Orthopedic implant for promoting repair and preparation method thereof
Print and modify titanium alloy orthopedic implants through SLM technology, and use the reaction of PDA and phosphate solution to form a titanium alloy bionic scaffold with osteoinductive activity, solving the problem of difficulty in integrating titanium alloy implants with bone tissue, significantly improving the problem of Its adhesion and repair effect in bone tissue.
Patent Information
- Application Number
- CN202411311591.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing titanium and titanium alloy orthopedic implants are difficult to integrate with the host bone tissue due to bioindifference and lack of osteogenic induction activity, resulting in poor shedding and repair results.
Ti6Al4V titanium alloy ball powder was printed using SLM technology, and through the reaction of PDA solution and Ca(NO3)2.4H2O and (NH4)2HPO4 solutions, a titanium alloy bionic scaffold with osteoinductive activity was formed to enhance its compatibility with bone tissue and Cell attachment ability.
It significantly improves the compatibility and cell adhesion of orthopedic implants with bone tissue, enhances the osteogenesis effect, has excellent osseobinding ability, and solves the problems of biological inertia and lack of osteogenesis inducing activity.
Smart Images

Figure CN118903539A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of orthopedic implants, and in particular to an orthopedic implant for promoting repair and a preparation method thereof. Background Art
[0002] As one of the largest and most important tissues and organs in the human body, bones bear vital life responsibilities, including supporting the body, protecting internal organs, and producing blood. Unfortunately, bone defects caused by trauma, tumors, or infections affect the health and quality of life of countless patients.
[0003] Existing titanium and titanium alloy orthopedic implants have the following disadvantages: 1) Biological inertness: titanium and titanium alloys are inert materials, difficult to integrate with host bone tissue, and easy to fall off; 2) No osteoinductive activity: titanium and titanium alloys only provide mechanical stress to promote cell osteogenic differentiation, and do not have osteoinductive activity themselves. Summary of the invention
[0004] The object of the present invention is to provide an orthopedic implant for promoting repair and a preparation method thereof.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing an orthopedic implant for promoting repair comprises the following steps:
[0007] S1, using SLM technology to print Ti6Al4V titanium alloy ball powder, wash it, and obtain a titanium alloy bionic scaffold;
[0008] S2, taking PDA powder and adding tris(hydroxymethyl)aminomethane solution to prepare PDA solution;
[0009] S3, taking the titanium alloy bionic stent and immersing it in the PDA solution, shaking it, washing it with ultrapure water, and drying it with nitrogen gas to obtain a spare stent;
[0010] S4, take Ca(NO3) 2. 4H2O is dissolved in deionized water to prepare Ca(NO3) 2. 4H2O solution; dissolve (NH4)2HPO4 in deionized water to prepare (NH4)2HPO4 solution; add the (NH4)2HPO4 solution to Ca(NO3) 2. 4H2O solution, and fully stirred, and the pH was adjusted to 8.5-10 with aqueous ammonia, and stirred to obtain a reaction kettle solution;
[0011] S5, placing the spare bracket and the reaction kettle solution in a reaction kettle, and reacting at 160-200° C. for 12-48 hours to obtain a primary finished product;
[0012] S6, washing the finished product alternately with water and ethanol for three times each, and drying at room temperature to obtain a finished orthopedic implant.
[0013] Furthermore, the concentration of the PDA solution in step S2 is 0.5-3 g / L.
[0014] Furthermore, the shaking in step S3 is performed at 4-37° C. and a shaking speed of 50-400 rpm for 24-72 hours.
[0015] Further, in step S4, Ca(NO3) 2. The concentration of the (NH4)2HPO4 solution is 0.8-1.2M; the concentration of the (NH4)2HPO4 solution is 0.8-1.2M; the (NH4)2HPO4 solution and Ca(NO3) are stirred thoroughly. 2. The mass ratio of 4H2O solution is 0.67-1.5.
[0016] Furthermore, the ethanol in step S6 is 75% ethanol.
[0017] Furthermore, the washing in step S1 is to use ultrapure water, n-hexane, 6M hydrochloric acid and 75% ethanol in sequence for 5 minutes each under ultrasound, and repeat the operation 3 times.
[0018] Furthermore, an orthopedic implant is prepared by any of the preparation methods described above.
[0019] Compared with the prior art, the orthopedic implant prepared by the present invention effectively improves its compatibility with bone tissue, promotes cell attachment and growth, thereby enhancing the osteogenesis effect, and has excellent bone bonding ability. The present invention solves the problem of biological inertness of titanium and titanium alloys, as well as the problem that titanium and titanium alloys themselves do not have osteoinductive activity.
[0020] Instruction Manual
[0021] Figure 1 Results of cell adhesion experiments.
[0022] Figure 2 This is the result of alkaline phosphatase (ALP) activity detection experiment.
[0023] Figure 3 Result graph of maximum thrust for animal experiments.
[0024] ****(P<0.0001), **(P<0.01); error bars indicate the standard deviation of three parallel measurements.
[0025] The unmodified orthopedic implant in the figure refers to the existing titanium alloy orthopedic implant; the modified orthopedic implant refers to the modified orthopedic implant prepared in Example 1, that is, the finished orthopedic implant of the present invention. DETAILED DESCRIPTION
[0026] The technical scheme of the present invention is further described below in conjunction with specific examples. It should be understood that the following examples are only exemplary descriptions and explanations of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0027] Example 1
[0028] The orthopedic implants are prepared as follows:
[0029] S1, taking Ti6Al4V titanium alloy ball powder, with a laser power of 220W, a scanning speed of 1200mm / s, a scanning interval of 0.12mm, a powder thickness of 30μm, and argon as a protective gas, SLM technology printing; the finished product after printing is washed in an ultrasonic machine with ultrapure water, n-hexane, 6M hydrochloric acid and 75% ethanol for 5min each, and the operation is repeated 3 times to obtain a finished titanium alloy bionic stent;
[0030] S2, taking PDA powder and adding tris(hydroxymethyl)aminomethane solution to prepare a 2 g / L PDA solution;
[0031] S3, taking a titanium alloy bionic stent and immersing it in a PDA solution, shaking it at 37°C and a shaking speed of 200 rpm for 24 hours, washing it with ultrapure water, and drying it with nitrogen gas to obtain a spare stent;
[0032] S4, take 7.88g Ca(NO3) 2. 4H2O was dissolved in 30mL of deionized water to prepare Ca(NO3) 2. 4H2O solution; dissolve 2.64g (NH4)2HPO4 in 20mL deionized water to prepare (NH4)2HPO4 solution; add the (NH4)2HPO4 solution to Ca(NO3) 2. 4H2O solution and fully stirred and adjusted the pH to 8.5-10 with aqueous ammonia, stirred for 5-30 minutes to obtain a reaction kettle solution;
[0033] S5, placing the spare bracket and the reaction kettle solution in a reaction kettle, and reacting at 160-200° C. for 12-48 hours to obtain a primary finished product;
[0034] S6, washing the finished product alternately with water and 75% ethanol for three times each, and drying at room temperature to obtain a modified orthopedic implant.
[0035] 1. The modified orthopedic implant prepared in Example 1 was subjected to an in vitro cytotoxicity test to evaluate the biosafety of the biomimetic scaffold according to the methods specified in the national standards GB / T16886.5 and ISO10993-5:
[0036] According to the national technical standard GB / T 16886.5, the toxicity evaluation standard is graded according to the relative proliferation rate of cells. The toxicity evaluation of the modified orthopedic implant is grade 0, which means it is not cytotoxic.
[0037] According to the requirements of ISO 10993-5, the cell viability of MC3T3-E1 cells cultured in the biomimetic scaffold extract was determined using the CCK-8 method, and the cell viability was greater than 100%.
[0038] In summary, the modified orthopedic implants are safe and have good biocompatibility.
[0039] 2. The adhesion of cells on the scaffold surface affects the ability of cell proliferation and differentiation, and may also affect the ingrowth of bone tissue inside the scaffold. In order to observe the adhesion effect of cells on the surface of each group of bionic scaffolds, the cells were stained with phalloidin (green, cytoskeleton) and DAPI (blue, cell nucleus), and the growth state of cells on the surface of bionic scaffolds was observed by fluorescent staining:
[0040] Results Figure 1 Compared with the unmodified orthopedic implant, the modified orthopedic implant of the present invention has more pseudopodia on the surface and a more obvious skeleton. In summary, the present invention improves cell adhesion.
[0041] 3. The higher the ALP expression level, the higher the osteogenic activity. The quantitative analysis of ALP activity can be used to evaluate the effect of bionic scaffolds on the osteogenic differentiation ability of MC3T3-E1 cells:
[0042] Results Figure 2 Compared with the unmodified orthopedic implant, the modified orthopedic implant of the present invention has higher ALP activity. The present invention helps to promote the differentiation of bone cells and has osteoinductive activity.
[0043] 4. Animal experiment, through mechanical push-out experiment to detect the degree of integration of bionic scaffolds with host bone tissue after implantation in vivo:
[0044] Twenty-four SD rats were randomly divided into three groups: a blank group (only bone defect surgery, no orthopedic implants), a control group (surgery + unmodified orthopedic implants), and an experimental group (surgery + modified orthopedic implants), with 8 rats in each group. SD rats were anesthetized by intraperitoneal injection of sodium pentobarbital (50 mg / kg), and the rats were placed in a supine position with their limbs fixed. The hair near the right knee joint of the SD rats was shaved, and the skin was disinfected with iodine disinfectant. After the skin was prepared in the surgical area, a longitudinal incision of about 1 cm was made in the middle of the knee joint, and then the skin, synovium and capsule at the knee joint were separated layer by layer to expose the medial femoral condyle. A pre-sterilized cobalt alloy drill with a diameter of 3 mm was used to drill a hole on the medial side of the femoral condyle to form a bone defect with a diameter of 3 mm and a depth of 3.5 mm. The femoral bone defect model of SD rats was established.
[0045] Each group of implants was implanted into the defect position to complete the repair of the bone defect. After confirming the stability of the implant, it was rinsed with sterile saline, and then the muscle was sutured with 6-0 absorbable catgut and the skin was sutured with 4-0 non-absorbable sutures. After the suturing was completed, each rat was injected with 0.8mL (100,000 U / mL) of veterinary penicillin into the gluteus maximus muscle to prevent infection, and the injection was continued for 3 days. At 4 and 8 weeks of the experiment, 4 rats were randomly selected from each group, and the SD rats were killed by injecting an overdose of anesthetics and the samples were collected. The tissue of the removed joint was peeled clean, washed with saline until bloodless, and fixed in 4% paraformaldehyde for subsequent experiments.
[0046] The femoral surface was trimmed using a micro electric grinder to form a rectangle with only the middle bone defect left. At room temperature, a nut (with an inner diameter greater than 3 mm) was placed in the center of the workbench of the electronic universal testing machine; then, the femoral sample was placed parallel to the nut, and a 3 mm diameter push rod fixed to the electronic universal testing machine was used to slowly push down the scaffold implanted inside the bone defect at a speed of 1 mm / min. The maximum push force recorded during the experiment was the bonding strength between the bionic scaffold and the host bone tissue.
[0047] Results Figure 3 As the implantation time increases, the stress required to push out the implant increases. Compared with the unmodified orthopedic implant, the modified orthopedic implant of the present invention has a more excellent bone bonding ability. The present invention can further improve the bone tissue ingrowth ability.
[0048] Although the specific implementation modes of the present invention are described above, those skilled in the art should understand that the specific implementation modes described are only illustrative and are not intended to limit the scope of the present invention. Any modifications and changes made by those skilled in the art in accordance with the spirit of the present invention should be included in the scope of protection of the claims of the present invention.
Claims
1. A method for preparing an orthopedic implant that promotes repair, characterized in that: The following steps are involved: S1, using SLM technology to print Ti6Al4V titanium alloy ball powder, wash it, and obtain a titanium alloy bionic scaffold; S2, taking PDA powder and adding tris(hydroxymethyl)aminomethane solution to prepare PDA solution; S3, taking the titanium alloy bionic stent and immersing it in the PDA solution, shaking it, washing it with ultrapure water, and drying it with nitrogen gas to obtain a spare stent; S4, take Ca(NO3) 2. 4H2O is dissolved in deionized water to prepare Ca(NO3) 2. 4H2O solution; dissolve (NH4)2HPO4 in deionized water to prepare (NH4)2HPO4 solution; add the (NH4)2HPO4 solution to Ca(NO3) 2. 4H2O solution, and fully stirred, and the pH was adjusted to 8.5-10 with aqueous ammonia, and stirred to obtain a reaction kettle solution; S5, placing the spare bracket and the reaction kettle solution in a reaction kettle, and reacting at 160-200° C. for 12-48 hours to obtain a primary finished product; S6, washing the finished product alternately with water and ethanol for three times each, and drying at room temperature to obtain a finished orthopedic implant.
2. The method for preparing a repair-promoting orthopedic implant according to claim 1, characterized in that: The concentration of the PDA solution in step S2 is 0.5-3 g / L.
3. The method for preparing a repair-promoting orthopedic implant according to claim 1, characterized in that: The shaking in step S3 is performed at 4-37° C. and a shaking speed of 50-400 rpm for 24-72 hours.
4. The method for preparing a repair-promoting orthopedic implant according to claim 1, characterized in that: Step S4 Ca(NO3) 2. The concentration of the (NH4)2HPO4 solution is 0.8-1.2M; the concentration of the (NH4)2HPO4 solution is 0.8-1.2M; the (NH4)2HPO4 solution and Ca(NO3) are stirred thoroughly.
2. The mass ratio of 4H2O solution is 0.67-1.
5.
5. The method for preparing a repair-promoting orthopedic implant according to claim 1, characterized in that: The ethanol in step S6 is 75% ethanol.
6. The method for preparing a repair-promoting orthopedic implant according to claim 1, characterized in that: The washing in step S1 is to use ultrapure water, n-hexane, 6M hydrochloric acid and 75% ethanol in sequence under ultrasound for 5 minutes each, and repeat the operation 3 times.
7. An orthopedic implant obtained by the preparation method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method of titanium alloy material with good biocompatibility and antibacterial function coating
CN110115777A
Bioactivity improvement method and application of bone trabecular structure-imitated titanium alloy stent
CN114344562A
Preparation and experiment method of medical bionic plasma titanium alloy orthopedic implant
CN115212347A
Nano-drug carrier for promoting defective bone regeneration based on piezoelectric effect as well as preparation method and application of nano-drug carrier
CN117717622A
Surface-modified implant using titanium nanotube and dopamine coating and preparing method thereof