Composite stent for rotator cuff repair and preparation method thereof
By using a composite scaffold of braided sheets and braided threads in rotator cuff repair, combining porous natural polymer coating and nano-hydroxyapatite, the problem of coordinated repair of tendons and bone tracts is solved, and efficient healing and mechanical of rotator cuffs is achieved. stability.
Patent Information
- Application Number
- CN202410336779.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing rotator cuff repair technology, tendon generation and bone tract cannot be repaired in concert, resulting in unsatisfactory healing effect after rotator cuff injury, especially in the case of large-scale tear and tissue contracture.
Design a composite bracket, including braided sheets and braided lines made through the braided sheet, the surface of which is degradable porous natural polymer coating, the nano-hydroxyapatite content on the braided line is high, and it forms a sponge through freeze-drying process. Coating to promote the coordinated repair of tendons and bone tracts.
The tight bond between the rotator cuff and the humeral head is achieved, the healing process is accelerated, the shear damage of polymer silk to native tissue is reduced, the tissue is promoted better and faster reconstruction, and the tissue is provided with high initial fixation strength and mechanical stability.
Smart Images

Figure CN118903543A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of medical devices, and in particular to a composite bracket for rotator cuff repair and a preparation method thereof. Background Art
[0002] Rotator cuff injury is a common injury of the shoulder joint. Factors such as decreased rotator cuff quality, subacromial impingement and trauma can cause rotator cuff injury, which seriously affects the patient's quality of life. Literature reports that the prevalence rate is 13% in people aged 50-59, 20%-30% in people aged 60-80, and more than 50% in people over 80 years old. Among them, giant rotator cuff tears account for about 40% of all rotator cuff tears. If active treatment is not received after the injury, as the disease progresses and tissue degenerates, it will eventually develop into an irreparable tear.
[0003] The tendon is the weak point in the rotator cuff repair process, especially when the defect is large, it is difficult to fix the torn rotator cuff tissue back to the original attachment point. Currently, the commonly used rotator cuff injury repair techniques in clinical practice include single / double-row wire anchor transbone suture technology, and the technology of repairing the rotator cuff by transferring tendons, such as pectoralis major transfer technology and latissimus dorsi transfer technology. However, some rotator cuffs cannot be repaired due to huge tears and tissue contracture. When the patient has anterior-superior instability in the shoulder joint or a huge rotator cuff injury, the effect is not ideal in terms of pain or function.
[0004] Currently, drugs or porous, sponge-like natural polymer coatings are added around the patch to promote body growth. The natural polymer coating has a weak bonding force with the patch, and there is no strong bonding force generated directly on the patch by the natural polymer coating.
[0005] With the development of arthroscopic technology, patch technology provides a new solution for rotator cuff re-tear after suture surgery. The polymer braided patch has a high initial fixation strength, which can reach the initial strength of the rotator cuff and can still maintain mechanical stability after repeated activities. However, patch fixation usually requires the use of transbone suture technology. There are certain differences in histological characteristics between artificial patches and host bones. The patch itself lacks bone conductivity and cannot stimulate bone canal healing, resulting in graft-bone healing disorders, severe bone canal enlargement, and difficulty in autogenization of materials in the bone canal. Therefore, the design of a new type of bone and soft tissue integrated scaffold is of extremely important clinical significance.
[0006] In view of the above problems, it is necessary to improve the existing patch structure, precisely design and integrate its structure, and prepare an integrated bone and soft tissue scaffold to achieve coordinated repair of soft tissue and bone. Summary of the invention
[0007] In order to solve the problems in the above-mentioned background technology, the present invention provides a composite stent for rotator cuff repair, which solves the problem in the prior art that tendon generation and bone tunnel cannot be repaired in coordination during rotator cuff repair.
[0008] The solution adopted by the present invention to solve its technical problem is: a composite stent for rotator cuff repair, including a woven sheet and a woven wire. The woven sheet is made by a woven process and is in the shape of a sheet. One or more woven wires made by a woven process are respectively arranged at both ends of the woven sheet. One end of the woven wire is connected to one end of the woven sheet, and the other end is placed freely. The woven wires at both ends of the woven sheet are arranged on the same side of the woven sheet. The surfaces of the woven sheet and the woven wire are provided with a degradable natural polymer coating. The natural polymer coating is formed by attaching natural polymers in a natural polymer solution to the woven sheet and the woven wire through a freeze-drying process. The natural polymer solution is a solution formed by dissolving natural polymers in physiological saline. The natural polymer coating is porous.
[0009] Furthermore, the natural polymer includes animal-derived collagen and / or recombinant collagen and / or gelatin and / or chitosan and / or silk fibroin, and the woven sheet is prepared from a non-degradable polymer substrate through a weaving process, and the polymer substrate includes polyethylene terephthalate and / or polypropylene and / or polyethylene and / or polydioxanone and / or polydioxanone and / or polycaprolactone and / or poly-L-lactide and / or polyglycolic acid.
[0010] Furthermore, the thickness of the woven sheet is 0.08-3.0 mm, and the diameter of the polymer substrate in the woven sheet 1 is 0.025-1 mm.
[0011] Furthermore, the natural polymer solution used to soak the braided wire contains nano-hydroxyapatite.
[0012] Furthermore, a plurality of braided wires are arranged at one end of the braided sheet, and the distance between two adjacent braided wires among the plurality of braided wires is between 0.1-3 cm.
[0013] Furthermore, the yarn diameter of the braided wire is 0.025-1 mm; the thickness of the braided wire is 0.08-3 mm; the width of the braided wire is 0.08-3 mm; and the length of the braided wire 2 is 2-15 cm.
[0014] Furthermore, the natural polymer coating is biodegradable.
[0015] Furthermore, the weaving process is warp knitting or weft knitting.
[0016] Further, the coating on the braided wire is connected to the coating on the braided sheet, and the coating on the braided wire is disconnected from the coating on another braided wire so that the braided wires pass through different bone holes respectively.
[0017] Furthermore, the polymer substrate is polyethylene terephthalate, and the natural polymer is collagen.
[0018] A method for preparing a composite stent comprises the following steps:
[0019] 1. Connect, connect one end of the braided sheet with one end of multiple braided wires;
[0020] 2. Soaking, soaking the braided sheet and the braided wire in a freezing device, the braided sheet is placed in a braided sheet freezing tank, each braided wire is placed in a braided wire freezing tank, and then the braided sheet and the braided wire are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire contains nano-hydroxyapatite, the concentration of the natural polymer is 0.01-1 mg / mL, the upper surface of the braided sheet or the braided wire is 0.01-2 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet or the braided wire is 0.01-3 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet or the braided wire is 0.01-1 mm away from the interface of the collagen solution, the braided sheet or the braided wire soaking time is 0.1-60 min, the braided sheet or the braided wire soaking temperature is 0-40° C., and the distance between two adjacent braided wires in the multiple braided wires is 0.1-3 cm;
[0021] 3. Preliminary freezing: freeze-dry the braided sheets and braided wires in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15-60min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0022] 4. Freeze drying: After freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze-dry for 24-72 hours, freeze-dry until completely dry. The natural polymer in the natural polymer solution adheres to the woven sheets and woven wires to form a natural polymer coating.
[0023] Furthermore, the concentration of natural polymer is 0.3-0.6 mg / mL, the upper surface of the woven sheet or woven wire is 0.2-0.6 mm away from the upper interface of the natural polymer solution, the lower surface of the woven sheet or woven wire is 0.4-2 mm away from the lower interface of the natural polymer solution, the four sides of the woven sheet or woven wire are 0.2-0.6 mm away from the interface of the collagen solution, the immersion time of the woven sheet or woven wire is 0.1-20 min, and the immersion temperature of the woven sheet or woven wire is 25-35°C.
[0024] A freezing device includes a freezing tank and a partition. The freezing tank is provided with two large partitions to divide the freezing tank into a woven sheet freezing tank and a plurality of woven wire freezing tanks. The large partitions are provided with a plurality of woven wire through holes for the woven wires to pass through. The woven wire freezing tank is provided with a plurality of small partitions to divide the woven wire freezing tank into a plurality of independent freezing units to prevent the natural polymer coatings on the woven wires from being connected to each other. The partition is placed on the large partitions to prevent the natural polymer solution from flowing between the woven sheet freezing tank and the woven wire freezing tank.
[0025] Furthermore, a method for preparing a composite scaffold comprises the following steps:
[0026] 1. Connect, connect one end of the braided sheet with one end of multiple braided wires;
[0027] 2. Soaking, soaking the braided sheet and the braided wire in a freezing device, the braided sheet is placed in a braided sheet freezing tank, each braided wire is placed in a braided wire freezing tank, and then the braided sheet and the braided wire are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire contains nano-hydroxyapatite, the natural polymer concentration is 0.5 mg / mL, the thickness of the braided sheet is 0.9 mm, the thickness and width of the braided wire are both 0.6 mm, the content of nano-hydroxyapatite is 20% of the collagen, the upper surface of the braided sheet or the braided wire is 0.6 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet or the braided wire is 1.0 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet or the braided wire is 0.5 mm away from the interface of the collagen solution, the braided sheet or the braided wire is soaked for 10 min, the braided sheet or the braided wire is soaked at 25° C., and the distance between two adjacent braided wires 2 in the multiple braided wires is 1.0 cm;
[0028] 3. Preliminary freezing: freeze-dry the braided sheets and braided wires in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0029] 4. Freeze drying: After freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze dry for 48 hours, and freeze dry until completely dry. The natural polymer in the natural polymer solution adheres to the woven sheets and woven wires to form a natural polymer coating.
[0030] In summary, the beneficial effects of the present invention are as follows: by arranging the braided wire on the braided sheet, the braided wire can be connected to the bone through the hole on the bone, so that the tendon is easier to generate, and the generated tendon is not easy to be strained. At the same time, the natural polymer solution soaked with the braided wire contains nano-hydroxyapatite, which can stimulate the repair of the bone channel and realize the coordinated repair of the tendon and the bone channel. By adopting the freeze-drying process, the water molecules in the natural polymer solution form ice crystals and then sublimate, and the remaining natural polymer forms a porous, sponge-like natural polymer coating, and the porosity of the composite scaffold is 50-90%; due to the porous structure of the coating, the hole structure is conducive to cell adhesion and growth, so that the human body's own tissue growth is easier to enter the micropores of the natural polymer coating, and the composite scaffold is easier to make the rotator cuff and the humeral head tightly combined, and it is easier to form an overall structure, accelerate the healing of the rotator cuff, the natural polymer coating and the braided sheet or braided wire have a large bonding area and strong bonding strength. At the same time, the sponge-like porous structure of the natural polymer coating can reduce the shear damage of the polymer silk thread shear force on the braided sheet or braided wire to the native tissue, thereby promoting better and faster reconstruction of the tissue.
[0031] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a structural diagram of the present invention;
[0033] Figure 2 is a three-dimensional diagram of a freezing tank of the present invention;
[0034] Figure 3 is an exploded view of the freezing tank of the present invention;
[0035] Figure 4 The figure is a comparative bar graph of the experimental examples of the present invention.
[0036] In the figure: 1. woven sheet; 2. woven wire; 3. natural polymer coating; 4. freezing tank; 5. partition; 6. large partition bone; 7. small partition bone; 8. woven wire through hole; 9. woven wire freezing tank; 10. woven sheet freezing tank. DETAILED DESCRIPTION
[0037] In order to make the content of the present invention more clearly understood, the present invention is further described below based on specific embodiments in conjunction with the accompanying drawings.
[0038] It should be noted that the terms "center", "upper", "lower", "front", "back", "left", "right", "inner", "outer" and the like used herein to indicate directions or positional relationships are based on directions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention. Unless otherwise specified, "plurality" means two or more.
[0039] Unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0040] Referring to the accompanying drawings, a composite stent for rotator cuff repair includes a woven sheet 1 and a woven wire 2. The woven sheet 1 is made by a woven process and is in the shape of a sheet. One or more woven wires 2 made by a woven process are respectively arranged at both ends of the woven sheet 1. One end of the woven wire 2 is connected to one end of the woven sheet 1, and the other end is placed freely. The woven wires 2 at both ends of the woven sheet 1 are arranged on the same side of the woven sheet 1. The surfaces of the woven sheet 1 and the woven wire 2 are provided with a degradable natural polymer coating 3. The natural polymer coating 3 is formed by attaching natural polymers in a natural polymer solution to the woven sheet 1 and the woven wire 2 through a freeze-drying process. The natural polymer solution is a solution formed by dissolving natural polymers in physiological saline. The natural polymer coating 3 is porous.
[0041] Furthermore, the natural polymer includes animal-derived collagen and / or recombinant collagen and / or gelatin and / or chitosan and / or silk fibroin, and the woven sheet 1 is prepared from a non-degradable polymer substrate through a weaving process, and the polymer substrate includes polyethylene terephthalate and / or polypropylene and / or polyethylene and / or polydioxanone and / or polydioxanone and / or polycaprolactone and / or poly-L-lactide and / or polyglycolic acid.
[0042] Furthermore, the thickness of the woven sheet 1 is 0.08-3.0 mm, preferably 0.6-1.2 mm, and the diameter of the polymer substrate in the woven sheet 1 is 0.025-1 mm, preferably 0.025-0.4 mm.
[0043] Furthermore, the natural polymer solution used to soak the braided wire 2 contains nano-hydroxyapatite.
[0044] Furthermore, the coating on the braided wire 2 is connected to the coating on the braided sheet 1, and the coating on the braided wire 2 is disconnected from the coating on another braided wire 2 so that the braided wires 2 pass through different bone holes respectively.
[0045] Furthermore, a plurality of braided wires 2 are provided at one end of the braided sheet 1, and a distance between two adjacent braided wires 2 among the plurality of braided wires 2 is between 0.1-3 cm, preferably, 0.5-1.5 cm.
[0046] Furthermore, the yarn diameter of the braided wire 2 is 0.025-1mm, preferably 0.025-0.4mm; the thickness of the braided wire 2 is 0.08-3mm, preferably 0.08-1.2mm; the width of the braided wire 2 is 0.08-3mm, preferably 0.08-1.2mm; preferably, the length of the braided wire 2 is 2-15cm.
[0047] Furthermore, the natural polymer coating 3 is degradable.
[0048] Furthermore, the weaving process is warp knitting or weft knitting.
[0049] Furthermore, the polymer substrate is polyethylene terephthalate, the natural polymer is collagen, and the collagen refers to animal-derived collagen or recombinant collagen.
[0050] A freezing device includes a freezing tank 4 and a partition 5. The freezing tank 4 is provided with two large partitions 6 to divide the freezing tank 4 into a woven sheet freezing tank 10 and a plurality of woven wire freezing tanks 9. The large partitions 6 are provided with a plurality of woven wire through holes 8 for the woven wires 2 to pass through. The woven wire freezing tank 9 is provided with a plurality of small partitions 6 to divide the woven wire freezing tank 9 into a plurality of independent freezing units to prevent the natural polymer coatings 3 on the woven wires from being connected to each other. The partition 5 is placed on the large partitions 6 to prevent the natural polymer solution from flowing between the woven sheet freezing tank 10 and the woven wire freezing tank 9. The woven sheet 1 is placed in the woven sheet freezing tank 10, and each woven wire 2 is placed in the woven wire freezing tank 9 separately. At this time, the natural polymer solution in the woven sheet freezing tank 10 and the natural polymer solution in the woven wire freezing tank 9 have different components.
[0051] A method for preparing a composite stent:
[0052] 1. Connecting: connecting one end of the braided sheet 1 with one end of the plurality of braided wires 2;
[0053] 2. Soaking, soaking the braided sheet 1 and the braided wire 2 in a freezing device, the braided sheet 1 is placed in the braided sheet freezing tank 10, each braided wire 2 is placed in the braided wire freezing tank 9, and then the braided sheet 1 and the braided wire 2 are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire 2 contains nano-hydroxyapatite, the natural polymer concentration is 0.01-1 mg / mL, the upper surface of the braided sheet 1 or the braided wire 2 is 0.01-2 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet 1 or the braided wire 2 is 0.01-3 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet 1 or the braided wire 2 is 0.01-1 mm away from the interface of the collagen solution, the braided sheet 1 or the braided wire 2 is soaked for 0.1-60 min, the braided sheet 1 or the braided wire 2 is soaked at a temperature of 0-40°C, and the distance between two adjacent braided wires 2 in multiple braided wires 2 is 0.1-3 cm;
[0054] 3. Preliminary freezing: freeze-dry the braided sheet 1 and braided wire 2 in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15-60min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0055] 4. Freeze drying, after freezing for 2 hours, cool down to -50°C at a cooling rate of 2°C / min, freeze drying for 24h-72h, freeze drying until completely dry, the natural polymer in the natural polymer solution adheres to the woven sheet 1 and the woven wire 2 to form a natural polymer coating 3.
[0056] Furthermore, the concentration of natural polymer is 0.3-0.6 mg / mL, the upper surface of the woven sheet 1 or the woven wire 2 is 0.2-0.6 mm away from the upper interface of the natural polymer solution, the lower surface of the woven sheet 1 or the woven wire 2 is 0.4-2 mm away from the lower interface of the natural polymer solution, the surrounding of the woven sheet 1 or the woven wire 2 is 0.2-0.6 mm away from the interface of the collagen solution, the immersion time of the woven sheet 1 or the woven wire 2 is 0.1-20 min, and the immersion temperature of the woven sheet 1 or the woven wire 2 is 25-35°C.
[0057] Furthermore, the thickness of the woven sheet 1 is 0.08-3 mm, and the ultimate tensile load of the woven sheet 1 is 200-1000N.
[0058] Furthermore, the thickness of the woven sheet 1 is 0.6-1.2 mm, and the ultimate tensile load of the woven sheet 1 is 500-800N.
[0059] Five embodiments and comparative examples are formulated according to the invention content, and the comparison results of several key performances are given below:
[0060] Embodiment 1: A method for manufacturing a braided sheet 1 and a braided wire 2 using polyethylene terephthalate wire with a diameter of 0.025 mm:
[0061] 1. Connecting: connecting one end of the braided sheet 1 with one end of the plurality of braided wires 2;
[0062] 2. Soaking, soaking the braided sheet 1 and the braided wire 2 in a freezing device, the braided sheet 1 is placed in the braided sheet freezing tank 10, and each braided wire 2 is placed in the braided wire freezing tank 9, and then the braided sheet 1 and the braided wire 2 are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire 2 contains nano-hydroxyapatite, the natural polymer concentration is 0.01 mg / mL, the thickness of the braided sheet 1 is 0.08 mm, the thickness and width of the braided wire 2 are both 0.08 mm, and the nano-hydroxyapatite The content of stone is 0.5% of collagen, the upper surface of the woven sheet 1 or the woven wire 2 is 0.01mm away from the upper interface of the natural polymer solution, the lower surface of the woven sheet 1 or the woven wire 2 is 0.01mm away from the lower interface of the natural polymer solution, the surrounding of the woven sheet 1 or the woven wire 2 is 0.5mm away from the interface of the collagen solution, the immersion time of the woven sheet 1 or the woven wire 2 is 20min, the immersion temperature of the woven sheet 1 or the woven wire 2 is 4°C, and the distance between two adjacent woven wires 2 in the multiple woven wires 2 is 0.1cm;
[0063] 3. Preliminary freezing: freeze-dry the braided sheet 1 and braided wire 2 in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0064] 4. Freeze drying, after freezing for 2 hours, cool down to -50°C at a cooling rate of 2°C / min, freeze dry for 24 hours, freeze dry until completely dry, the natural polymer in the natural polymer solution adheres to the woven sheet 1 and the woven wire 2 to form a natural polymer coating 3.
[0065] Embodiment 2: A method for preparing a composite stent using polyethylene terephthalate wire with a diameter of 0.2 mm to manufacture a braided sheet 1 and a braided wire 2:
[0066] 1. Connecting: connecting one end of the braided sheet 1 with one end of the plurality of braided wires 2;
[0067] 2. Soaking, soaking the braided sheet 1 and the braided wire 2 in a freezing device, the braided sheet 1 is placed in the braided sheet freezing tank 10, each braided wire 2 is placed in the braided wire freezing tank 9 separately, and then the braided sheet 1 and the braided wire 2 are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire 2 contains nano-hydroxyapatite, the natural polymer concentration is 0.3 mg / mL, the thickness of the braided sheet 1 is 0.6 mm, the thickness and width of the braided wire 2 are both 0.3 mm, the content of nano-hydroxyapatite is 5% of the collagen, the upper surface of the braided sheet 1 or the braided wire 2 is 0.2 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet 1 or the braided wire 2 is 0.4 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet 1 or the braided wire 2 is 0.5 mm away from the interface of the collagen solution, the braided sheet 1 or the braided wire 2 is soaked for 15 min, the braided sheet 1 or the braided wire 2 is soaked at 25°C, and the distance between two adjacent braided wires 2 in multiple braided wires 2 is 0.5 cm;
[0068] 3. Preliminary freezing: freeze-dry the braided sheet 1 and braided wire 2 in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0069] 4. Freeze drying, after freezing for 2 hours, cool down to -50°C at a cooling rate of 2°C / min, freeze dry for 24 hours, freeze dry until completely dry, the natural polymer in the natural polymer solution adheres to the woven sheet 1 and the woven wire 2 to form a natural polymer coating 3.
[0070] Embodiment 3: A method for preparing a composite stent using polyethylene terephthalate wire with a diameter of 0.4 mm to manufacture a braided sheet 1 and a braided wire 2:
[0071] 1. Connecting: connecting one end of the braided sheet 1 with one end of the plurality of braided wires 2;
[0072] 2. Soaking, soaking the braided sheet 1 and the braided wire 2 in a freezing device, the braided sheet 1 is placed in the braided sheet freezing tank 10, each braided wire 2 is placed in the braided wire freezing tank 9 separately, and then the braided sheet 1 and the braided wire 2 are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire 2 contains nano-hydroxyapatite, the natural polymer concentration is 0.6 mg / mL, the thickness of the braided sheet 1 is 1.2 mm, the thickness and width of the braided wire 2 are both 1.2 mm, the content of nano-hydroxyapatite is 30% of the collagen, the upper surface of the braided sheet 1 or the braided wire 2 is 1.0 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet 1 or the braided wire 2 is 2.0 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet 1 or the braided wire 2 is 0.5 mm away from the interface of the collagen solution, the braided sheet 1 or the braided wire 2 is soaked for 0.1 min, the braided sheet 1 or the braided wire 2 is soaked at a temperature of 35°C, and the distance between two adjacent braided wires 2 in multiple braided wires 2 is 1.5 cm;
[0073] 3. Preliminary freezing: freeze-dry the braided sheet 1 and braided wire 2 in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0074] 4. Freeze drying, after freezing for 2 hours, cool down to -50°C at a cooling rate of 2°C / min, freeze drying for 72 hours, freeze drying until completely dry, the natural polymer in the natural polymer solution adheres to the woven sheet 1 and the woven wire 2 to form a natural polymer coating 3.
[0075] Embodiment 4: A method for preparing a composite stent using polyethylene terephthalate wire with a diameter of 1.0 mm to manufacture a braided sheet 1 and a braided wire 2:
[0076] 1. Connecting: connecting one end of the braided sheet 1 with one end of the plurality of braided wires 2;
[0077] 2. Soaking, soaking the braided sheet 1 and the braided wire 2 in a freezing device, the braided sheet 1 is placed in the braided sheet freezing tank 10, each braided wire 2 is placed in the braided wire freezing tank 9 separately, and then the braided sheet 1 and the braided wire 2 are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire 2 contains nano-hydroxyapatite, the natural polymer concentration is 1.0 mg / mL, the thickness of the braided sheet 1 is 3.0 mm, the thickness and width of the braided wire 2 are both 3.0 mm, the content of nano-hydroxyapatite is 50% of the collagen, the upper surface of the braided sheet 1 or the braided wire 2 is 2.0 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet 1 or the braided wire 2 is 3.0 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet 1 or the braided wire 2 is 0.5 mm away from the interface of the collagen solution, the braided sheet 1 or the braided wire 2 is soaked for 60 min, the braided sheet 1 or the braided wire 2 is soaked at 40°C, and the distance between two adjacent braided wires 2 in multiple braided wires 2 is 3.0 cm;
[0078] 3. Preliminary freezing: freeze-dry the braided sheet 1 and braided wire 2 in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0079] 4. Freeze drying, after freezing for 2 hours, cool down to -50°C at a cooling rate of 2°C / min, freeze drying for 72 hours, freeze drying until completely dry, the natural polymer in the natural polymer solution adheres to the woven sheet 1 and the woven wire 2 to form a natural polymer coating 3.
[0080] Embodiment 5: A method for preparing a composite stent by using polyethylene terephthalate wire with a diameter of 0.3 mm to manufacture the braided sheet 1 and using polyethylene terephthalate wire with a diameter of 0.2 mm to manufacture the braided wire 2:
[0081] 1. Connecting: connecting one end of the braided sheet 1 with one end of the plurality of braided wires 2;
[0082] 2. Soaking, soaking the braided sheet 1 and the braided wire 2 in a freezing device, the braided sheet 1 is placed in the braided sheet freezing tank 10, each braided wire 2 is placed in the braided wire freezing tank 9 separately, and then the braided sheet 1 and the braided wire 2 are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire 2 contains nano-hydroxyapatite, the natural polymer concentration is 0.5 mg / mL, the thickness of the braided sheet 1 is 0.9 mm, the thickness and width of the braided wire 2 are both 0.6 mm, the content of nano-hydroxyapatite is 20% of the collagen, the upper surface of the braided sheet 1 or the braided wire 2 is 0.6 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet 1 or the braided wire 2 is 1.0 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet 1 or the braided wire 2 is 0.5 mm away from the interface of the collagen solution, the braided sheet 1 or the braided wire 2 is soaked for 10 min, the braided sheet 1 or the braided wire 2 is soaked at 25°C, and the distance between two adjacent braided wires 2 in multiple braided wires 2 is 1.0 cm;
[0083] 3. Preliminary freezing: freeze-dry the braided sheet 1 and braided wire 2 in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0084] 4. Freeze drying, after freezing for 2 hours, cool down to -50°C at a cooling rate of 2°C / min, freeze dry for 48 hours, freeze dry until completely dry, the natural polymer in the natural polymer solution adheres to the woven sheet 1 and the woven wire 2 to form a natural polymer coating 3.
[0085] Experimental Example 1 Tensile Strength Test:
[0086] The prepared composite polymer scaffold was cut into strips by laser to obtain the test sample. The test sample was clamped on the upper and lower clamps of the tensile tester, and the tester was started. The moving speed of the clamp was 500mm / min, and the changes in the test length and force were monitored during the entire test. The results are shown in Table 1 below:
[0087] Table 1 Tensile test results
[0088]
[0089] Experimental Example 2
[0090] The Alizarin Red Quantitative Detection Kit was used to detect the ability of each part of the integrated scaffold to induce bone differentiation of BMSC cells. The second part of each sample was cut into 14 mm fragments, sterilized and placed in the wells of a 24-well cell culture plate. 25,000 BMSC cells were planted in each well and cultured in a carbon dioxide incubator. On the 21st day, the absorbance was measured at 562 nm using the Alizarin Red Quantitative Detection Kit. The sample without nanohydroxyapatite was used as a control and the same operation was performed as above. The results are as follows Figure 4 As shown, the OD values of Experimental Examples 2, 3, and 5 were significantly higher than those of the control group, indicating that the second part of the integrated scaffold has the effect of promoting bone differentiation of stem cells, and the scaffold has the potential to guide bone-soft tissue regeneration after implantation.
[0091] It can be seen from the table that the following conditions are optimal: the woven sheet 1 and the woven wire 2 are respectively immersed in the natural polymer solution, the natural polymer concentration is 0.5 mg / mL, the thickness of the woven sheet 1 is 0.9 mm, the thickness and width of the woven wire 2 are both 0.6 mm, the content of nano-hydroxyapatite is 20% of the collagen, the top of the woven sheet 1 or the woven wire 2 is 0.6 mm away from the upper interface of the natural polymer solution, the bottom of the woven sheet 1 or the woven wire 2 is 1.0 mm away from the lower interface of the natural polymer solution, the surrounding of the woven sheet 1 or the woven wire 2 is 0.5 mm away from the interface of the collagen solution, the immersion time of the woven sheet 1 or the woven wire 2 is 10 min, the immersion temperature of the woven sheet 1 or the woven wire 2 is 25°C, the distance between two adjacent woven wires 2 in the multiple woven wires 2 is 1.0 cm, and the negative pressure is maintained for 15 min.
[0092] The present invention provides a tendon-bone integrated scaffold by arranging a braided wire 2 on a braided sheet 1 so that the braided wire 2 can be connected to the bone after punching holes on the bone, and a natural polymer coating containing hydroxyapatite is arranged on the surface of the braided wire, thereby realizing the coordinated repair of tendon tissue and bone tissue. By adopting a freeze-drying process, water molecules in the natural polymer solution are formed into ice crystals and then sublimated, and the remaining natural polymers form a porous, sponge-like natural polymer coating 3, and the porosity of the composite scaffold is 50-90%; due to the porous structure of the coating, the hole structure is conducive to cell adhesion and growth, so that the human body's own tissue growth can more easily enter the natural polymer coating 3, the composite scaffold is more likely to make the rotator cuff and the humeral head tightly combined, and it is easier to form an overall structure, so as to accelerate the healing of the rotator cuff, the natural polymer coating 3 and the braided sheet 1 or the braided wire 2 have a large bonding area and a strong bonding strength. At the same time, the natural polymer coating 3 can reduce the shear damage of the polymer silk thread shear force on the braided sheet 1 or the braided wire 2 to the native tissue, thereby promoting better and faster reconstruction of the tissue. The present invention adopts a purely physical method to form the natural polymer coating 3, without other chemical components generated by chemical reactions, and is more in line with the specifications of medical devices. The woven sheet 1 or woven wire 2 of the present invention can provide a higher initial fixation strength, reaching the initial strength of the rotator cuff; can make the gap between the rotator cuff and the humeral head smaller; the woven sheet 1 or woven wire 2 can still maintain mechanical stability after repeated activities of the human body; the woven wire 1 can still maintain mechanical stability when loaded with cyclic loads; the porous structure of the natural polymer coating 3 can optimize the biological environment of the "healing site" and reduce the shear force of the woven sheet 1 or woven wire 2 on the native tissue. At the same time, the natural polymer solution soaking the woven wire contains nano-hydroxyapatite, which can stimulate bone canal repair and achieve coordinated repair of tendons and bone canals. In summary, the present invention is a very good rotator cuff repair material.
[0093] Specifically, the technical effects are as follows:
[0094] 1. The present invention arranges a braided wire 2 on a braided sheet 1 so that the braided wire 2 can be connected to the bone after punching holes in the bone, making it easier to generate tendons, and the generated tendons are not easily strained;
[0095] 2. The present invention can form a natural polymer coating 3 of suitable thickness by setting the natural polymer concentration to 0.01-1 mg / mL, the upper surface of the woven sheet 1 or the woven wire 2 to be 0.01-1 mm away from the upper interface of the natural polymer solution, and the lower surface of the woven sheet 1 or the woven wire 2 to be 0.01-2 mm away from the lower interface of the natural polymer solution. The natural polymer coating 3 can reduce the shear damage of the polymer wire shear force on the woven sheet 1 or the woven wire 2 to the native tissue, thereby promoting better and faster reconstruction of the tissue;
[0096] 3. The present invention sets preliminary freezing so that water molecules in the natural polymer solution form ice crystals and then sublime, and the remaining natural polymer forms a porous, sponge-like natural polymer coating 3. The loose porous structure is conducive to the growth of human connective tissue into the micropores of the natural polymer coating 3 and combines with the woven sheet 1 or the woven wire 2. The natural polymer coating 3 has a large bonding area and a strong bonding strength with the woven sheet 1 or the woven wire 2.
[0097] 4. The woven sheet 1 or woven wire 2 of the present invention is prepared by a warp weaving process, and the woven sheet 1 or woven wire 2 has high tensile strength, mechanical strength, mechanical stability and good biological activity;
[0098] 5. Compared with adding drugs or porous, sponge-like natural polymer coating 3 around the woven sheet 1 or the woven wire 2 to promote the growth of the body, the natural polymer coating 3 has a weak bonding force with the woven sheet 1 or the woven wire 2. The present invention soaks the woven sheet 1 or the woven wire 2 in a collagen solution and then freeze-dries it. The porous, sponge-like natural polymer coating 3 has a strong bonding force with the woven sheet 1 or the woven wire 2 and a large bonding contact area. The generated body also has a strong bonding force with the woven sheet 1 or the woven wire 2.
[0099] The embodiments described above are only preferred implementation modes of the present invention and cannot be used to limit the protection scope of the present invention. Any non-substantial changes and modifications made by those skilled in the art on the basis of the invention shall fall within the protection scope of the present invention.
Claims
1. A composite stent for rotator cuff repair, Features: The invention comprises a woven sheet and a woven wire, wherein the woven sheet is made by a woven process and is in the shape of a sheet. One or more woven wires made by a woven process are respectively arranged at two ends of the woven sheet, one end of the woven wire is connected to one end of the woven sheet, and the other end is placed freely. The woven wires at two ends of the woven sheet are arranged on the same side of the woven sheet, and the surfaces of the woven sheet and the woven wire are provided with a degradable natural polymer coating, and the natural polymer coating is formed by attaching natural polymers in a natural polymer solution to the woven sheet and the woven wire through a freeze-drying process, and the natural polymer solution is a solution formed by dissolving natural polymers in physiological saline, and the natural polymer coating is porous.
2. The composite stent according to claim 1, Features: The thickness of the braided sheet is 0.08-3.0 mm, the diameter of the polymer substrate in the braided sheet is 0.025-1 mm, and the natural polymer solution for soaking the braided wire contains nano-hydroxyapatite.
3. The composite stent according to claim 1, Features: The natural polymer includes animal-derived collagen and / or recombinant collagen and / or gelatin and / or chitosan and / or silk fibroin. The woven sheet is prepared from a non-degradable polymer substrate through a weaving process. The polymer substrate includes polyethylene terephthalate and / or polypropylene and / or polyethylene and / or polydioxanone and / or polydioxanone and / or polycaprolactone and / or poly-L-lactide and / or polyglycolic acid.
4. The composite stent according to claim 3, Features: The polymer substrate is polyethylene terephthalate, and the natural polymer is collagen.
5. The composite stent according to claim 1, Features: The yarn diameter of the braided wire is 0.025-1mm; the thickness of the braided wire is 0.08-3mm; the width of the braided wire is 0.08-3mm; and the length of the braided wire is 2-15cm.
6. The composite stent according to claim 5, Features: A plurality of braided wires are arranged at one end of the braided sheet, and the distance between two adjacent braided wires among the plurality of braided wires is between 0.1-3 cm.
7. The composite stent according to claim 1, Features: The coating on the braided wire is connected to the coating on the braided sheet, and the coating on the braided wire is disconnected from the coating on another braided wire so that the braided wires pass through different bone holes respectively.
8. A method for preparing a composite scaffold, Features: The following steps are involved:
1. Connect, connect one end of the braided sheet with one end of multiple braided wires; 2. Soaking, soaking the braided sheet and the braided wire in a freezing device, the braided sheet is placed in a braided sheet freezing tank, each braided wire is placed in a braided wire freezing tank separately, and then the braided sheet and the braided wire are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire contains nano-hydroxyapatite, and the concentration of natural polymer is 0.01-1 mg / mL, the upper surface of the braided sheet or the braided wire is 0.01-2 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet or the braided wire is 0.01-3 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet or the braided wire is 0.01-1 mm away from the interface of the collagen solution, the braided sheet or the braided wire is soaked for 0.1-60 min, the braided sheet or the braided wire soaking temperature is 0-40° C., and the distance between two adjacent braided wires in the multiple braided wires is 0.1-3 cm; 3. Preliminary freezing: freeze-dry the braided sheets and braided wires in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15-60min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
4. Freeze drying: After freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze-dry for 24-72 hours, freeze-dry until completely dry. The natural polymer in the natural polymer solution adheres to the woven sheets and woven wires to form a natural polymer coating.
9. The preparation method according to claim 8, Features: The freezing device includes a freezing tank and a partition. The freezing tank is provided with two large partition bones to divide the freezing tank into a woven sheet freezing tank and a plurality of woven wire freezing tanks. The large partition bones are provided with a plurality of woven wire through holes for the woven wires to pass through. The woven wire freezing tank is provided with a plurality of small partition bones to divide the woven wire freezing tank into a plurality of independent freezing units to prevent the natural polymer coatings on the woven wires from being connected to each other. The partition is placed on the large partition bones to prevent the natural polymer solution from flowing between the woven sheet freezing tank and the woven wire freezing tank.
10. The preparation method according to claim 8, Features: The following steps are involved:
1. Connect, connect one end of the braided sheet with one end of multiple braided wires; 2. Soaking, soaking the braided sheet and the braided wire in a freezing device, the braided sheet is placed in a braided sheet freezing tank, each braided wire is placed in a braided wire freezing tank separately, and then the braided sheet and the braided wire are respectively soaked in a natural polymer solution, wherein the natural polymer solution for soaking the braided wire contains nano-hydroxyapatite, the natural polymer concentration is 0.5 mg / mL, the thickness of the braided sheet is 0.9 mm, the thickness and width of the braided wire are both 0.6 mm, the content of nano-hydroxyapatite is 20% of collagen, the upper surface of the braided sheet or the braided wire is 0.6 mm away from the upper interface of the natural polymer solution, the lower surface of the braided sheet or the braided wire is 1.0 mm away from the lower interface of the natural polymer solution, the surrounding of the braided sheet or the braided wire is 0.5 mm away from the interface of the collagen solution, the braided sheet or the braided wire is soaked for 10 min, the braided sheet or the braided wire is soaked at 25° C., and the distance between two adjacent braided wires 2 in the multiple braided wires is 1.0 cm; 3. Preliminary freezing: freeze-dry the braided sheets and braided wires in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
4. Freeze drying: After freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze dry for 48 hours, and freeze dry until completely dry. The natural polymer in the natural polymer solution adheres to the woven sheets and woven wires to form a natural polymer coating.
Citation Information
Patent Citations
Integrated artificial bone ligament bone graft and preparation method thereof
CN106691628A
Preparation method of drug-loading type bionic bone repairing porous scaffold, product prepared by preparation method and application of product
CN109568674A
Ligament regeneration stent with gradient induction activity and preparation method thereof
CN112226871A
Plug pin type soft tissue repair patch and preparation method thereof
CN112972064A
Rotator cuff patch and manufacturing method thereof
CN113499165A