Then, each small non-aqueous secondary battery was evaluated according to the step (3-2). It should be noted that charging and discharging were performed using a charge-discharge device ACD-M01A (trade name) manufactured by ASKA Electronic Co., Ltd. and a program thermostatic bath IN804 (trade name) manufactured by Yamato Scientific Co., Ltd.

[0608] In the third embodiment, 1C refers to a current value at which a fully charged battery is discharged at a constant current and the discharge is expected to be completed in 1 hour.

[0609] Specifically, in the small non-aqueous secondary battery (3-C1 / F1 / 3-A1), 1C refers to the current value when the battery is discharged from a fully charged state of 4.2V to 2.5V at a constant current and the discharge is expected to be completed in 1 hour. In the small non-aqueous secondary battery (3-C2 / F1 / 3-A1), 1C refers to the current value when the battery is discharged from a fully charged state of 3.6V to 2.0V at a constant current and the discharge is expected to be completed in 1 hour.

[0610] The small non-aqueous secondary battery (3-C1 / F1 / 3-A1, 3-C2 / F1 / 3-A1) assembled according to the above steps (2-4) is a 3mAh-class battery cell, and the battery voltage in the fully charged state is set to 4.2V and 3.6V, which is equivalent to a current value of 3mA at 1C. Hereinafter, unless otherwise specified, the textual description of the current value and voltage will be omitted for convenience.

[0611] (3-1) Initial charge and discharge treatment of small non-aqueous secondary batteries

[0612] The ambient temperature of the small non-aqueous secondary battery (3-C1 / F1 / 3-A1 or 3-C2 / F1 / 3-A1) is set to 25°C, and after charging at a constant current equivalent to 0.1C to reach a fully charged state, charging is performed at a constant voltage for 1.5 hours. The initial efficiency is calculated by dividing the discharge capacity during charge and discharge at 0.1C by the charge capacity. For batteries with an initial efficiency of less than 80%, it is difficult to obtain a correct evaluation result because the specified battery capacity is not met, and therefore, subsequent evaluation tests cannot be carried out.

[0613] (3-2) Two-stage electrolyte injection process for small non-aqueous secondary batteries

[0614] For the battery cell that was initially charged and discharged using the method (3-1) above, the battery box was opened in an argon (Ar) box, and the electrolyte was added using a pipette. After the battery was fully charged at a constant current equivalent to 1C, two discharge steps were performed at a constant current equivalent to 1C. The composition and volume of the initial injection electrolyte and the second-stage injection electrolyte in each battery cell are shown in Table 3-3.

[0615] Table 3-3

[0616]

[0617] (3-3) Output test of small non-aqueous secondary batteries (3-C1 / F1 / 3-A1)

[0618] The small non-aqueous secondary battery (3-C1 / F1 / 3-A1) that was subjected to the initial charge and discharge treatment and two-stage injection by the methods described in (3-1) and (3-2) above was charged at a constant current of 1C to 4.2V with the ambient temperature set to 25°C, and then charged at a constant voltage of 4.2V until the current value decayed to 0.025C. Then, it was discharged at 0.1C to 2.8V.

[0619] Then, after charging at a constant current of 1 C to 4.2 V, the battery was charged at a constant voltage of 4.2 V until the current value decayed to 0.025 C. Then, the battery was discharged at 0.5 C to 2.8 V.

[0620] Then, after charging at a constant current of 1 C to 4.2 V, the battery was charged at a constant voltage of 4.2 V until the current value decayed to 0.025 C. Then, the battery was discharged at 1.0 C to 2.8 V.

[0621] Then, after charging at a constant current of 1 C to 4.2 V, the battery was charged at a constant voltage of 4.2 V until the current value decayed to 0.025 C. Then, the battery was discharged at 5.0 C to 2.8 V.

[0622] Then, after charging at a constant current of 1 C to 4.2 V, the battery was charged at a constant voltage of 4.2 V until the current value decayed to 0.025 C. Then, the battery was discharged at 10 C to 2.8 V.

[0623] Then, after charging at a constant current of 1 C to 3.5 V, the battery was charged at a constant voltage of 3.5 V until the current value decayed to 0.025 C. Then, the battery was discharged at 20 C to 2.0 V.

[0624] Then, after charging at a constant current of 1 C to 4.2 V, the battery was charged at a constant voltage of 4.2 V until the current value decayed to 0.025 C. Then, the battery was discharged at 0.1 C to 2.8 V.

[0625] The discharge capacity under each discharge rate condition was recorded.

[0626] (3-4) Cycle test of small non-aqueous secondary batteries (3-C2 / F1 / 3-A1)

[0627] The small non-aqueous secondary battery (3-C2 / F1 / 3-A1) that had been subjected to the initial charge and discharge treatment and two-stage injection by the methods described in (3-1) and (3-2) above was charged at a constant current of 1C to 3.5V with the ambient temperature set to 25°C, and then charged at a constant voltage of 3.5V until the current value decayed to 0.025C. Then, it was discharged at 0.1C to 2.7V.

[0628] For the small non-aqueous secondary battery (3-C2 / F1 / 3-A1) that has been injected in two stages by the method described in (3-2) above, the ambient temperature is set to 25°C. First, the battery is charged to 4.2V at a constant current of 3mA, which is equivalent to 1C, and then charged at a constant voltage of 4.2V until the current decays to 0.025C. Then, the battery is discharged to 2.7V at a constant current of 3mA. This process of charging and discharging once each is regarded as a cycle, and 100 cycles of charging and discharging are performed. The discharge capacity of the 100th cycle when the discharge capacity of the first cycle is set to 100% is used as the capacity retention rate of the 25°C cycle test. Similarly, the capacity retention rate of the 50th cycle is also obtained.

[0629] (4) XPS analysis of negative electrode coating

[0630] For the non-aqueous secondary battery adjusted and tested as described above, the negative electrode coating of the small non-aqueous secondary battery subjected to two cycles of charge and discharge after two-stage injection as described above (3-2) was analyzed. The battery was disassembled in an atmospheric non-exposed environment, and after the negative electrode was taken out, it was immersed in EMC for 5 minutes to remove the electrolyte, and then vacuum dried at room temperature to obtain a sample. The obtained sample was maintained in a sample holding component under an inactive environment, and XPS measurement was performed. The ratio of the relative element concentration (Sred / Li) of the compound containing sulfur atoms with a valence of greater than -2 and less than 0 and the Li compound generated by the reduction of ES contained in the negative electrode coating was determined. The XPS measurement was performed using Versa ProbeII manufactured by Ulvac-Phi, and the measurement conditions are as follows.

[0631] [Measurement conditions]

[0632] Excitation source: mono.AlKα 20kV×5mA 100W.

[0633] Analysis size: 100 μmφ×1.4 mm, 100 μmφ X-ray beam vibrates with 1.4 mm width.

[0634] Photoelectron extraction angle: 45°.

[0635] The entry areas are as follows.

[0636] Full spectrum scan: 0~1100eV.

[0637] Narrow area scanning: C 1s, O 1s, Li 1s, S2p, F 1s, N 1s, Cu 2p3 / 2.

[0638] The general function is as follows.

[0639] Full spectrum scan: 117.4eV.

[0640] Narrow area scan: 46.95eV.

[0641] The method of deriving the relative element concentrations of sulfur atoms and Li compounds having a valence of -2 or more and 0 or less is as follows.

[0642] [Derivation of relative element concentrations]

[0643] Use the following formula to find it.

[0644] Mathematical formula 1

[0645] Cj(%)=100×(I j / RSF j ) / ∑(I j / RSF j )

[0646] The parameters are as follows.

[0647] C j : Relative element concentration (atomic %).

[0648] j: C, O, Li, S, F, N, P, Cu, Cl.

[0649] I j : Area intensity of Li 1s and S2p spectra.

[0650] (Unit: cps·eV)

[0651] RSF j : Corrected relative sensitivity coefficients of Li 1s and S2p.

[0652] (Li 1s: 1.284, S2p: 37.634)

[0653] Furthermore, regarding the S concentration, Sred, which is a reduced sulfur component, was quantified by curve fitting processing of the S2p spectrum.

[0654] Sred:162~164eV.

[0655] The discreteness between the above components is good, and the valleys between the peaks can be observed. The purpose of this curve fitting process is to quantify the above components separately. Therefore, the curve fitting is performed without setting restrictions between the components.

[0656] [Examples 3-1 to 3-2, Comparative Example 3-1]

[0657] Here, the composition of the negative electrode coating of the small non-aqueous secondary battery (3-C1 / F1 / 3-A1) and the output test results are described. The small non-aqueous secondary battery (3-C1 / F1 / 3-A1) was produced according to the method described in (2) above. Then, the adjustment and negative electrode coating and output performance of each small non-aqueous secondary battery (3-C1 / F1 / 3-A1) were evaluated according to the steps (3) and (4) above. The test results are shown in Table 3-4.

[0658] Table 3-4

[0659]

[0660] As shown in Table 3-4, according to Examples 3-1 and 3-2, it is characterized in that the ratio (Sred / Li) of the compound containing sulfur atoms with a valence of -2 or more and 0 or less in the negative electrode coating after the two-stage injection is 0.1% or more and 3.80% or less, and it is confirmed that the smaller the value of Sred / Li, the higher the discharge capacity can be obtained under high rate conditions. On the other hand, in the battery cell (Comparative Example 3-1) where the two-stage injection was not performed, it was confirmed that the value of Sred / Li was greater than 3.80%, and the discharge capacity also became low.

[0661] Through two-stage injection, the first injection is carried out with an electrolyte having a lower acetonitrile concentration than the electrolyte composition after the second-stage injection for charging and discharging, and then a high concentration of acetonitrile is added, thereby ensuring high ion conductivity and suppressing excessive reductive decomposition of the electrolyte on the negative electrode surface. As a result, it can be considered that good output performance is obtained.

[0662] [Examples 3-3 to 6, Comparative Examples 3-2 to 4]

[0663] Here, the test results of the small non-aqueous secondary battery (3-C2 / F1 / 3-A1) are described. The small non-aqueous secondary battery (3-C2 / F1 / 3-A1) was produced according to the method described in (2) above. Then, the adjustment, negative electrode coating, and cycle performance of each small non-aqueous secondary battery (3-C2 / F1 / 3-A1) were evaluated according to the steps (3) and (4) above. The test results are shown in Table 3-5.

[0664] Table 3-5

[0665]

[0666] As shown in Table 3-5, except for the battery cells to which the two-stage injection was applied, where the Sred / Li value was less than 3.80%, no tendency was observed in the battery cells to which only the initial injection was performed (Comparative Examples 3-2 to 3-4) that the Sred / Li value decreased even when the VC amount was increased. On the other hand, in the battery cells to which the two-stage injection was applied, a tendency was observed that the Sred / Li value decreased as the VC increased.

[0667] It was confirmed that in battery cells that only underwent initial injection, low initial charge and discharge efficiency of less than 40% and a decrease in capacity retention during the cycle were observed. In contrast, by applying two-stage injection, a battery with high charge and discharge stability can be obtained even if the final electrolyte composition is the same.

[0668] In addition, in the two-stage injection method, when the VC amount is the same, it is confirmed that the lower the acetonitrile concentration of the first injected electrolyte is, the higher the cycle performance tends to be.

[0669] It is considered that by reducing the acetonitrile concentration of the initially injected electrolyte, it is possible to suppress excessive reductive decomposition of the electrolyte on the negative electrode surface during initial charge, thereby making the negative electrode coating uniform and suppressing degradation.

[0670] According to the non-aqueous lithium ion secondary battery containing acetonitrile injected in the second stage of the third embodiment of the present invention, in addition to suppressing the excessive reduction and decomposition of the electrolyte on the negative electrode surface, a small amount of negative electrode additives can also strengthen the negative electrode SEI, thereby obtaining good output performance and cycle performance. Therefore, in a non-aqueous secondary battery using an acetonitrile electrolyte, in a state where the initial charge is implemented, if the composition of the negative electrode coating as described above is present, the manufacturing process of the non-aqueous electrolyte having the third embodiment can be inferred.

[0671] Industrial Applicability

[0672] The nonaqueous electrolyte and nonaqueous secondary battery of the present invention are expected to be used not only in automotive batteries such as hybrid vehicles, plug-in hybrid vehicles, and electric vehicles, but also in industrial batteries such as power tools, drones, and electric bicycles, and even in residential power storage systems.

[0673] Description of Reference Numerals

[0674] 100: Non-aqueous secondary battery.

[0675] 110: Battery exterior.

[0676] 120: Space for external battery installation.

[0677] 130: Positive electrode lead body.

[0678] 140; Negative electrode lead body.

[0679] 150: Positive electrode.

[0680] 160: Negative pole.

[0681] 170: Spacer.

Claims

1. A non-aqueous electrolyte for a non-aqueous lithium ion secondary battery, the non-aqueous lithium ion secondary battery comprising a negative electrode comprising graphite and containing X mass % of the non-aqueous electrolyte relative to the mass of the negative electrode excluding the negative electrode current collector, wherein: X is greater than 50 and less than 2000, The non-aqueous electrolyte contains a lithium salt and a non-aqueous solvent. The non-aqueous solvent contains A volume % of acetonitrile relative to the volume of the non-aqueous solvent. A is 5 or more and 70 or less, and The non-aqueous electrolyte solution contains VC as an additive, wherein the VC is vinylene carbonate, and the content of the VC is greater than or equal to (7×A / X) mass % and less than or equal to 10 mass % relative to the non-aqueous electrolyte solution.

2. The non-aqueous electrolyte according to claim 1, wherein The X is 200 or less.

3. The non-aqueous electrolyte according to claim 1 or 2, wherein The A is greater than or equal to 16 and less than or equal to 35.

4. The non-aqueous electrolyte according to claim 1 or 2, wherein The content of the VC is greater than or equal to (15×A / X) mass % and less than or equal to 9 mass % relative to the non-aqueous electrolyte solution.

5. The non-aqueous electrolyte according to claim 4, wherein The X is 98 or less.

6. The non-aqueous electrolyte according to claim 1 or 2, wherein The non-aqueous electrolyte contains vinyl sulfite.

7. The non-aqueous electrolyte according to claim 1 or 2, wherein The nonaqueous electrolyte contains at least one of sulfate ions and sulfite ions.

8. The non-aqueous electrolyte according to claim 1 or 2, wherein The content of the VC is 7% by mass or less based on the non-aqueous electrolyte solution.

9. The non-aqueous electrolyte according to claim 1 or 2, wherein The X is 65 or more.

10. A non-aqueous lithium-ion secondary battery, wherein: The nonaqueous lithium ion secondary battery comprises: a positive electrode having a positive electrode active material layer on one or both sides of a positive electrode collector; a negative electrode having a negative electrode active material layer containing the graphite on one or both sides of the negative electrode collector; a separator; and the nonaqueous electrolyte according to claim 1.

11. A non-aqueous secondary battery comprising a negative electrode, a positive electrode, a separator and a non-aqueous electrolyte, wherein: The non-aqueous secondary battery is charged once. The negative electrode comprises one or more inorganic lithium compounds and one or more organic lithium compounds that can be extracted by immersion in an extraction solvent. The non-aqueous electrolyte solution contains a lithium salt, acetonitrile as a non-aqueous solvent, and a cyclic carbonate.

12. The nonaqueous secondary battery according to claim 11, wherein The nonaqueous secondary battery comprises a component that can be extracted from the negative electrode by using water as the extraction solvent, and comprises at least the following inorganic lithium compound (a) and the following organic lithium compounds (b) to (d), respectively. (a) LiF; (b) LiOCOOCH2CH2OCOOLi; (c) CH3CH2OCOOLi; (d) CH3OCOOLi, Furthermore, the molar ratios of (a) to (d) relative to the total content of (a) to (d) are: (a) is 20 mol% to 70 mol%, (b) is 20 mol% to 70 mol%, (c) is 1 mol% to 20 mol%, and (d) is 1 mol% to 20 mol%.

13. The nonaqueous secondary battery according to claim 11 or 12, wherein: The cyclic carbonate includes ethylene carbonate and vinylene carbonate, and the molar ratio of vinylene carbonate to ethylene carbonate is 0.01 mol % to 30 mol %.

14. The nonaqueous secondary battery according to claim 11 or 12, wherein: The positive electrode active material of the positive electrode includes lithium iron phosphate.

15. The non-aqueous secondary battery according to claim 11, wherein The nonaqueous secondary battery uses the nonaqueous electrolyte solution according to claim 1.

16. A secondary battery manufacturing process, wherein: The secondary battery manufacturing process has at least two electrolyte injection steps of injecting a non-aqueous electrolyte into the battery casing, and at least one charging step after the initial electrolyte injection step and before the final electrolyte injection step. In the electrolyte injection step after the initial one, an electrolyte having a higher volume ratio of acetonitrile to the total electrolyte than the electrolyte used in the initial electrolyte injection step is injected into the battery casing.

17. The secondary battery manufacturing process according to claim 16, wherein: In the electrolyte injection step after the first injection, an electrolyte containing 20 volume % or more and 100 volume % or less of acetonitrile is injected into the battery exterior.

18. A non-aqueous secondary battery, wherein: The non-aqueous secondary battery is a non-aqueous secondary battery comprising a non-aqueous electrolyte containing 5% by volume or more and 60% by volume or less of acetonitrile and vinyl sulfite, a positive electrode having a positive electrode active material layer on one or both sides of a positive electrode collector, a negative electrode having a negative electrode active material layer on one or both sides of a negative electrode collector, and a separator, and the non-aqueous secondary battery is a non-aqueous secondary battery in which a compound containing sulfur atoms having a valence of -2 or more and 0 or less is contained in a negative electrode coating after initial charge and discharge, and the compound contains at least one of sulfur or copper sulfide, The non-aqueous secondary battery is obtained by the following method: there is at least one charging process after the initial electrolyte injection process and before the final electrolyte injection process, and in the electrolyte injection process after the initial time, an electrolyte having a higher volume ratio of acetonitrile to the total electrolyte than the electrolyte used in the initial electrolyte injection process is injected into the battery outer packaging.

19. The nonaqueous secondary battery according to claim 18, wherein: The concentration of the vinyl sulfite in the non-aqueous electrolyte is 0.01 volume % or more and 4 volume % or less.

20. The nonaqueous secondary battery according to claim 18 or 19, wherein: The non-aqueous electrolyte further contains vinylene carbonate.