Heating body assembly and preparation method thereof

By combining the ceramic matrix with the heating element and using eutectic bonding or active metal brazing method to prepare the ceramic heating element components, the problems of high cost of preparation of ceramic heating needles and complex process are solved, economical and simple production is achieved, and improved Component reliability and durability.

CN118902185APending Publication Date: 2024-11-08SHENZHEN GEEKVAPE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411107657.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing ceramic heating needles are cost-effective and complex in preparation, making it difficult to achieve economical and simple production.

Method used

By obtaining the ceramic substrate and the heating element, and combining part of the heating element with eutectic bonding or active metal brazing method to form a ceramic heating element assembly, the ceramic substrate is used to absorb heat and heat the aerosol to form a matrix .

Benefits of technology

It reduces the preparation cost of heating element components, improves the reliability and durability of components, simplifies the process flow, and adapts to large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118902185A_ABST
    Figure CN118902185A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aerosol atomization, and provides a heating element assembly and a preparation method thereof. The preparation method comprises the following steps: obtaining a ceramic substrate and a heating body; wherein the heating body is used for heating to generate heat after being electrified; combining at least part of the surface of the heating element with the ceramic substrate to obtain a heating element assembly; the ceramic substrate is used to absorb at least a portion of the heat and heat the aerosol-forming substrate. The heating body assembly comprises a heating body which is used for heating to generate heat after being electrified; a ceramic substrate for absorbing at least part of the heat and heating the aerosol-forming substrate; wherein at least partial area of the heating body is connected to the ceramic substrate. The heating body comprises a first element, a second transition layer and a second element; and the second transition layer is arranged between the first element and the second element and is used for enhancing the binding force between the first element and the second element. The cost of preparing the heating element assembly through the preparation method is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aerosol atomization, and in particular to a heating element component and a preparation method thereof. Background Art

[0002] At present, the ceramic heating element of the heat-not-burn electronic cigarette can be roughly divided into two types: one is a ceramic heating sheet with a thick film circuit printed on the surface of a zirconia ceramic sheet, and the other is a ceramic heating needle prepared by coating an alumina cast sheet with a printed circuit on the surface of an alumina rod core. The existing ceramic heating needles usually adopt multi-layer thick film co-firing technology, and the preparation process is complicated. For example, a zirconia ceramic heating element disclosed in a Chinese patent document with publication number CN211932568U. The zirconia ceramic heating element includes a zirconia rod body, the zirconia rod body includes a rod core and a pointed piece arranged at one end of the rod core, and the outer surface of the rod core is sequentially provided with a first alumina insulating layer, a printed circuit layer, a second alumina insulating layer and a zirconia ceramic substrate from the inside to the outside; the pointed piece includes a tip portion and an embedded portion arranged on the bottom surface of the tip portion, and the embedded portion is embedded in the inside of the rod core; the outer surface of the zirconia ceramic substrate and the outer surface of the tip portion are coated with a first protective glaze layer. It can be seen that the preparation cost of the existing ceramic heating needles is high and the process is complicated.

[0003] Therefore, it is necessary to improve the deficiencies in the prior art. Summary of the invention

[0004] The main technical problem solved by the present invention is to provide a heating element component and a preparation method of the component, and the preparation method can reduce the cost of preparing the heating element component.

[0005] According to the first aspect, an embodiment provides a method for preparing a heating element assembly. The preparation method comprises:

[0006] Obtain a ceramic matrix and a heating element; wherein the heating element is used to generate heat by heating after being energized;

[0007] The heating element assembly is obtained by bonding at least a portion of the surface of the heating element to the ceramic substrate; wherein the ceramic substrate is used to absorb at least a portion of the heat and heat the aerosol-forming matrix.

[0008] In one embodiment, the step of combining at least a portion of the surface of the heating element with the ceramic substrate to obtain the heating element assembly comprises:

[0009] The step of bonding: heating the heating element and the ceramic substrate to a preset temperature, and bonding at least a portion of the heating element to the ceramic substrate by eutectic bonding; wherein the preset temperature is higher than a preset temperature threshold;

[0010] The ceramic substrate and the heating element that have undergone the combining step are used as the heating element assembly.

[0011] In one embodiment, the step of combining at least a portion of the heating element with the ceramic substrate to obtain the heating element assembly comprises:

[0012] The step of combining: using a metal brazing material containing active elements to braze at least a portion of the heating element to a surface of one side of the ceramic substrate to obtain the heating element assembly; wherein the active element includes at least one of titanium, zirconium, hafnium and tantalum.

[0013] In one embodiment, the heating element includes a first element; the first element is used to generate heat by heating after being energized.

[0014] In one embodiment, the heating element includes a first element and a second element; wherein the second element is used to generate heat by heating after being energized; the first element is used to serve as a first transition layer to connect the second element to the ceramic substrate; the resistivity of the second element is greater than the resistivity of the first element.

[0015] In one embodiment, the heating body includes a first element, a second transition layer and a second element; wherein the second transition layer is arranged between the first element and the second element to enhance the bonding force between the first element and the second element; the thickness of the second transition layer is less than a preset thickness threshold; the second transition layer contains elements in the first element and elements in the second element.

[0016] In one embodiment, the combining step also includes: pre-treating the heating element; wherein the pre-treating the heating element includes: blackening the surface of the second element facing the ceramic substrate or coating the surface of the second element facing the ceramic substrate to increase the emissivity of thermal radiation generated by the surface of the second element facing the ceramic substrate; and / or optimizing the smoothness of the surface of the second element away from the ceramic substrate; and / or optimizing the flatness of the surface of the first element and the second element facing the ceramic substrate; and / or providing holes of a preset shape on the second element; and / or arranging at least part of the first element between the second element and the ceramic substrate in a preset arrangement.

[0017] In one embodiment, the combining step also includes: pre-treating the heating element; wherein the pre-treating the heating element includes: blackening the surface of the first element facing the ceramic substrate or coating the surface of the first element facing the ceramic substrate to increase the emissivity of thermal radiation generated by the surface of the first element facing the ceramic substrate; and / or optimizing the smoothness of the surface of the first element facing away from the ceramic substrate; and / or optimizing the flatness of the surface of the first element facing the ceramic substrate; and / or providing holes of a preset shape on the first element.

[0018] In one embodiment, the first element includes one of copper foil, silver foil, silver-copper alloy foil, copper-aluminum alloy foil, aluminum bronze foil or copper-titanium alloy foil; the material of the ceramic matrix includes one of alumina ceramic, aluminum nitride ceramic, zirconium oxide toughened alumina ceramic or composite ceramic; wherein the composite ceramic contains alumina.

[0019] In one embodiment, when the ceramic substrate does not contain aluminum, the step of combining at least a portion of the heating element to the ceramic substrate to obtain the heating element assembly further includes: before the combining step, spraying or covering a third transition layer on the surface of the ceramic substrate facing the heating element; wherein the third transition layer contains aluminum oxide.

[0020] In one embodiment, the material of the second element includes any one of titanium, iron-nickel alloy, austenitic stainless steel, constantan alloy, manganese-copper alloy, germanium-manganese-copper alloy, nickel-chromium alloy, iron-chromium-aluminum alloy or tungsten; wherein at least part of the first element is used as an electrode, and the electrode is used to be connected to a power source.

[0021] According to the second aspect, an embodiment provides a heating element assembly, which comprises: a heating element, which is used to generate heat by heating after being energized; and a ceramic matrix, which is used to absorb at least part of the heat and heat the aerosol-forming matrix; wherein at least part of the heating element is connected to the ceramic matrix.

[0022] In one embodiment, the heating element includes a first element; the first element is used to generate heat by heating after being energized.

[0023] In one embodiment, the surface of the first element facing the ceramic substrate is blackened; and / or the surface of the first element away from the ceramic substrate has a smoothness greater than a preset smoothness threshold; and / or the surface of the first element facing the ceramic substrate has a flatness greater than a preset flatness threshold; and / or a hole of a preset shape is provided on the first element.

[0024] In one embodiment, the heating element includes a first element and a second element; wherein the second element is used to generate heat by heating after being energized; the first element is used to serve as a first transition layer to connect the second element to the ceramic substrate; the resistivity of the second element is greater than the resistivity of the first element.

[0025] In one embodiment, the heating body also includes a second transition layer; wherein the second transition layer is arranged between the first element and the second element to enhance the bonding force between the first element and the second element; the thickness of the second transition layer is less than a preset thickness threshold; the second transition layer contains elements in the first element and elements in the second element.

[0026] In one embodiment, the surface of the second element facing the ceramic substrate is blackened or coated with a coating; and / or the surface of the second element facing the ceramic substrate has a smoothness greater than a preset smoothness threshold; and / or the flatness of the surface of the first element and the second element facing the ceramic substrate is greater than a preset flatness threshold; and / or the second element is provided with holes of a preset shape; and / or at least part of the first element is arranged between the second element and the ceramic substrate in a preset manner.

[0027] In one embodiment, the ceramic matrix is ​​located between the heating element and the aerosol generating substrate.

[0028] The beneficial effects of this application are:

[0029] The preparation method of the present application includes: obtaining a ceramic substrate and a heating element; wherein the heating element is used to generate heat by heating after being energized; combining at least a portion of the surface of the heating element with the ceramic substrate to obtain a heating element assembly; the ceramic substrate is used to absorb at least a portion of the heat and heat the aerosol-forming matrix; since the above-mentioned step of "combining at least a portion of the surface of the heating element with the ceramic substrate to obtain a heating element assembly" is achieved with the aid of "direct copper plating method" or "active metal brazing method", and "direct copper plating method" or "active metal brazing method" itself is very mature and can be easily adapted to large-scale production, and is relatively simple and economical, therefore, the cost of preparing the heating element assembly by the preparation method of the present application is relatively low; the heating element assembly of the present application includes: a heating element, used to generate heat by heating after being energized; a ceramic substrate, used to absorb at least a portion of the heat and heat the aerosol-forming matrix; wherein at least a portion of the heating element is connected to the ceramic substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A schematic diagram of a process for preparing a heating element assembly according to an embodiment;

[0031] Figure 2 A schematic diagram of a process of combining at least a partial area of ​​a heating element with a ceramic substrate to obtain a heating element assembly according to an embodiment;

[0032] Figure 3 A schematic diagram of a process of combining at least a partial area of ​​a heating element with a ceramic substrate to obtain a heating element assembly according to another embodiment;

[0033] Figure 4 A schematic diagram of a top view of a heating element assembly according to an embodiment;

[0034] Figure 5 A schematic diagram of the cross-sectional structure of a heating element assembly according to an embodiment of the present invention along the axial center line of the heating element;

[0035] Figure 6 A schematic diagram of the structure of a heating element and a ceramic substrate according to an embodiment;

[0036] Figure 7 A schematic diagram of the structure of a heating element and a ceramic substrate in another embodiment;

[0037] Figure 8 A schematic diagram of the structure of a first element and a second element of an embodiment;

[0038] Fig. 9 A schematic structural diagram of a first element and a second element of another embodiment;

[0039] Fig.10 The present invention is a schematic flow chart of a method for preparing a heating element assembly according to another embodiment. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below by specific embodiments in conjunction with the accompanying drawings. Wherein similar elements in different embodiments adopt associated similar element numbers. In the following embodiments, many detailed descriptions are for making the present application better understood. However, those skilled in the art can easily recognize that some features can be omitted in different situations, or can be replaced by other elements, materials, methods. In some cases, some operations related to the present application are not shown or described in the specification, this is to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and they can fully understand the related operations according to the description in the specification and the general technical knowledge in the art.

[0041] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate manner to form various implementations. At the same time, the steps or actions in the method description can also be interchanged or adjusted in a manner that is obvious to those skilled in the art. Therefore, the various sequences in the specification and the drawings are only for the purpose of clearly describing a certain embodiment and are not meant to be a required sequence, unless otherwise specified that a certain sequence must be followed.

[0042] The serial numbers of the components in this document, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in this application, unless otherwise specified, include direct and indirect connections (couplings).

[0043] The technical solution of the present application will be described in detail below in conjunction with embodiments.

[0044] Please refer to Figure 1 The present application provides a method for preparing a heating element assembly. The method comprises:

[0045] Step S100: obtaining a ceramic substrate and a heating element;

[0046] Step S200: combining at least a portion of the heating element with a ceramic substrate to obtain a heating element assembly.

[0047] Specifically, in step S100, a ceramic substrate and a heating element are obtained; wherein the heating element is used to generate heat by heating after being energized.

[0048] Specifically, in step S200, at least a portion of the heating element is combined with a ceramic matrix to obtain a heating element assembly; wherein the ceramic matrix is ​​used to absorb at least a portion of the heat and heat the aerosol-forming matrix.

[0049] It should be noted that in step S100, the ceramic matrix can have a preset shape; the ceramic matrix is ​​directly made using the existing technology in the field. For example, it can be obtained by batch molding using existing molding methods (such as ceramic injection molding, die casting, dry powder pressing or extrusion molding) and further sintering. The material of the ceramic matrix includes any one of the following: YSZ (yttria reinforced zirconia), ZTA (zirconia reinforced alumina), alumina or silicon nitride, etc.

[0050] In some embodiments, the ceramic substrate in step S100 may be in a two-dimensional planar structure, for example, the ceramic substrate may be in a rectangular shape, etc. At this time, the heating element may also be in a two-dimensional planar structure, for example, the heating element may also be in a rectangular shape, etc.

[0051] In some embodiments, the ceramic substrate in step S100 may be a three-dimensional structure. For example, the ceramic substrate may be cylindrical or rectangular. For example, the top of the ceramic substrate may be conical, and the ceramic substrate other than the top may be cylindrical.

[0052] Since if the heating element and the aerosol generating matrix are located on the same side of the ceramic matrix, the aerosol generating matrix will frequently collide / rub / contact with the heating element outside the ceramic matrix during use, which will cause the heating element to fall off and be damaged, etc., that is, the reliability and durability of the existing heating element assembly are low. Therefore, in one embodiment, the ceramic matrix is ​​located between the heating element and the aerosol generating matrix, and the heating element and the aerosol generating matrix are separated by the ceramic matrix as a shell to avoid direct contact between the heating element and the aerosol generating matrix, thereby preventing the strength of the heating element from being reduced and / or causing the heating element to fall off during the repeated contact between the heating element and the aerosol generating matrix, that is, the above-mentioned ceramic matrix substantially protects the heating element, thereby improving the reliability and durability of the heating assembly obtained by the present preparation method. In some embodiments, in step S100, the ceramic matrix has a cavity, and the inner wall of the cavity has a certain roughness. That is to say, at least a part of the area of ​​the heating element is combined with the inner wall of the cavity. The ceramic matrix can be used to protect the heating element in the cavity, that is, the heating element is separated from the aerosol generating matrix by the ceramic matrix as a shell to avoid direct contact between the heating element and the aerosol generating matrix, thereby preventing the strength of the heating element from being reduced and / or causing the heating element to fall off during repeated contact between the heating element and the aerosol generating matrix. The wall thickness of the ceramic matrix is ​​usually less than the preset wall thickness threshold. Those skilled in the art can determine the preset wall thickness threshold according to actual needs.

[0053] It should be noted that, in some embodiments, since the heating element in the heating element assembly must have a certain rigidity and a fixed shape, the heating element assembly can be repeatedly inserted into the aerosol-forming matrix in the atomization device and baked and atomized. Therefore, the roles of the above-mentioned ceramic matrix include: 1) giving the heating element a certain shape and rigidity so that the contact state and heat transfer state of the heating element in the atomization device are relatively stable; 2) the above-mentioned ceramic matrix acts as an outer shell, that is, it substantially protects and supports the heating element; 3) it buffers the heat released by the heating element, that is, it prevents the heating element from directly contacting the heating object of the heating needle and causing local over-baking or burning.

[0054] It should be noted that the person skilled in the art can determine the type of the aerosol-forming substrate according to actual needs. Since the specific types of aerosol-forming substrates are common knowledge in the art, the specific composition of the aerosol-forming substrate will not be described in detail.

[0055] In some embodiments, the heating element in step S100 includes a first element; the first element is used to generate heat after being powered on; wherein, please refer to Figure 2 Step S200: combining at least a portion of the heating element with a ceramic substrate to obtain a heating element assembly, comprising:

[0056] The step of combining S210a: heating the heating element and the ceramic substrate to a preset temperature, and combining at least a portion of the heating element (such as the first element) with the ceramic substrate by eutectic bonding; wherein the preset temperature is higher than a preset temperature threshold;

[0057] Step S220a: The ceramic substrate and the heating element combined in step S210a are used as a heating element assembly.

[0058] In some embodiments, a partial area of ​​the heating element in step S210a can also be used as a first transition layer to connect the heating element to the ceramic substrate. The heating element can be connected to a surface of the ceramic substrate that is away from the aerosol-forming substrate.

[0059] In some embodiments, one side surface of the ceramic substrate in step S210a has a preset groove. In this case, the above step S210a may include: heating the heating element and the ceramic substrate to a preset temperature, and bonding at least a portion of the heating element to the groove of the ceramic substrate by eutectic bonding.

[0060] It should be noted that the above-mentioned combined step S210a and step S220a are a mature process of copper coating on a ceramic substrate, i.e., direct copper coating (DBC), with at least a part of the above-mentioned heating element (such as a first element made of copper or other medium) as an intermediate bonding phase, and the above-mentioned heating element (such as the first element) is bonded to the inner wall of the ceramic substrate. In other words, the above-mentioned combined step S210a can be basically the same as the specific process of the existing direct copper coating (DBC). The direct copper coating method is a metallization method for bonding copper or other similar media on the surface of a ceramic substrate. It is a new process developed with the rise of chip-on-board packaging technology. The basic principle of the direct copper coating method is to introduce oxygen elements between copper and the ceramic substrate, and then form a Cu / O eutectic liquid phase at 1065-1083°C, and then react with the ceramic substrate and copper foil to form CuAlO2 or Cu(AlO2)2, and realize the bonding of copper foil or other similar media to the ceramic substrate under the action of the intermediate phase. The above-mentioned "preset temperature" refers to the temperature required for the direct copper plating method. For example, the range of the above-mentioned "preset temperature" includes: 1065~1083℃.

[0061] It should be noted that, in some embodiments, since the above-mentioned combined step S210a and step S220a may be substantially the same as the specific steps of the above-mentioned direct copper plating method, the detailed process of step S210a and step S220a will not be repeated here.

[0062] In some embodiments, in step S210a, after the heating element and the ceramic substrate are heated to a preset temperature, the ceramic substrate and the heating element heated to the preset temperature can be pressed together, and then at least a portion of the first element is bonded to one side surface of the ceramic substrate by eutectic bonding.

[0063] The eutectic bonding in the above step S210a, also known as eutectic welding, refers to a bonding process in which two or more metal layers are directly transformed from solid to liquid at a certain temperature, and a eutectic phase is formed on the bonding surface through metal recrystallization. The advantage of eutectic bonding is that the temperature of the bonding process is lower than that of direct bonding, and is much lower than the melting point of a single layer of metal; at the same time, the outgassing volume during the bonding process is very low, and high vacuum zero-level packaging can be achieved; in addition, since eutectic bonding is liquid phase bonding, it is not sensitive to the flatness, scratches and particles of the bonding surface, which is conducive to ensuring the bonding yield and mass production.

[0064] In some embodiments, the above-mentioned combined step S210a also includes: pre-treating the heating element; wherein the pre-treating the heating element includes: blackening the surface of the first element facing the ceramic substrate or coating the surface of the first element facing the ceramic substrate; and / or optimizing the smoothness of the surface of the first element facing away from the ceramic substrate; and / or optimizing the flatness of the surface of the first element facing the ceramic substrate; and / or setting holes of a preset shape on the first element.

[0065] In some embodiments, the "pretreatment of the heating element" in the above step S210a can be performed before or after "heating the heating element and the ceramic substrate to a preset temperature" in step S210a; or, the "pretreatment of the heating element" can be performed after "pressing the ceramic substrate heated to the preset temperature and the heating element" in step S210a; or, the "pretreatment of the heating element" can be performed after "bonding at least a partial area of ​​the first element to one side surface of the ceramic substrate by eutectic bonding" in step S210a.

[0066] It should be noted that the purpose of "blackening the surface of the first element facing the ceramic substrate" in the "pre-treating the heating element" in the above step S210a is to form an oxide film on the surface of the first element facing the ceramic substrate, so as to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate, thereby improving the baking effect of the heating element. The principle of the blackening treatment is to oxidize the surface of the object to be blackened so that it forms a dense oxide film protective layer. The blackening treatment can adopt the existing alkaline heating blackening and room temperature blackening methods. The purpose of "coating the coating on the surface of the first element facing the ceramic substrate" is also to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate. Those skilled in the art can select the existing technology as the coating according to actual needs.

[0067] It should be noted that the purpose of "optimizing the smoothness of the surface of the side of the first element away from the ceramic substrate" in the "pre-treatment of the heating element" in the above step S210a is to reduce the emissivity of the thermal radiation generated by the surface of the side of the first element away from the ceramic substrate. Specifically, the existing technical means such as mechanical polishing, chemical polishing, electrolytic polishing or ultrasonic polishing can be used to "optimize the smoothness of the surface of the side of the first element away from the ceramic substrate".

[0068] It should be noted that the purpose of "optimizing the flatness of the surface of the first element facing the ceramic substrate" in the "pre-processing the heating element" in the above step S210a is also to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate. For example, the existing technology can be directly used to "optimize the flatness of the surface of the first element facing the ceramic substrate".

[0069] It should be noted that the purpose of "arranging a hole of a preset shape on the first element" in the "pre-treatment of the heating element" in the above step S210a is to adjust the resistance of the first element and / or alleviate the thermal stress on the first element according to actual needs. Punching or etching methods can be used to "arrange a hole of a preset shape on the first element". Those skilled in the art can determine the "preset shape" according to actual needs. For example, the "preset shape" can be a rhombus; the "preset shape" can also be other shapes (such as a square, etc.).

[0070] In some embodiments, the combining step S210a further includes: connecting a lead wire to one end of at least part of the first elements, the lead wire being used to connect to a power source. In other words, part of the first elements or all of the first elements are used as electrodes.

[0071] Since the heating performance of the first element after power-on is poor if the first element is made of copper foil or an element with lower resistivity, in some embodiments, an element with higher resistivity (e.g., an element with higher resistivity than copper foil) is used as the second element, and the second element is heated to generate heat after power-on. That is, the heating element in step S100 includes a first element and a second element; wherein the second element is used to generate heat after power-on; the first element is used as a first transition layer to connect the second element to the ceramic substrate; and the resistivity of the second element is greater than that of the first element. At this time, please refer to Figure 3 In step S200, at least a portion of the heating element is combined with a ceramic substrate to obtain a heating element assembly, including:

[0072] The step of combining S210b: placing the first element between the ceramic substrate and the second element, heating the ceramic substrate, the first element and the second element to a preset temperature, and combining at least a portion of the first element to the ceramic substrate and the second element respectively by eutectic bonding; wherein the preset temperature is higher than a preset temperature threshold;

[0073] Step S220b: The ceramic substrate, the first element and the second element that have undergone the combining step are used as a heating element assembly.

[0074] In some embodiments, the first element in the above step S210b is used as a first transition layer to connect the second element to the ceramic substrate. For example, the first element is used as a first transition layer to connect the second element to a surface of the ceramic substrate away from the aerosol-forming substrate.

[0075] In some embodiments, in step S210b, after "heating the ceramic substrate, the first element and the second element to a preset temperature", the ceramic substrate, the first element and the second element heated to the preset temperature can be pressed together, and then at least a portion of the first element can be bonded to one side surface of the ceramic substrate and one side surface of the second element respectively by eutectic bonding.

[0076] It should be noted that, in some embodiments, the above step S210b may be substantially the same as the above step S210a, and the difference between the two is that the heating element in step S210b includes a first element and a second element, and the second element is used to generate heat by heating after being energized; while the heating element in step S210a includes only a first element, and the first element is used to generate heat by heating after being energized. Therefore, the specific process of the above step S210b will not be described here.

[0077] In some embodiments, at least a portion of the first element in step S210b may serve as a first transition layer to connect the second element to the ceramic substrate. The second element may also be connected to a surface of the ceramic substrate away from the aerosol-forming substrate.

[0078] In some embodiments, one side surface of the ceramic substrate in step S210b has a groove of a preset shape. The above step S210b may include: positioning the first element between the ceramic substrate and the second element, heating the ceramic substrate, the first element and the second element to a preset temperature, and bonding at least a portion of the first element to the groove of the ceramic substrate and one side surface of the second element respectively by eutectic bonding.

[0079] In some embodiments, in order to further enhance the bonding force between the first element and the second element in step S200, an ultra-thin second transition layer that is easier to bond with the second element may be introduced between the first element and the second element. That is, the heating element includes a first element, a second transition layer, and a second element; wherein the second transition layer is disposed between the first element and the second element, and is used to enhance the bonding force between the first element and the second element after completing step S200; the thickness of the second transition layer is less than a preset thickness threshold; the second transition layer contains elements in the first element and elements in the second element. For example, when the first element and the second element are copper foil and titanium foil, respectively, the second transition layer may be an ultra-thin copper-titanium alloy layer. The second transition layer contains elements in the first element and elements in the second element, that is, the specific material of the second transition layer is determined based on the elements in the first element and the elements in the second element.

[0080] The above preset thickness threshold can be determined by those skilled in the art. The purpose of setting the thickness of the second transition layer to be less than the preset thickness threshold is to make the thickness of the second transition layer relatively thin or within the preset thickness threshold.

[0081] In some embodiments, the above-mentioned combined step S210b also includes: pre-treating the heating element; wherein the pre-treating the heating element includes: blackening the surface of the second element on the side facing the ceramic substrate or coating the surface of the second element on the side facing the ceramic substrate to increase the emissivity of the thermal radiation generated by the surface of the second element on the side facing the ceramic substrate, thereby improving the baking effect of the heating element; and / or, optimizing the smoothness of the surface of the second element on the side away from the ceramic substrate; and / or, optimizing the flatness of the surface of the first element and the second element on the side facing the ceramic substrate; and / or, setting holes of a preset shape on the second element; and / or, arranging at least part of the first element between the second element and the ceramic substrate in a preset arrangement.

[0082] In some embodiments, the "pretreatment of the heating element" in the above-mentioned step S210b may be performed before or after "locating the first element between the ceramic substrate and the second element, and heating the ceramic substrate, the first element and the second element to a preset temperature" in step S210b; or, the "pretreatment of the heating element" may be performed after "pressing the ceramic substrate, the first element and the second element heated to the preset temperature" in step S210b; or, the "pretreatment of the heating element" may be performed after "bonding at least a portion of the first element to one side surface of the ceramic substrate and one side surface of the second element, respectively, by eutectic bonding" in step S210b.

[0083] It should be noted that the purpose of "blackening the surface of the second element facing the ceramic substrate" in the "pre-treating the heating element" in the above step S210b is to form an oxide film on the surface of the first element facing the ceramic substrate, so as to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate, thereby improving the baking effect of the heating element. The principle of the blackening treatment is to oxidize the surface of the object to be blackened so that it forms a dense oxide film protective layer. The blackening treatment can adopt the existing alkaline heating blackening and room temperature blackening methods. The purpose of "coating the coating on the surface of the second element facing the ceramic substrate" is also to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate. Those skilled in the art can select the existing technology as the coating according to actual needs.

[0084] It should be noted that the purpose of "optimizing the smoothness of the surface of the second element away from the ceramic substrate" in the "pre-treating the heating element" in the above step S210b is to reduce the emissivity of the thermal radiation generated by the surface of the second element away from the ceramic substrate. Specifically, the existing technical means such as mechanical polishing, chemical polishing, electrolytic polishing or ultrasonic polishing can be used to "optimize the smoothness of the surface of the second element away from the ceramic substrate".

[0085] It should be noted that the purpose of "optimizing the flatness of the surface of the first element and the second element facing the ceramic substrate" in the "pre-processing the heating element" in the above step S210b is also to improve the emissivity of the thermal radiation generated by the surface of the first element and the second element facing the ceramic substrate. For example, the existing technology can be directly used to "optimize the flatness of the surface of the first element and the second element facing the ceramic substrate".

[0086] It should be noted that the purpose of "arranging a hole of a preset shape on the second element" in the "pre-treatment of the heating element" in the above step S210b is to adjust the resistance of the second element and / or alleviate the thermal stress on the second element according to actual needs. Punching or etching methods can be used to "arrange a hole of a preset shape on the second element". Those skilled in the art can determine the "preset shape" according to actual needs. For example, the "preset shape" can be a rhombus; the "preset shape" can also be other shapes (such as a square, etc.).

[0087] It should be noted that the purpose of "arranging at least part of the first element between the second element and the ceramic substrate in a preset arrangement" in the "pre-treating the heating element" in the above step S210b is to optimize the tightness and uniformity of the fit between the second element and the ceramic substrate. Those skilled in the art can determine the preset arrangement according to actual needs. For example, the first element that is not part of the electrode is arranged in a discrete lattice to optimize the tightness and uniformity of the fit between the second element and the ceramic substrate.

[0088] In some embodiments, the combining step S210b further includes: connecting a lead wire to one end of at least part of the first elements, the lead wire being used to connect to a power source. In other words, part of the first elements or all of the first elements are used as electrodes.

[0089] In some embodiments, the first element includes one of copper foil, silver foil, silver-copper alloy foil, copper-aluminum alloy foil, aluminum bronze foil or copper-titanium alloy foil; the material of the ceramic matrix includes one of alumina ceramic, aluminum nitride ceramic, zirconium oxide toughened alumina ceramic or composite ceramic; wherein the composite ceramic contains alumina.

[0090] In some embodiments, when the ceramic substrate does not contain aluminum, in step S200, at least a portion of the heating element is bonded to the ceramic substrate to obtain a heating element assembly, and the step further includes: before the bonding step (such as the above-mentioned step S210a or S210b), spraying or covering a third transition layer on the surface of the ceramic substrate facing the heating element; wherein the third transition layer contains aluminum oxide. For example, the third transition layer can directly use aluminum oxide material. The third transition layer can also be a mixed ceramic layer containing aluminum oxide. Those skilled in the art can determine the specific material of the third transition layer by themselves, as long as the third transition layer contains aluminum oxide.

[0091] In some embodiments, the material of the second element includes any one of titanium, iron-nickel alloy, austenitic stainless steel, constantan alloy, manganese-copper alloy, germanium-manganese-copper alloy, nickel-chromium alloy, iron-chromium-aluminum alloy or tungsten; wherein at least part of the first element is used as an electrode, and the electrode is used to connect to a power source. The austenitic stainless steel can be SUS904, SUS316 or SUS310s. The SUS904, SUS316 or SUS310s are all existing models of austenitic stainless steel.

[0092] It can be seen that in some embodiments, since step S200 of the preparation method includes step S210a or S210b of the above-mentioned combination using the "direct copper plating method", and the "direct copper plating method" itself is very mature and can be easily adapted to large-scale production, this method is relatively simple and economical. Therefore, the cost of preparing the heating element assembly by the preparation method of the present application is relatively low.

[0093] For some examples, please refer to Fig.10 , the preparation method comprises:

[0094] Step S100: obtaining a ceramic substrate and a heating element;

[0095] Brazing step S210c: using a metal brazing material containing active elements, brazing at least a portion of the heating element to a surface of one side of the ceramic substrate to obtain a heating element assembly.

[0096] That is, in the above step S200, at least a part of the heating element is combined with the ceramic substrate to obtain the heating element assembly, including:

[0097] Brazing step S210c: using a metal brazing material containing active elements, brazing at least a portion of the heating element to a surface of one side of the ceramic substrate to obtain a heating element assembly.

[0098] Those skilled in the art can also determine the specific types of the above-mentioned active elements and metal brazing materials according to actual needs. For example, the active elements include titanium (Ti), zirconium (Zr), hafnium (Hf) and / or tantalum (Ta); the metal brazing material can be a silver-copper alloy solder (AgCu) containing titanium (Ti) and zirconium (Zr). The small amount of active elements added to the metal brazing material has high activity, which can improve the wettability of the metal brazing material to the ceramic substrate after melting, so that the surface of the ceramic substrate can be well welded with the heating element without metallization.

[0099] It should be noted that the above step S210c is a mature process of active metal brazing, with at least a part of the above first element (such as copper foil or other medium) as the intermediate bonding phase, to combine the above second element on the inner wall of the ceramic substrate. That is to say, the above combined step S210c can be basically the same as the specific process of the existing active metal brazing method. The active metal brazing method is also a widely used ceramic-metal sealing process, which is characterized by fewer steps and the ceramic-metal sealing can be completed in one heating process. The brazing alloy contains active elements, such as titanium (Ti), zirconium (Zr), hafnium (Hf) and / or tantalum (Ta). The added active elements react with aluminum oxide (Al2O3) to form a reaction layer with metallic properties at the interface. This method can be easily adapted to large-scale production. Compared with the molybdenum-manganese process, this method is relatively simple and economical.

[0100] It should be noted that, in some embodiments, since the above step S210c may be substantially the same as the specific steps of the above active metal brazing method, the detailed process of step S210c will not be described in detail herein.

[0101] It should be noted that the main differences between the above-mentioned combined step S210a or S210b using the "direct copper plating method" and the above-mentioned brazing step S210c using the "active metal brazing method" include: the first element (such as copper foil) and the ceramic substrate in the above-mentioned combined steps S210a and S210b are directly bonded, while the first element (such as copper foil) and the ceramic substrate in the above-mentioned brazing step S210c are brazed using active metal brazing filler metal, which requires an additional screen printing process. Before brazing, the active metal brazing filler metal is evenly placed on the ceramic substrate. In addition to the above-mentioned main differences, the other processes and technical effects of the above-mentioned brazing step S210c using the "active metal brazing method" can be basically the same as the other processes and technical effects of the above-mentioned combined steps S210a and S210b using the "direct copper plating method". Therefore, the other specific processes of the above-mentioned brazing step S210c using the "active metal brazing method" can directly refer to the other processes and technical effects of the above-mentioned combined steps S210a and S210b, and will not be repeated here.

[0102] It can be seen that in some embodiments, since step S200 of the preparation method includes the above-mentioned brazing step S210c using the "active metal brazing method", and the "active metal brazing method" itself is very mature and can be easily adapted to large-scale production, and compared with the molybdenum-manganese process, this method is relatively simple and economical. Therefore, the cost of preparing the heating element assembly by the preparation method of the present application is lower.

[0103] It can be seen that in some embodiments, since the ceramic substrate obtained by the present preparation method is located between the heating element and the aerosol generating matrix, the heating element and the aerosol generating matrix are separated by the ceramic substrate as an outer shell to avoid direct contact between the heating element and the aerosol generating matrix, thereby preventing the strength of the heating element from being reduced and / or the heating element from falling off during repeated contact between the heating element and the aerosol generating matrix. That is, the above-mentioned ceramic substrate substantially protects the heating element, thereby improving the reliability and durability of the heating component obtained by the present preparation method.

[0104] The above is an explanation of a method for preparing a heating element assembly. Some embodiments of the present application also disclose a heating element assembly. The heating element assembly comprises: a heating element, which is used to generate heat by heating after being energized; a ceramic substrate, which is used to absorb at least part of the heat and heat the aerosol-forming matrix; wherein at least part of the heating element is connected to the ceramic substrate.

[0105] In some embodiments, the ceramic matrix may have a preset shape. The material of the ceramic matrix includes any one of the following: YSZ (yttria reinforced zirconia), ZTA (zirconia reinforced alumina), alumina or silicon nitride.

[0106] In some embodiments, the ceramic substrate may be in a two-dimensional planar structure, for example, the ceramic substrate may be in a rectangular shape, etc. At this time, the heating element may also be in a two-dimensional planar structure, for example, the heating element may also be in a rectangular shape, etc.

[0107] In some embodiments, the ceramic substrate may be a three-dimensional structure. For example, the ceramic substrate may be cylindrical or rectangular. For example, please refer to Figure 4 The top of the ceramic substrate 100 may be conical, and the ceramic substrate 100 other than the top may be cylindrical.

[0108] For some examples, please refer to Figure 5 , the ceramic substrate 100 has a cavity. The inner wall of the cavity has a certain degree of roughness. That is, at least a portion of the heating element is bonded to the inner wall of the cavity. The ceramic substrate 100 can be used to protect the heating element located in the cavity. Among them, the wall thickness of the ceramic substrate 100 is usually less than a preset wall thickness threshold. Those skilled in the art can determine the preset wall thickness threshold according to actual needs.

[0109] It should be noted that, in some embodiments, since the heating element in the heating element assembly must have a certain rigidity and a fixed shape, the heating element assembly can be repeatedly inserted into the aerosol-forming matrix in the atomization device and baked and atomized. Therefore, the roles of the above-mentioned ceramic matrix include: 1) giving the heating element a certain shape and rigidity so that the contact state and heat transfer state of the heating element in the atomization device are relatively stable; 2) the above-mentioned ceramic matrix acts as an outer shell, that is, it substantially protects and supports the heating element; 3) it buffers the heat released by the heating element, that is, it prevents the heating element from directly contacting the heating object of the heating needle and causing local over-baking or burning.

[0110] It should be noted that the person skilled in the art can determine the type of the aerosol-forming substrate according to actual needs. Since the specific types of aerosol-forming substrates are common knowledge in the art, the specific composition of the aerosol-forming substrate will not be described in detail.

[0111] In some embodiments, the heating element includes a first element; the first element is used to generate heat by heating after being energized.

[0112] In some embodiments, a partial area of ​​the first element can also serve as a first transition layer to connect the first element to the ceramic substrate. Figure 5 The heating element assembly 1 includes: a ceramic substrate 100, a heating element ( Figure 5 The heating element comprises only the first element 210; the first element 210 is connected to the surface of the ceramic base 100 which is away from the aerosol-forming substrate.

[0113] In some embodiments, a surface of one side of the ceramic substrate has a preset groove. At least a portion of the first element 210 can be bonded to the groove of the ceramic substrate by brazing or eutectic bonding.

[0114] For some examples, please refer to Figure 4 The heating element assembly 1 includes: a ceramic substrate 100, a heating element ( Figure 4 The heating element comprises a first element. One end of at least part of the first element is connected to the lead 300, and the lead 300 is used to connect to a power source. In other words, part of the first element or all of the first element is used as an electrode.

[0115] In some embodiments, the surface of the first element facing the ceramic substrate is blackened; and / or the surface of the first element away from the ceramic substrate has a smoothness greater than a preset smoothness threshold; and / or the surface of the first element facing the ceramic substrate has a flatness greater than a preset flatness threshold; and / or a hole of a preset shape is provided on the first element.

[0116] It should be noted that the purpose of blackening the surface of the first element facing the ceramic substrate is to form an oxide film on the surface of the first element facing the ceramic substrate, so as to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate, thereby improving the baking effect of the heating element. The principle of the blackening treatment is to oxidize the surface of the object to be blackened so that it forms a dense oxide film protective layer. The blackening treatment can adopt the existing alkaline heating blackening and room temperature blackening methods. The purpose of coating the surface of the first element facing the ceramic substrate is also to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate. Those skilled in the art can select the existing technology as the coating according to actual needs.

[0117] It should be noted that the purpose of "the smoothness of the surface of the first element away from the ceramic substrate is greater than a preset smoothness threshold" is to reduce the emissivity of thermal radiation generated by the surface of the first element away from the ceramic substrate. Specifically, existing technical means such as mechanical polishing, chemical polishing, electrolytic polishing or ultrasonic polishing can be used.

[0118] It should be noted that the purpose of "the flatness of the surface of the first element facing the ceramic substrate is greater than a preset flatness threshold" is also to increase the emissivity of thermal radiation generated by the surface of the first element facing the ceramic substrate. For example, the existing technology can be directly used.

[0119] It should be noted that the purpose of "providing a hole of a preset shape on the first element" is to adjust the resistance value of the first element and / or relieve the thermal stress on the first element according to actual needs. Punching or etching can be used to "provide a hole of a preset shape on the first element". Those skilled in the art can determine the "preset shape" according to actual needs. For example, the "preset shape" can be a rhombus; the "preset shape" can also be other shapes (such as a square, etc.).

[0120] Since the first element has poor heating performance after being energized if copper foil or an element with low resistivity is used as the first element, in some embodiments, an element with higher resistivity (such as an element with higher resistivity than copper foil) is used as the second element, and the second element is heated to generate heat after being energized. Figure 6 The heating element 200 includes a first element 210 and a second element 230; wherein the second element 230 is used to generate heat by heating after being energized; the first element 210 is used to connect the second element 230 to the ceramic substrate as a first transition layer; the resistivity of the second element 230 is greater than the resistivity of the first element 210. At least a portion of the first element 210 can be used as a first transition layer to connect the second element 230 to the ceramic substrate 100. For example, the second element 230 can be connected to a side surface of the ceramic substrate 100 away from the aerosol forming matrix. Please refer to Figure 7, a side surface of the ceramic substrate 100 has a groove of a preset shape. Among them, at least a part of the first element 210 is respectively bonded to the groove of the ceramic substrate 100 and a side surface of the second element 230 by eutectic bonding. At least one end of a part of the first element 210 is connected to a lead wire, which is used to connect to a power source. In other words, a part of the first element 210 or all of the first element 210 is used as an electrode.

[0121] In some embodiments, in order to further enhance the bonding force between the first element and the second element in step S200, an ultra-thin second transition layer that is easier to bond with the second element may be introduced between the first element and the second element. That is, the heating element includes a first element, a second transition layer, and a second element; wherein the second transition layer is disposed between the first element and the second element to enhance the bonding force between the first element and the second element; the thickness of the second transition layer is less than a preset thickness threshold; and the second transition layer contains elements in the first element and elements in the second element. For example, when the first element and the second element are copper foil and titanium foil, respectively, the second transition layer may be an ultra-thin copper-titanium alloy layer. The second transition layer contains elements in the first element and elements in the second element, that is, the specific material of the second transition layer is determined based on the elements in the first element and the elements in the second element. Those skilled in the art may determine the above-mentioned preset thickness threshold by themselves. The purpose of setting the thickness of the second transition layer to be less than the preset thickness threshold is also to make the thickness of the second transition layer relatively thin or within the preset thickness threshold.

[0122] In some embodiments, a partial area of ​​the first element can also serve as a first transition layer to connect the first element to the ceramic substrate. At least a partial area of ​​the first element can serve as a first transition layer to connect the second element to the ceramic substrate. The second element can be connected to a side surface of the ceramic substrate away from the aerosol forming matrix. One side surface of the ceramic substrate has a groove of a preset shape. Among them, at least a partial area of ​​the first element is respectively bonded to the groove of the ceramic substrate and a side surface of the second element by eutectic bonding. A lead is connected to one end of at least a portion of the first element, and the lead is used to connect to a power source. That is, a portion of the first element or all of the first element is used as an electrode.

[0123] In some embodiments, the surface of the second element facing the ceramic substrate is blackened or coated; and / or the surface of the second element facing the ceramic substrate has a smoothness greater than a preset smoothness threshold; and / or the surface of the first element and the second element facing the ceramic substrate has a flatness greater than a preset flatness threshold; and / or the second element is provided with holes of a preset shape; and / or at least a portion of the first element is arranged between the second element and the ceramic substrate in a preset manner.

[0124] In some embodiments, at least one end of a portion of the first elements is connected to a lead wire, and the lead wire is used to connect to a power source. In other words, a portion of the first elements or all of the first elements are used as electrodes.

[0125] It should be noted that the purpose of the above-mentioned "blackening treatment of the surface of the second element facing the ceramic substrate" is to form an oxide film on the surface of the first element facing the ceramic substrate, so as to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate, thereby improving the baking effect of the heating element. The principle of the blackening treatment is to oxidize the surface of the object to be blackened so that it forms a dense oxide film protective layer. The blackening treatment can adopt the existing alkaline heating blackening and room temperature blackening methods. The purpose of coating the surface of the second element facing the ceramic substrate is also to increase the emissivity of the thermal radiation generated by the surface of the first element facing the ceramic substrate, thereby improving the baking effect of the heating element. Those skilled in the art can select the existing technology as the coating according to actual needs.

[0126] It should be noted that the purpose of the above “the smoothness of the surface of the second element away from the ceramic substrate is greater than the preset smoothness threshold” is to reduce the emissivity of thermal radiation generated by the surface of the second element away from the ceramic substrate. Specifically, it can be performed by existing technical means such as mechanical polishing, chemical polishing, electrolytic polishing or ultrasonic polishing.

[0127] It should be noted that the purpose of the above-mentioned "the flatness of the surface of the first element and the second element facing the ceramic substrate is greater than the preset flatness threshold" is also to increase the emissivity of the thermal radiation generated by the surface of the first element and the second element facing the ceramic substrate. For example, the existing technology can be directly used for this purpose.

[0128] Please note that, please refer to Figure 8 A hole 231 of a preset shape is provided on the second element 230, the purpose of which is to adjust the resistance value of the second element 230 and / or relieve the thermal stress on the second element 230 according to actual needs. The hole of the preset shape can be provided on the second element 230 by punching or etching. The first element 210 is connected to the second element 230. Those skilled in the art can determine the "preset shape" according to actual needs. For example, the "preset shape" can be a rhombus; the "preset shape" can also be other shapes (such as a square, etc.).

[0129] It should be noted that the purpose of "arranging at least part of the first element between the second element and the ceramic substrate in a preset arrangement" is to optimize the tightness and uniformity of the second element and the ceramic substrate. Those skilled in the art can determine the preset arrangement according to actual needs. For example, please refer to Fig. 9, the first element 210a, which is not a part of the electrode, is arranged in a discrete matrix to optimize the second element 230 and the ceramic substrate ( Fig. 9 The first element 210b is used as an electrode.

[0130] In some embodiments, at least a portion of the heating element is connected to the ceramic substrate by brazing or eutectic bonding; wherein the first element includes one of copper foil, silver foil, silver-copper alloy foil, copper-aluminum alloy foil, aluminum bronze foil or copper-titanium alloy foil; the material of the ceramic substrate includes one of alumina ceramic, aluminum nitride ceramic, zirconium oxide toughened alumina ceramic or composite ceramic; the composite ceramic contains alumina.

[0131] In some embodiments, at least a portion of the heating element is connected to the ceramic substrate by brazing or eutectic bonding; wherein, when the ceramic substrate does not contain aluminum, a third transition layer is provided on the surface of the ceramic substrate facing the heating element; the third transition layer contains aluminum oxide.

[0132] In some embodiments, the material of the second element includes any one of titanium, iron-nickel alloy, austenitic stainless steel, constantan alloy, manganese-copper alloy, germanium-manganese-copper alloy, nickel-chromium alloy, iron-chromium-aluminum alloy or tungsten; wherein at least part of the first element is used as an electrode, and the electrode is used to connect to a power source. The austenitic stainless steel can be SUS904, SUS316 or SUS310s. The above SUS904, SUS316 or SUS310s are all existing models of austenitic stainless steel.

[0133] In some embodiments, at least a portion of the heating element is connected to the ceramic substrate by brazing, eutectic bonding or brazing.

[0134] In some embodiments, when the ceramic substrate does not contain aluminum, a third transition layer is sprayed or coated on the surface of the ceramic substrate facing the heating element in order to enhance the bonding force between the heating element and the ceramic substrate when the heating element is connected to the ceramic substrate, thereby making the heating element and the ceramic substrate more firmly connected. Preferably, the third transition layer contains aluminum oxide. For example, the third transition layer can directly use aluminum oxide material. The third transition layer can also contain a mixed ceramic layer of aluminum oxide. Those skilled in the art can determine the specific material of the third transition layer by themselves, as long as the third transition layer contains aluminum oxide.

[0135] It can be seen that in some embodiments, since the ceramic substrate in the heating element assembly of the present application is located between the heating element and the aerosol generating matrix, the heating element and the aerosol generating matrix are separated by the ceramic substrate as an outer shell to avoid direct contact between the heating element and the aerosol generating matrix, thereby preventing the strength of the heating element from being reduced and / or the heating element from falling off during repeated contact between the heating element and the aerosol generating matrix. That is, the above-mentioned ceramic substrate substantially protects the heating element, thereby improving the reliability and durability of the heating element assembly of the present application.

[0136] This document is described with reference to various exemplary embodiments. However, those skilled in the art will recognize that changes and modifications may be made to the exemplary embodiments without departing from the scope of this document. For example, various operating steps and components for performing the operating steps may be implemented in different ways (e.g., one or more steps may be deleted, modified, or incorporated into other steps) depending on the specific application or considering any number of cost functions associated with the operation of the system.

[0137] In the above embodiments, it can be implemented in whole or in part by software, hardware, firmware or any combination thereof. In addition, as understood by those skilled in the art, the principles of this article can be reflected in a computer program product on a computer-readable storage medium, which is pre-installed with a computer-readable program code. Any tangible, non-temporary computer-readable storage medium can be used, including magnetic storage devices (hard disks, floppy disks, etc.), optical storage devices (CD to ROM, DVD, Blu Ray disks, etc.), flash memory and / or the like. These computer program instructions can be loaded onto a general-purpose computer, a special-purpose computer or other programmable data processing device to form a machine, so that these instructions executed on a computer or other programmable data processing device can generate a device that implements a specified function. These computer program instructions can also be stored in a computer-readable memory, which can instruct a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer-readable memory can form a manufactured product, including an implementation device that implements a specified function. Computer program instructions can also be loaded onto a computer or other programmable data processing device, so that a series of operating steps are performed on a computer or other programmable device to generate a computer-implemented process, so that the instructions executed on a computer or other programmable device can provide steps for implementing a specified function.

[0138] Although the principles of this invention have been shown in various embodiments, many modifications of structures, arrangements, proportions, elements, materials and components particularly suitable for specific environments and operational requirements can be used without departing from the principles and scope of this invention. The above modifications and other changes or amendments will be included in the scope of this invention.

[0139] The foregoing specific description has been described with reference to various embodiments. However, those skilled in the art will recognize that various modifications and changes can be made without departing from the scope of the present disclosure. Therefore, the consideration of the present disclosure will be illustrative rather than restrictive, and all these modifications will be included in its scope. Similarly, the advantages, other advantages and solutions to the problems of various embodiments have been described above. However, the benefits, advantages, solutions to the problems and any elements that can produce these, or make them more clear, should not be interpreted as critical, necessary or necessary. The term "include" and any other variants used in this article are all non-exclusive inclusions, so that the process, method, article or device including the list of elements not only includes these elements, but also includes other elements that are not explicitly listed or do not belong to the process, method, system, article or device. In addition, the term "coupled" and any other variants used in this article refer to physical connections, electrical connections, magnetic connections, optical connections, communication connections, functional connections and / or any other connections.

[0140] Those skilled in the art will appreciate that many changes may be made to the details of the above-described embodiments without departing from the basic principles of the invention. Therefore, the scope of the present invention should be determined solely by the claims.

Claims

1. A method for preparing a heating element assembly, characterized in that: include: Obtain a ceramic matrix and a heating element; wherein the heating element is used to generate heat by heating after being energized; At least a portion of the surface of the heating element is bonded to the ceramic matrix to obtain a heating element assembly; wherein the ceramic matrix is ​​used to absorb at least a portion of the heat and heat the aerosol-forming matrix.

2. The preparation method according to claim 1, characterized in that The step of combining at least a portion of the surface of the heating element with the ceramic substrate to obtain the heating element assembly comprises: The step of bonding: heating the heating element and the ceramic substrate to a preset temperature, and bonding at least a portion of the heating element to the ceramic substrate by eutectic bonding; wherein the preset temperature is higher than a preset temperature threshold; The ceramic substrate and the heating element that have undergone the combining step are used as the heating element assembly.

3. The preparation method according to claim 1, characterized in that: The step of combining at least a portion of the heating element with the ceramic substrate to obtain the heating element assembly comprises: The step of combining: using a metal brazing material containing active elements to braze at least a portion of the heating element to a surface of one side of the ceramic substrate to obtain the heating element assembly; wherein the active element includes at least one of titanium, zirconium, hafnium and tantalum.

4. The preparation method according to claim 2 or 3, characterized in that: The heating element comprises a first element; the first element is used for heating and generating heat after being energized.

5. The preparation method according to claim 2 or 3, characterized in that: The heating element comprises a first element and a second element; Wherein, the second element is used for heating and generating heat after being energized; The first element is used as a first transition layer to connect the second element to the ceramic substrate; The resistivity of the second element is greater than the resistivity of the first element.

6. The preparation method according to claim 2 or 3, characterized in that: The heating element comprises a first element, a second transition layer and a second element; Among them, the second transition layer is arranged between the first element and the second element to enhance the bonding force between the first element and the second element; the thickness of the second transition layer is less than a preset thickness threshold; the second transition layer contains elements in the first element and elements in the second element.

7. The preparation method according to claim 5 or 6, characterized in that: The combined step S210b further includes: pre-treating the heating element; Wherein, the pre-processing of the heating element comprises: Performing a blackening treatment on the surface of the second element facing the ceramic substrate or applying a coating on the surface of the second element facing the ceramic substrate to increase the emissivity of thermal radiation generated by the surface of the second element facing the ceramic substrate; and / or, optimizing the smoothness of the surface of the second element on a side away from the ceramic substrate; and / or, optimizing the flatness of the surface of the first element and the second element on one side facing the ceramic substrate; and / or, providing a hole of a preset shape on the second element; And / or, at least part of the first elements are arranged between the second elements and the ceramic substrate in a preset arrangement.

8. The preparation method according to claim 4, characterized in that: The combining step further comprises: pre-treating the heating element; Wherein, the pre-processing of the heating element comprises: Performing a blackening treatment on the surface of the first element facing the ceramic substrate or applying a coating on the surface of the first element facing the ceramic substrate to increase the emissivity of thermal radiation generated by the surface of the first element facing the ceramic substrate; and / or, optimizing the smoothness of the surface of the first element on a side away from the ceramic substrate; and / or, optimizing the flatness of a surface of a side of the first element facing the ceramic substrate; And / or, a hole of a preset shape is provided on the first element.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The first element includes one of copper foil, silver foil, silver-copper alloy foil, copper-aluminum alloy foil, aluminum bronze foil or copper-titanium alloy foil; the material of the ceramic matrix includes one of alumina ceramic, aluminum nitride ceramic, zirconium oxide toughened alumina ceramic or composite ceramic; wherein the composite ceramic contains alumina.

10. The preparation method according to any one of claims 1 to 8, characterized in that: When the ceramic substrate does not contain aluminum, the step of combining at least a portion of the heating element with the ceramic substrate to obtain the heating element assembly further includes: Before the step of combining, a third transition layer is sprayed or covered on the surface of the ceramic substrate facing the heating element; wherein the third transition layer contains aluminum oxide.

11. The preparation method according to claim 5, 6 or 7, characterized in that: The material of the second element includes any one of titanium, iron-nickel alloy, austenitic stainless steel, constantan alloy, manganese-copper alloy, germanium-manganese-copper alloy, nickel-chromium alloy, iron-chromium-aluminum alloy or tungsten; At least part of the first element is used as an electrode, and the electrode is used to be connected to a power source.

12. A heating element assembly, characterized in that: include: A heating element, used for heating and generating heat after being energized; A ceramic matrix is ​​used to absorb at least part of the heat and heat the aerosol-forming matrix; wherein at least a part of the heating element is connected to the ceramic matrix.

13. The heating element assembly according to claim 12, characterized in that: The heating element comprises a first element; the first element is used for heating and generating heat after being energized.

14. The heating element assembly according to claim 13, characterized in that: The surface of the first element facing the ceramic substrate is blackened; and / or, the smoothness of a surface of a side of the first element away from the ceramic substrate is greater than a preset smoothness threshold; And / or, the flatness of a surface of a side of the first element facing the ceramic substrate is greater than a preset flatness threshold; And / or, a hole of a preset shape is arranged on the first element.

15. The heating element assembly according to claim 12, characterized in that: The heating element comprises a first element and a second element; The second element is used for heating and generating heat after being energized; the first element is used as a first transition layer to connect the second element to the ceramic substrate; and the resistivity of the second element is greater than that of the first element.

16. The heating element assembly according to claim 15, characterized in that: The heating element further comprises a second transition layer; Among them, the second transition layer is arranged between the first element and the second element to enhance the bonding force between the first element and the second element; the thickness of the second transition layer is less than a preset thickness threshold; the second transition layer contains elements in the first element and elements in the second element.

17. The heating element assembly according to claim 15 or 16, characterized in that: The surface of the second element facing the ceramic substrate is blackened or coated with a coating; And / or, the smoothness of the surface of the second element on a side away from the ceramic substrate is greater than a preset smoothness threshold; And / or, the flatness of the surface of the first element and the second element on one side facing the ceramic substrate is greater than a preset flatness threshold; And / or, the second element is provided with a hole of a preset shape; And / or, at least part of the first elements are arranged between the second elements and the ceramic substrate in a preset arrangement.

18. The heating element assembly according to claim 12, characterized in that: The ceramic matrix is ​​located between the heating element and the aerosol generating substrate.