Preparation method and application of hydrophobic modified natural plant powder

Through acidic solution pretreatment and silicone modification technology, the hydrophobicity of rosemary extract powder is improved, and the problem of its reduced stability in cosmetics is solved, and stable application and long-term storage in cosmetics are achieved.

CN118902873APending Publication Date: 2024-11-08SHANGHAI CO FUN BIOTECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411033067.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Rosemary extract powder has a lot of hydrophilic ingredients, which leads to its stability in cosmetics, which easily interacts with other ingredients, and has stratification or precipitation, which limits its application in cosmetics.

Method used

The natural plant powder is pretreated with an acid solution, the pH is adjusted to 2-4, and it is modified with a silicone treatment agent to increase the reaction site and contact area, making it hydrophobic.

Benefits of technology

Through surface treatment, natural plant powders have achieved excellent hydrophobicity, solving the problem of easy dissolution and group accumulation in water, and maintaining the long-term storage stability of the product and its application in cosmetics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method and application of hydrophobic modified natural plant powder, and relates to the technical field of cosmetic materials, the preparation method comprises the following steps: S1, weighing basic natural plant powder; s2, uniformly spraying an acidic solution on the natural plant powder, uniformly mixing, and adjusting the pH value of the natural plant powder to 2-4 to obtain the natural plant powder subjected to first treatment; s3, uniformly spraying an organic silicon treatment agent on the natural plant powder subjected to the first treatment, uniformly mixing, and modifying the natural plant powder subjected to the first treatment to obtain natural plant powder subjected to second treatment; and S4, drying the natural plant powder subjected to the second treatment to obtain the natural plant powder subjected to surface treatment. The hydrophobic modified natural plant powder provided by the invention can be applied to cosmetics and has relatively good hydrophobic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of cosmetic materials, and in particular to a preparation method and application of hydrophobically modified natural plant powder. Background Art

[0002] In modern society, science and technology have developed rapidly, which has greatly promoted the transformation of people's lifestyles and the improvement of living standards. In daily life, people not only pay attention to food, clothing, housing and transportation, but also pay more attention to skin management. Natural cosmetics are increasingly favored by consumers because of their gentle, effective and skin-friendly characteristics.

[0003] Rosemary, a perennial evergreen subshrub from the Mediterranean coast of North Africa and Europe, not only has a long history in the fields of cooking and medicine, but also has won a high reputation in the cosmetics industry. Rosemary leaves have a tea-like aroma, spicy and slightly bitter taste. This unique aroma makes rosemary a leader in cosmetic raw materials such as perfumes and soaps. Rosemary extract is also rich in a variety of biologically active ingredients, which gives it a variety of skin care effects in cosmetics, such as its strong antibacterial and anti-inflammatory effects, which can fight bacteria and dirt on the skin surface, thoroughly clean pores, and reduce the occurrence of acne and blackheads; rosemary extract is rich in polyphenols and vitamin E and other ingredients, which can effectively neutralize free radicals in cells and resist oxidative damage, thereby helping to slow down the aging process of the skin.

[0004] However, since rosemary extract has more hydrophilic chemical components, it has strong hydrophilicity. These hydrophilic components may cause the rosemary extract powder to interact with other ingredients in the formula, resulting in decreased product stability and the occurrence of stratification, precipitation and other phenomena, thereby greatly limiting its application in cosmetics. Summary of the invention

[0005] In order to improve the hydrophobicity of natural plant powder and overcome the problem that natural plant powder is easily soluble and agglomerated in water, the present application provides a preparation method and application of hydrophobically modified natural plant powder.

[0006] The present application provides a method for preparing a hydrophobically modified natural plant powder, which adopts the following technical scheme: A method for preparing hydrophobically modified natural plant powder comprises the following steps: S1. Weigh the basic natural plant powder; S2. The acidic solution is evenly sprayed on the natural plant powder and mixed evenly, and the pH value of the natural plant powder is adjusted to 2-4 to obtain a natural plant powder after the first treatment; S3. The organosilicon treatment agent is evenly sprayed on the first treated natural plant powder and mixed evenly, and the first treated natural plant powder is modified to obtain a second treated natural plant powder; S4. Drying the second treated natural plant powder to obtain surface treated natural plant powder.

[0007] By adopting the above technical scheme, the natural plant powder is pretreated with an acidic solution, and the pH of the natural plant powder is controlled within the range of 2-4, which can effectively activate the surface of the rosemary extract powder, expose more reaction sites, thereby increasing the contact area and reaction possibility with the organosilicon treatment agent; then the treated natural plant powder is hydrophobically modified with an organosilicon treatment agent, and the organosilicon treatment agent contains reactive functional groups such as silanol groups (Si-OH), which can react with hydroxyl groups (-OH) and other active groups on the surface of the natural plant powder, thereby effectively changing the surface properties of the natural plant powder and making it hydrophobic.

[0008] Preferably, the natural plant powder is rosemary extract powder.

[0009] Preferably, the mass ratio of the acidic solution to the basic natural plant powder is 1:4-6.

[0010] Preferably, the pH value of the acidic solution is 0.5-1.

[0011] Preferably, the acidic solution is an aqueous solution of hydrochloric acid or an alcoholic solution of hydrochloric acid.

[0012] Preferably, the mass of the organosilicon treatment agent is 4-6% of the natural plant powder.

[0013] Preferably, the organosilicon treatment agent is hydrogenated polydimethylsiloxane.

[0014] Preferably, the drying temperature in S4 is 105° C.-110° C., and the drying time is 2-3 h.

[0015] The present application also provides an application of hydrophobically modified natural plant powder, using the following technical solution: An application of hydrophobically modified natural plant powder, and an application of the hydrophobically modified natural plant powder in hydrophobic cosmetics.

[0016] By adopting the above technical scheme, the surface-treated natural plant powder provided in the present application is used as a raw material in hydrophobic cosmetics. The surface-treated natural plant powder has good hydrophobicity and good compatibility with other chemical ingredients, which is beneficial to the formula design of cosmetics.

[0017] In summary, the present application includes at least one of the following beneficial technical effects: 1. After being treated by the natural plant powder surface treatment method provided in this application, the surface of the natural plant powder has excellent hydrophobicity; 2. The surface treatment method of natural plant powder provided in this application overcomes the problem that natural plant powder is easily soluble in water and aggregates, and has long-term storage stability; 3. The surface treatment method of natural plant powder provided in this application maintains the characteristics of the natural plant powder itself, facilitating its use in cosmetics. DETAILED DESCRIPTION

[0018] The present application is further described in detail below in conjunction with embodiments. Example

[0019] Example 1 S1. Weigh 50g of natural plant powder rosemary extract powder; S2. Spray 10 g of an aqueous solution of hydrochloric acid having a pH value of 0.5 evenly on the rosemary extract powder, stir at high speed to mix evenly, adjust the pH value of the rosemary extract powder to 2-4, and obtain a natural plant powder after the first treatment; S3. Spray 2.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 85 ° C for 1.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0020] Example 2 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. The hydrochloric acid and ethanol solution were mixed to prepare a hydrochloric acid aqueous alcohol solution having a pH value of 0.5, and 2 g of the hydrochloric acid aqueous alcohol solution was evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder was adjusted to 2-3 to obtain a natural plant powder after the first treatment; S3. Spray 0.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0021] Example 3 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. Spray 2g of an aqueous solution of hydrochloric acid having a pH value of 0.5 evenly on the rosemary extract powder, stir at high speed to mix evenly, adjust the pH value of the rosemary extract powder to 2-3, and obtain a natural plant powder after the first treatment; S3. Spray 0.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0022] Example 4 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. Spray 2g of an aqueous solution of hydrochloric acid having a pH value of 1 evenly on the rosemary extract powder, stir at high speed to mix evenly, adjust the pH value of the rosemary extract powder to 2-4, and obtain a natural plant powder after the first treatment; S3. Spray 0.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0023] Example 5 S1. Weigh 50g of natural plant powder rosemary extract powder; S2. Spray 10 g of an aqueous solution of hydrochloric acid having a pH value of 0.5 evenly on the rosemary extract powder, stir at high speed to mix evenly, adjust the pH value of the rosemary extract powder to 2-4, and obtain a natural plant powder after the first treatment; S3. Spray 2.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 110° C. and dry for 2 hours to obtain surface treated natural plant powder.

[0024] Example 6 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. 2.5g of a hydrochloric acid solution having a pH value of 0.5 is evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder is adjusted to 3-4 to obtain a natural plant powder after the first treatment; S3. Spray 0.6 g of the organosilicon treatment agent hydrogenated polydimethylsiloxane evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 110° C. and dry for 2 hours to obtain surface treated natural plant powder.

[0025] Example 7 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. 2.5g of a hydrochloric acid solution having a pH value of 0.5 is evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder is adjusted to 3-4 to obtain a natural plant powder after the first treatment; S3. Spray 0.4 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 110° C. and dry for 2 hours to obtain surface treated natural plant powder.

[0026] Example 8 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. 2.5g of a hydrochloric acid solution having a pH value of 0.5 is evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder is adjusted to 3-4 to obtain a natural plant powder after the first treatment; S3. Spray 0.2 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 110° C. and dry for 2 hours to obtain surface treated natural plant powder.

[0027] Example 9 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. 2.5g of a hydrochloric acid solution having a pH value of 0.5 is evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder is adjusted to 3-4 to obtain a natural plant powder after the first treatment; S3. Spray 0.8 g of the organosilicon treatment agent hydrogenated polydimethylsiloxane evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 110° C. and dry for 2 hours to obtain surface treated natural plant powder.

[0028] Example 10 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. 2.5g of a hydrochloric acid solution having a pH value of 0.5 is evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder is adjusted to 2-3 to obtain a natural plant powder after the first treatment; S3. Spray 0.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0029] Embodiment 11 S1. Weigh 10 g of basic natural plant powder rosemary extract powder; S2. 1.7 g of a hydrochloric acid solution having a pH value of 0.5 is evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder is adjusted to 3-4 to obtain a natural plant powder after the first treatment; S3. Spray 0.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 75 ° C for 2.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0030] Example 12 S1. Weigh 150g of natural plant powder rosemary extract powder; S2. Spray 30 g of a 0.5 pH value of hydrochloric acid alcohol solution evenly on the rosemary extract powder, stir at high speed to mix evenly, adjust the pH value of the rosemary extract powder to 2-3, and obtain a natural plant powder after the first treatment; S3. Spray 7.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 85 ° C for 1.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0031] Comparative Example Comparative Example 1 S1. Weigh 50g of natural plant powder rosemary extract powder; S2. 6 g of a 0.5 pH aqueous solution of hydrochloric acid was evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder was adjusted to 4-5 to obtain a natural plant powder after the first treatment; S3. Spray 2.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 85 ° C for 1.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0032] Comparative Example 2 S1. Weigh 50g of natural plant powder rosemary extract powder; S2. 17 g of an aqueous solution of hydrochloric acid having a pH value of 0.5 is evenly sprayed on the rosemary extract powder, stirred at high speed to mix evenly, and the pH value of the rosemary extract powder is adjusted to 1-2 to obtain a natural plant powder after the first treatment; S3. Spray 2.5 g of an organosilicon treatment agent, hydrogenated polydimethylsiloxane, evenly on the first treated natural plant powder and mix evenly, modify the first treated natural plant powder at 85 ° C for 1.5 h to obtain a second treated natural plant powder; S4. Place the second treated natural plant powder in an oven at 105°C and dry for 3 hours to obtain surface treated natural plant powder.

[0033] Performance testing 1. The contact angles of the surface-treated natural plant powders obtained in Examples 1-12 and Comparative Examples 1-2 were tested, and the testing method was as follows: 0.3 g of each sample was weighed, and tablets were pressed using a YP-2 hydraulic tablet press, and the pressure was maintained at 20 MPa for 5 min, with a water droplet size of 10 μL. Then, a KJ.63-JJC-1 contact angle meter was used for measurement, and the tablets were pressed three times respectively, and the average value was taken as the final value. The results are shown in Table 1.

[0034] The specific test results are as follows: Table 1 Contact angle test results Contact angle (°) Contact angle (°) Example 1 124 Comparative Example 1 87 Example 2 118 Comparative Example 2 62 Example 3 115 Example 4 112 Example 5 123 Example 6 114 Example 7 110 Example 8 96 Example 9 110 Example 10 112 Embodiment 11 109 Example 12 106 It can be seen from the test results in Table 1 that the contact angle of the surface-treated natural plant powder provided in the present application can reach more than 100° after the surface hydrophobic modification, indicating that the hydrophobically modified natural plant powder has excellent hydrophobicity.

[0035] It can be seen from the test results of Examples 1-12 and Comparative Examples 1-2 that when the present application uses an acidic solution to pretreat the natural plant powder, when the pH value of the natural plant powder is between 2 and 4, the hydrophobicity of the natural plant powder can be more effectively improved. When the pH value of the natural plant powder is lower than or higher than 2-4, the contact angle of the surface-treated natural plant powder is significantly reduced.

[0036] It can be seen from the test results of Examples 6, 7, 8 and 9 that when the mass of the organosilicon treatment agent used in the preparation of the surface-treated natural plant powder in the present application is 4-6% of the natural plant powder, the hydrophobicity of the natural plant powder can be effectively improved. When the mass of the organosilicon treatment agent is lower than or higher than this range, the contact angle of the surface-treated natural plant powder becomes significantly smaller.

[0037] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing hydrophobically modified natural plant powder, characterized in that: The following steps are involved: S1. Weigh the basic natural plant powder; S2. The acidic solution is evenly sprayed on the natural plant powder and mixed evenly, and the pH value of the natural plant powder is adjusted to 2-4 to obtain a natural plant powder after the first treatment; S3. The organosilicon treatment agent is evenly sprayed on the first treated natural plant powder and mixed evenly, and the first treated natural plant powder is modified to obtain a second treated natural plant powder; S4. Drying the second treated natural plant powder to obtain surface treated natural plant powder.

2. The method for preparing a hydrophobically modified natural plant powder according to claim 1, characterized in that: The natural plant powder is rosemary extract powder.

3. The method for preparing a hydrophobically modified natural plant powder according to claim 1, characterized in that: The mass ratio of the acidic solution to the basic natural plant powder is 1:4-6.

4. A method for preparing a hydrophobically modified natural plant powder according to claim 1 or 3, characterized in that: The pH value of the acidic solution is 0.5-1.

5. A method for preparing a hydrophobically modified natural plant powder according to claim 1, 3 or 4, characterized in that: The acidic solution is an aqueous solution of hydrochloric acid or an alcoholic solution of hydrochloric acid.

6. The method for preparing a hydrophobically modified natural plant powder according to claim 1, characterized in that: The mass of the organosilicon treatment agent is 4-6% of the natural plant powder.

7. A method for preparing a hydrophobically modified natural plant powder according to claim 1 or 6, characterized in that: The organic silicon treating agent is hydrogenated polydimethylsiloxane.

8. The method for preparing a hydrophobically modified natural plant powder according to claim 1, characterized in that: The drying temperature in S4 is 105° C.-110° C.; the drying time is 2-3 hours.

9. The use of a hydrophobically modified natural plant powder according to any one of claims 1 to 8, characterized in that: Application of the hydrophobically modified natural plant powder in hydrophobic cosmetics.