Etching method of phase change material layer
By using PVD and CVD processes to form SiN layer and silicon-containing anti-reflective layer in semiconductor integrated circuit manufacturing, the etching process of the GST layer is simplified, the problems of poor CD consistency and defects in the prior art are solved, and higher products are achieved Yield and reduce manufacturing costs.
Patent Information
- Application Number
- CN202280092779.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-07
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the etching process of the GST layer is complicated, resulting in poor CD consistency, defects, and high manufacturing cost, especially because the poor thickness uniformity of the SiO2 layer affects the lithography accuracy and the final consistency of the GST layer.
The GST layer and TiN layer were formed by PVD process, and then the SiN layer was formed by using the CVD process, and a carbon mask layer and a silicon-containing anti-reflection layer were formed on the SiN layer, simplifying the etching process, avoiding the formation of SiO2 layers, thereby improving CD consistency. sex and deficit reduction.
By simplifying the process and reducing the SiO2 layer products, the CD consistency of the GST layer is improved, manufacturing costs are reduced, and product yields are improved.
Smart Images

Figure CN118901298A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor integrated circuit manufacturing, and in particular to an etching method for a phase change material layer. Background Art
[0002] In the manufacture of semiconductor integrated circuits, especially in the manufacture of phase change memory, the requirements for etching of GST (phase change material) layers are getting higher and higher. Figure 7 As shown, in the prior art, the etching of the GST layer 91 usually forms a TiN (titanium nitride) layer 92, a SiN (silicon nitride) layer 93, a carbon HM (mask) layer 94, a SiO2 (silicon dioxide) layer 97, an ARC layer (anti-reflective layer) 95, and a PR (photoresist) layer 96 on the GST layer 91 in sequence, thereby forming a laminate 900. Then, the PR layer 96 is photolithographically processed to form a patterned PR layer. Then, the ARC layer 95, the SiO2 layer 97, the carbon HM layer 94, the SiN layer 93, the TiN layer 92, and the GST layer 91 are etched in sequence through the patterned PR layer to form a patterned GST layer.
[0003] Among them, the function of the ARC layer 95 is to absorb reflected light in the photolithography process and improve the photolithography accuracy. The function of the SiO2 layer 97 is to serve as a mask in the etching process of the carbon HM layer 94. Because the PR layer 96 and the ARC layer 95 are both relatively soft and cannot be used as masks in the etching process of the carbon HM layer 94, a SiO2 layer 97 must be formed under the ARC layer 95, and the carbon HM layer 94 is etched using the SiO2 layer 97 as a mask. The SiO2 layer 97 is usually formed by a CVD (chemical vapor deposition) process, but the U% (thickness uniformity) of the SiO2 layer 97 formed in this way is not good, which will affect the CD (feature size) uniformity (Uniformity) of the PR layer 96 and the ARC layer 95 during photolithography, thereby affecting the CD uniformity of the final GST layer. In addition, some products will be generated when etching the SiO2 layer 97, and these products will eventually fall on the GST layer, causing defects. In addition, the process of the prior art is also relatively complicated and the manufacturing cost is high.
[0004] Therefore, the industry is in urgent need of a GST layer etching method that can improve CD consistency, reduce defects, simplify the process, and reduce manufacturing costs. Summary of the invention
[0005] The present invention aims to provide a GST layer etching method which can improve CD consistency, reduce defects, simplify the process and reduce the manufacturing cost.
[0006] The etching method of the GST layer of the present invention comprises:
[0007] A laminate forming step, forming a laminate on a semiconductor substrate, wherein the laminate includes a phase change material layer, a titanium nitride layer, a silicon nitride layer, a carbon mask layer, a silicon-containing anti-reflection layer, and a photoresist layer formed in sequence from bottom to top;
[0008] A photolithography step of exposing and developing the photoresist layer to form a patterned photoresist layer;
[0009] a first etching step, etching the silicon-containing anti-reflection layer and the carbon mask layer through the patterned photoresist layer to form a patterned carbon mask layer;
[0010] a second etching step of etching the silicon nitride layer through the patterned carbon mask layer to form a patterned silicon nitride layer; and
[0011] A third etching step is to etch the titanium nitride layer and the phase-change material layer through the patterned silicon nitride layer to form a patterned titanium nitride layer and a patterned phase-change material layer.
[0012] The GST layer etching method of the present invention can improve CD consistency and reduce defects, thereby improving product yield, simplifying the manufacturing process and reducing manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is a flow chart of the etching method of the GST layer of the present invention;
[0014] Figures 2 to 6 is a schematic diagram of various steps of forming a patterned GST layer of the present invention; and
[0015] Figure 7 It is a schematic diagram of a laminated body of a GST layer etching method in the prior art.
[0016] Explanation of symbols
[0017] 100,900 laminated body
[0018] 1,91GST layer
[0019] 2. 92TiN layer
[0020] 3.93SiN layer
[0021] 4, 94 carbon HM layer
[0022] 5SHB layer
[0023] 6, 96PR layer
[0024] 11Patterned GST layer
[0025] 12 Patterned TiN layer
[0026] 13 Patterning SiN layer
[0027] 14 Patterned Carbon HM Layer
[0028] 15 Patterned SHB layer
[0029] 16 Patterned PR layer
[0030] 95ARC layer
[0031] 97SiO2 layer DETAILED DESCRIPTION
[0032] Refer to the following Figures 1 to 6 The etching method of the GST layer of the present invention is described. Figure 1 As shown, the etching method of the GST layer of the present invention includes: a laminate forming step S001, a photolithography step S002, a first etching step S003, a second etching step S004, and a third etching step S005. Each step will be described in detail below in conjunction with the accompanying drawings.
[0033] The layered body forming step S001, Figure 2 As shown, a laminate 100 is formed on a semiconductor substrate (not shown), and the laminate 100 includes a GST layer 1, a TiN layer 2, a SiN layer 3, a carbon HM layer 4, an SHB layer (Si rich hard mask bottom ARC, silicon-containing anti-reflection layer) 5, and a PR layer 6 formed in sequence from bottom to top.
[0034] In this embodiment, a GST layer 1 and a TiN layer 2 are first formed on a semiconductor substrate by a PVD (physical vapor deposition) process. The GST layer 1 and the TiN layer 2 may be formed directly on the semiconductor substrate, or there may be other layers between the semiconductor substrate and the GST layer 1 and the TiN layer 2. Then, a SiN layer 3 is formed on the TiN layer 2 by a CVD process. The SiN layer 3 may be formed directly on the TiN layer 2, or there may be other layers between the TiN layer 2 and the SiN layer 3. Then, a carbon HM layer 4, an SHB layer 5, and a PR layer 6 are sequentially formed on the SiN layer 3 by a coating process.
[0035] Due to the properties of the GST layer 1 and the TiN layer 2, SiN needs to be used as a mask for etching. Therefore, it is necessary to first form a SiN layer 3 on the GST layer 1 and the TiN layer 2. Before etching the GST layer 1 and the TiN layer 2, the SiN layer 3 must be etched first to form a patterned SiN layer, and then the GST layer 1 and the TiN layer 2 are etched through the patterned SiN layer. Because the SiN layer 3 is relatively hard and difficult to etch, when etching the SiN layer 3, the PR layer 6 and the SHB layer 5 cannot be directly used as a mask for the SiN layer 3. A carbon HM layer 4 must be formed on the SiN layer 3, and the carbon HM layer 4 must be used as a mask for etching the SiN layer 3.
[0036] Among them, the SHB layer 5 can play an anti-reflective role, so that it can absorb reflected light in the photolithography process and improve the photolithography accuracy. In addition, because the SHB layer 5 contains silicon, its hardness is relatively large, so it can be used as a mask for etching the carbon HM layer 4. In this way, there is no need to form a SiO2 layer on the carbon HM layer 4. In addition, the U% of the SHB layer 5 is better, so the CD consistency of the final GST layer will be improved. In addition, because there is no SiO2 layer, the product generated when etching the SiO2 layer will not appear, and it will not fall on the GST layer to cause defects. This also reduces the defects on the final GST layer. In addition, there is no need to use a CVD process to form a SiO2 layer, which can simplify the manufacturing process and reduce manufacturing costs.
[0037] Photolithography step S002, such as Figure 3 As shown, the PR layer 6 is exposed and developed to form a patterned PR layer 16. The PR layer 6 can be exposed and developed in any suitable manner in the prior art, which will not be described in detail herein.
[0038] The first etching step S003, such as Figure 4 As shown, the SHB layer 5 and the carbon HM layer 4 are etched through the patterned PR layer 16 to form a patterned carbon HM layer 14 .
[0039] The second etching step S004, such as Figure 5 As shown, the SiN layer 3 is etched through the patterned carbon HM layer 14 to form a patterned SiN layer 13 .
[0040] The third etching step S005, as Figure 6 As shown, the TiN layer 2 and the GST layer 1 are etched through the patterned SiN layer 13 to form the patterned TiN layer 12 and the patterned GST layer 11. In addition, after the patterned TiN layer 12 and the patterned GST layer 11 are formed, a thin layer of SiN will remain on the top of the patterned TiN layer 12, and this layer of SiN can be used as a protective layer and an insulating layer for the patterned TiN layer 12 and the patterned GST layer 11 in subsequent processes.
[0041] The carbon HM layer 4 , the SiN layer 3 , the TiN layer 2 and the GST layer 1 may be etched in any suitable manner in the prior art, which will not be described in detail herein.
[0042] The GST etching method of the present invention can improve CD consistency and reduce defects, thereby improving product yield, simplifying the manufacturing process and reducing manufacturing costs.
[0043] Although the present invention has been disclosed in the above embodiments, it is not intended to limit the present invention. Any professional and technical personnel in the field may make various necessary changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined by the attached claims.
Claims
1. A method for etching a phase change material layer, comprising: A laminate forming step S001, forming a laminate (100) on a semiconductor substrate, wherein the laminate (100) comprises a phase change material layer (1), a titanium nitride layer (2), a silicon nitride layer (3), a carbon mask layer (4), a silicon-containing anti-reflection layer (5), and a photoresist layer (6) formed in sequence from bottom to top; Photolithography step S002, exposing and developing the photoresist layer (6) to form a patterned photoresist layer (16); A first etching step S003, etching the silicon-containing anti-reflection layer (5) and the carbon mask layer (4) through the patterned photoresist layer (16) to form a patterned carbon mask layer (14); A second etching step S004, etching the silicon nitride layer (3) through the patterned carbon mask layer (14) to form a patterned silicon nitride layer (13); as well as A third etching step S005 is to etch the titanium nitride layer (2) and the phase change material layer (1) through the patterned silicon nitride layer (13) to form a patterned titanium nitride layer (12) and a patterned phase change material layer (11).
Citation Information
Patent Citations
Semiconductor device, manufacturing method thereof and electronic device
CN107437582A
Reworking method of three-layer photoetching material
CN111584348A
Method for forming ion implantation region
CN113130308A
Etching method for improving feature size uniformity