Composite nanofiltration membrane with high removal hardness as well as preparation device and preparation method thereof
By combining polyethyleneimine with diamine compounds with polyfunctional acid chloride, a composite nanofiltration membrane with high removal hardness is formed, which solves the problem of low removal rate of calcium and magnesium ions and water circulation of existing nanofiltration membranes. The problem of insufficient quantity achieves higher hardness removal and water flux.
Patent Information
- Application Number
- CN202411039737.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
AI Technical Summary
The existing nanofiltration membrane has low removal rate of calcium and magnesium ions, resulting in poor softening of water quality. The Na2SO4 intercept rate during routine preparation is high, which affects the water flux.
The aqueous solution of polyethyleneimine and diamine compounds is combined with the oil-phase solution of polyfunctional acid chloride, and the liquid level height difference force and air compressor purge to form a composite nanofiltration membrane with high removal hardness. , increase the positive charge on the film surface to increase the removal rate of calcium and magnesium ions.
The removal rate of calcium and magnesium ions and water flux are significantly improved, the hardness removal ability of the membrane is enhanced, and the high Na2SO4 retention rate is maintained.
Smart Images

Figure CN118904093A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of separation, and in particular relates to a composite nanofiltration membrane with high removal hardness and a preparation device and a preparation method thereof. Background Art
[0002] Membrane separation technology is widely used in water treatment, material separation, purification, concentration and other fields. At present, membrane technology has gradually replaced traditional water treatment processes due to its energy saving, high efficiency, simple process and easy operation.
[0003] The high hardness of drinking water significantly affects people's health. Nanofiltration membranes have good permeability selectivity and can effectively remove calcium and magnesium ions in water through steric effect, Donan effect and dielectric effect. They can also retain some beneficial minerals and trace elements in water; at the same time, they can maintain a higher water flux than reverse osmosis membranes. In addition, the low operating pressure of the nanofiltration process makes the energy consumption generated during its use lower. Therefore, nanofiltration membranes are widely used in water softening treatment.
[0004] In the conventional nanofiltration membrane preparation process, diamine compounds are usually used as aqueous phase monomers. After the interfacial polymerization reaction, a strongly negatively charged polyamide layer is formed, and the corresponding isoelectric point is generally around pH 4.0. Therefore, the prepared conventional nanofiltration membrane has a high Na2SO4 retention rate; but the removal rate of calcium and magnesium ions is low, and the corresponding prepared nanofiltration membrane has a poor dehardening effect. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a composite nanofiltration membrane with high removal hardness and a preparation device, preparation method and application thereof.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A preparation device for a composite nanofiltration membrane with high removal hardness comprises a membrane assembly of a base membrane, a water phase solution storage tank connected to the membrane assembly of the base membrane, an oil phase solution storage tank, and an air compressor.
[0008] The water phase solution storage tank and the oil phase solution storage tank are higher than the membrane assembly of the base membrane, and the force generated by the height difference causes the water phase solution and the oil phase solution to flow into the tube side of the membrane assembly of the base membrane;
[0009] Preferably, a first valve is provided on the pipeline between the oil phase solution storage tank and the inlet of the membrane assembly, a second valve is provided on the pipeline between the water phase solution storage tank and the inlet of the membrane assembly, a third valve is provided on the pipeline of the lower outlet of the membrane assembly, and a fourth valve is provided on the pipeline of the upper outlet; a rotor flowmeter, a pressure gauge and a water and oil removal filter are provided on the pipeline between the membrane assembly and the air compressor.
[0010] The present invention also includes a method for preparing a composite nanofiltration membrane with high removal hardness. Using the preparation device, the method includes the following steps: an aqueous phase solution flows into the tube side of the base membrane assembly to infiltrate the base membrane, an air compressor is used to blow the membrane surface, and then an oil phase solution flows into the tube side of the base membrane assembly to react to obtain a composite nanofiltration membrane with high removal hardness.
[0011] The aqueous phase solution is a mixture of an aqueous solution of polyethyleneimine and an aqueous solution of a diamine compound;
[0012] The mass concentration of polyethyleneimine in the aqueous phase solution is 0.1wt%-0.9wt%; the mass concentration of the diamine compound is 0.1wt%-0.3wt%.;
[0013] Preferably, the diamine compound is one of piperazine, m-phenylenediamine, or p-phenylenediamine.
[0014] The base membrane is a hollow fiber membrane or a flat membrane of polysulfone, polyvinylidene fluoride or polyvinyl chloride.
[0015] The molecular weight of the polyethyleneimine is 1800-70000Da.
[0016] The oil phase solution is a multifunctional acyl chloride solution;
[0017] The mass concentration of the oil phase solution is 0.05wt%-0.2wt%;
[0018] The multifunctional acyl chloride is one of trimesoyl chloride, adipoyl chloride and sebacoyl chloride;
[0019] The solvent of the oil phase solution is one of n-hexane, cyclohexane and heptane.
[0020] Specifically, the steps include: opening the second valve and the fourth valve, closing the first valve and the third valve, and utilizing the force generated by the liquid level difference to allow the aqueous phase solution to flow from bottom to top into the tube side of the membrane module;
[0021] After soaking, close the second valve and the fourth valve, and open the third valve to allow the liquid to flow out of the membrane assembly;
[0022] Then, use an air compressor to purge the membrane module from top to bottom to remove excess water phase solution. The purge time is 3-7 minutes. Then, open the first valve and the fourth valve, close the third valve, and use the force generated by the liquid level difference to pass the oil phase solution from bottom to top for 30-80 seconds.
[0023] Finally, the first valve and the fourth valve are closed, and the third valve is opened to allow the oil phase solution to flow out of the membrane assembly to obtain the composite nanofiltration membrane.
[0024] The present invention also includes a composite nanofiltration membrane with high removal hardness obtained by the preparation method.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The technical solution of the present invention introduces polyethyleneimine into the diamine aqueous phase solution, and uses the polyethyleneimine containing rich amine groups to make the separation layer of the nanofiltration membrane carry more positive charges, thereby achieving a high removal rate for divalent cations. Compared with conventional nanofiltration membranes, the nanofiltration membrane prepared by the present invention not only has a higher removal rate for divalent anions, but also has a better hardness removal rate and a higher membrane flux. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the preparation device of the composite nanofiltration membrane for high removal hardness of the present invention.
[0028] Figure 2 This is a graph showing the salt retention performance of nanofiltration membranes prepared with piperazine as the aqueous phase monomer and piperazine + polyethyleneimine as the aqueous phase monomer.
[0029] Figure 3 This is a graph showing the water flux results of nanofiltration membranes prepared with piperazine as the water phase monomer and piperazine + polyethyleneimine as the water phase monomer. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.
[0031] Figure 1 A preparation device for a composite nanofiltration membrane with high removal hardness is shown, which includes a membrane assembly 9 of a base membrane, an aqueous solution storage tank 2 connected to the membrane assembly of the base membrane, an oil phase solution storage tank 1, and an air compressor 7.
[0032] The heights of the water phase solution storage tank 2 and the oil phase solution storage tank 1 are higher than the membrane assembly 9 of the base membrane, and the height difference satisfies the pipe passage of the water phase solution and the oil phase solution flowing into the membrane assembly of the base membrane;
[0033] Preferably, a first valve 31 is provided on the pipeline between the oil phase solution storage tank 1 and the inlet of the membrane assembly 9, a second valve 32 is provided on the pipeline between the water phase solution storage tank 2 and the inlet of the membrane assembly 9, a third valve 33 is provided on the pipeline at the lower end outlet of the membrane assembly 9, and a fourth valve 34 is provided on the pipeline at the upper end outlet; a rotor flowmeter 4, a pneumatic set valuer 5, a pressure gauge 6 and a water and oil removal filter 8 are provided on the pipeline between the membrane assembly 9 and the air compressor 7.
[0034] The present invention also includes a method for preparing a composite nanofiltration membrane with high removal hardness. Using the preparation device, the method includes the following steps: an aqueous phase solution flows into the tube side of the base membrane assembly to infiltrate the base membrane, an air compressor is used to blow the membrane surface, and then an oil phase solution flows into the tube side of the base membrane assembly to react to obtain a composite nanofiltration membrane with high removal hardness.
[0035] The aqueous phase solution is a mixed aqueous solution of polyethyleneimine and diamine compounds;
[0036] The mass concentration of polyethyleneimine in the aqueous phase solution is 0.1wt%-0.9wt%; specifically, it can be 0.1wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.9wt%; preferably, it is 0.3-0.6wt%; more preferably, it is 0.3wt%; the mass concentration of the diamine compound is 0.1wt%-0.3wt%; specifically, it can be 0.1wt%, 0.2wt%, 0.3wt%.
[0037] The diamine compound is one of piperazine, m-phenylenediamine, or p-phenylenediamine.
[0038] The base membrane is a hollow fiber membrane or a flat membrane of polysulfone, polyvinylidene fluoride or polyvinyl chloride.
[0039] The molecular weight of the polyethyleneimine is 1800-70000Da, specifically 1800Da, 3000Da, 10000Da, 25000Da, 70000Da; preferably 1800-3000Da.
[0040] The oil phase solution is a solution of multifunctional acyl chloride; the mass concentration of the oil phase solution is 0.05wt%-0.2wt%; specifically, it can be 0.05wt%, 0.15wt%, 0.2wt%; the multifunctional acyl chloride is one of trimesoyl chloride, adipoyl chloride, and sebacyl chloride; the solvent of the oil phase solution is one of n-hexane, cyclohexane, and heptane.
[0041] The preparation method of the composite nanofiltration membrane with high removal hardness specifically comprises the following steps: opening the second valve 32 and the fourth valve 34, closing the first valve 31 and the third valve 33, and utilizing the force generated by the liquid level difference to make the aqueous phase solution flow from bottom to top into the tube side of the membrane assembly 9;
[0042] After the infiltration, the second valve 32 and the fourth valve 34 are closed, and the third valve 33 is opened to allow the liquid to flow out of the membrane assembly;
[0043] Then, the air compressor 7 is used to purge the tube side of the membrane assembly 9 from top to bottom to remove excess water phase solution, and the purge time is 3-7 minutes; then, the first valve 31 and the fourth valve 34 are opened, and the third valve 33 is closed, and the oil phase solution is introduced from bottom to top by the force generated by the liquid level difference, and the reaction is carried out for 30-80 seconds, specifically 30 seconds, 60 seconds, and 80 seconds;
[0044] Finally, the first valve 31 and the fourth valve 34 are closed, and the third valve 33 is opened to allow the oil phase solution to flow out of the membrane assembly to obtain a composite nanofiltration membrane.
[0045] The present invention also includes a composite nanofiltration membrane with high removal hardness obtained by the preparation method.
[0046] The present invention also includes an application of the composite nanofiltration membrane with high removal hardness, characterized in that it is applied to material separation, purification, or concentration.
[0047] The following is a description using a preferred embodiment as an illustrative example.
[0048] Example 1
[0049] The preparation method of the composite nanofiltration membrane with high removal hardness comprises the following steps: first, polyethyleneimine and piperazine with a molecular weight of 1800Da are added to deionized water respectively, and stirred to prepare a mixed aqueous phase solution containing 0.3wt% polyethyleneimine and 0.15wt% piperazine. Then, Figure 1 As shown, the force generated by the liquid level difference is used to make the aqueous solution flow from bottom to top into the tube side of the polyvinyl chloride hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0 m / s using an air compressor to remove excess aqueous solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top and react for 60 seconds. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0050] Comparative Example 1
[0051] like Figure 1 As shown, the force generated by the liquid level difference is used to make the 0.45wt% piperazine aqueous solution flow from bottom to top into the tube side of the hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0m / s using an air compressor to remove excess aqueous phase solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top, and the reaction is 60s. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0052] Example 2
[0053] The preparation method of the composite nanofiltration membrane with high removal hardness comprises the following steps: first, polyethyleneimine and piperazine with a molecular weight of 3000Da are added to deionized water respectively, and stirred and mixed to prepare a mixed aqueous phase solution containing 0.3wt% polyethyleneimine and 0.15wt% piperazine. Then, Figure 1 As shown, the force generated by the liquid level difference is used to make the aqueous solution flow from bottom to top into the tube side of the polyvinyl chloride hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0 m / s using an air compressor to remove excess aqueous solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top and react for 60 seconds. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0054] Example 3
[0055] The preparation method of the composite nanofiltration membrane with high removal hardness comprises the following steps: first, polyethyleneimine and piperazine with a molecular weight of 10,000 Da are added to deionized water respectively, and stirred to prepare a mixed aqueous phase solution containing 0.3 wt% polyethyleneimine and 0.15 wt% piperazine. Then, Figure 1 As shown, the force generated by the liquid level difference is used to make the aqueous solution flow from bottom to top into the tube side of the polyvinyl chloride hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0 m / s using an air compressor to remove excess aqueous solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top and react for 60 seconds. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0056] Example 4
[0057] The preparation method of the composite nanofiltration membrane with high removal hardness comprises the following steps: first, polyethyleneimine and piperazine with a molecular weight of 25000Da are added to deionized water respectively, and stirred to prepare a mixed aqueous phase solution containing 0.3wt% polyethyleneimine and 0.15wt% piperazine. Then, Figure 1As shown, the force generated by the liquid level difference is used to make the aqueous solution flow from bottom to top into the tube side of the polyvinyl chloride hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0 m / s using an air compressor to remove excess aqueous solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top and react for 60 seconds. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0058] Example 5
[0059] The preparation method of the composite nanofiltration membrane with high removal hardness comprises the following steps: first, polyethyleneimine and piperazine with a molecular weight of 70,000 Da are added to deionized water respectively, and stirred and mixed to prepare a mixed aqueous phase solution containing 0.3 wt % polyethyleneimine and 0.15 wt % piperazine. Then, Figure 1 As shown, the force generated by the liquid level difference is used to make the aqueous solution flow from bottom to top into the tube side of the polyvinyl chloride hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0 m / s using an air compressor to remove excess aqueous solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top, and the reaction is 60 seconds. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0060] Example 6
[0061] The preparation method of the composite nanofiltration membrane with high removal hardness comprises the following steps: first, polyethyleneimine and piperazine with a molecular weight of 1800Da are added to deionized water respectively, and stirred to prepare a mixed aqueous phase solution containing 0.1wt% polyethyleneimine and 0.15wt% piperazine. Then, Figure 1 As shown, the force generated by the liquid level difference is used to make the aqueous solution flow from bottom to top into the tube side of the polyvinyl chloride hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0 m / s using an air compressor to remove excess aqueous solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top, and the reaction is 60 seconds. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0062] Example 7
[0063] The preparation method of the composite nanofiltration membrane with high removal hardness comprises the following steps: first, polyethyleneimine and piperazine with a molecular weight of 1800Da are added to deionized water respectively, and stirred to prepare a mixed aqueous phase solution containing 0.6wt% polyethyleneimine and 0.15wt% piperazine. Then, Figure 1 As shown, the force generated by the liquid level difference is used to make the aqueous solution flow from bottom to top into the tube side of the polyvinyl chloride hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0 m / s using an air compressor to remove excess aqueous solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top, and the reaction is 60 seconds. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0064] Example 8
[0065] The preparation method of the composite nanofiltration membrane with high removal hardness comprises the following steps: first, polyethyleneimine and piperazine with a molecular weight of 1800Da are added to deionized water respectively, and stirred to prepare a mixed aqueous phase solution containing 0.9wt% polyethyleneimine and 0.15wt% piperazine. Then, Figure 1 As shown, the force generated by the liquid level difference is used to make the aqueous solution flow from bottom to top into the tube side of the polyvinyl chloride hollow fiber membrane module. After soaking for 5 minutes, the membrane module tube side is purged from top to bottom at a linear speed of 13.0 m / s using an air compressor to remove excess aqueous solution. The purging time is 5 minutes. Then, the force generated by the liquid level difference is used to pass 0.15wt% trimesoyl chloride / n-hexane solution from bottom to top, and the reaction is 60 seconds. After the experiment, the prepared polyamide nanofiltration membrane is stored in deionized water for testing.
[0066] Results test:
[0067] The membrane assembly prepared in the embodiment and the comparative example was fixed on a cross-flow filtration test device, and pure water passed through the membrane assembly under the internal pressure mode. The pressure of the cross-flow filtration test device was set to pre-press at 0.30 MPa for 1 hour. After the membrane was completely compacted, the water obtained within 10 minutes was collected, and the pure water flux was tested by weighing method; then the pure water was replaced with 1.0 g / L MgCl2 solution as the feed solution to continue the test. The MgCl2 solution passed through the membrane assembly under the internal pressure mode, and the operating pressure of the cross-flow filtration test device was 0.30 MPa. The conductivity of the produced water was tested using a conductivity meter every 10 minutes until it was stable and unchanged to obtain the retention rate.
[0068] Table 1 shows the performance parameters of different embodiments and comparative examples.
[0069] Table 1. Comparison of nanofiltration membrane performance
[0070]
[0071]
[0072] Result analysis:
[0073] 1. Comparison between polyethyleneimine + piperazine and piperazine system
[0074] Comparison of Example 1 and Comparative Example 1: Figure 2 As shown in Table 1, compared with the polyamide nanofiltration membrane prepared with piperazine in Comparative Example 1, the polyamide nanofiltration membrane prepared by the polyethyleneimine + piperazine system exhibited higher MgCl2 and CaCl2 retention rates of 96.5% and 95.7%, respectively, due to the enhanced positive charge on the membrane surface. Moreover, after polyethyleneimine was added to the aqueous phase, the Na2SO4 retention rate was not significantly affected. The retention rate remained above 94%.
[0075] like Figure 3 As shown in Table 1, after polyethyleneimine is added to the aqueous phase, the hydrophilicity of the membrane surface is enhanced due to the increase in the number of hydrophilic groups inside the polyamide. Therefore, the polyamide nanofiltration membrane prepared by the present invention exhibits a higher water flux result.
[0076] 2. Adding polyethyleneimine with different molecular weights (Examples 1-5)
[0077] As the molecular weight of polyethyleneimine increases, its molecular chains tend to twist and entangle with each other, thus easily forming a denser cross-linked network structure, which leads to a greater resistance to transmembrane mass transfer of water molecules. Moreover, as the molecular weight of polyethyleneimine increases, the hardness of the membrane gradually increases. This is because the increase in the molecular weight of polyethyleneimine increases the amount of amine groups on the membrane surface, which, according to the charge repulsion effect, causes the nanofiltration membrane to resist Mg 2+ and Ca 2+ The removal rate increased.
[0078] 3. Polyethyleneimine at different concentrations in the aqueous phase (Examples 6-8)
[0079] As the concentration of added polyethyleneimine increased from 0.1wt% to 0.3wt%, the water flux of the membrane gradually decreased. This is because the increase in polyethyleneimine concentration (i.e., the increase in the total concentration of aqueous monomers) increased the amount of aqueous monomers diffusing into the reaction area, which resulted in a denser polyamide membrane obtained by interfacial polymerization. At the same time, as the concentration of polyethyleneimine increased, the amount of positive charge on the corresponding membrane surface also gradually increased. Therefore, the combined effect of the two resulted in the prepared nanofiltration membrane being more resistant to Mg. 2+ and Ca 2+When the concentration of polyethyleneimine further increased from 0.3wt% to 0.9wt%, the Mg 2+ and Ca 2+ The rejection rate decreased and the flux increased. This is because when the aqueous phase monomer concentration is excessive, it is difficult to form a polyamide layer with a cross-linked network structure on the membrane surface, resulting in an increase in defects in the formed polyamide layer.
[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A preparation device for a composite nanofiltration membrane with high removal hardness, It is characterized in that The invention comprises a membrane assembly of a base membrane, a water phase solution storage tank communicated with the membrane assembly of the base membrane, an oil phase solution storage tank, and an air compressor.
2. The preparation device of the composite nanofiltration membrane with high removal hardness according to claim 1, It is characterized in that The water phase solution storage tank and the oil phase solution storage tank are higher than the membrane assembly of the base membrane, and the force generated by the height difference causes the water phase solution and the oil phase solution to flow into the tube side of the membrane assembly of the base membrane; Preferably, a first valve is provided on the pipeline between the oil phase solution storage tank and the inlet of the membrane assembly, a second valve is provided on the pipeline between the water phase solution storage tank and the inlet of the membrane assembly, a third valve is provided on the pipeline of the lower outlet of the membrane assembly, and a fourth valve is provided on the pipeline of the upper outlet; a rotor flowmeter, a pressure gauge and a water and oil removal filter are provided on the pipeline between the membrane assembly and the air compressor.
3. A method for preparing a composite nanofiltration membrane with high removal hardness, using the preparation device according to any one of claims 1 to 2, It is characterized in that The method comprises the following steps: an aqueous solution flows into the tube side of the membrane assembly to infiltrate the base membrane, an air compressor is used to purge the membrane surface, and an oil phase solution flows into the tube side of the membrane assembly of the base membrane to react and obtain a composite nanofiltration membrane with high removal hardness.
4. The method for preparing a composite nanofiltration membrane with high removal hardness according to claim 3, It is characterized in that The aqueous phase solution is a mixed aqueous solution of polyethyleneimine and diamine compounds; The mass concentration of the polyethyleneimine is 0.1wt%-0.9wt%, preferably 0.3wt%-0.6wt%; the mass concentration of the aqueous solution of the polyamine compound is 0.1wt%-0.3wt%; Preferably, the diamine compound is one of piperazine, m-phenylenediamine, or p-phenylenediamine.
5. The method for preparing a composite nanofiltration membrane with high removal hardness according to claim 4, It is characterized in that The base membrane is a hollow fiber membrane or a flat membrane of polysulfone, polyvinylidene fluoride or polyvinyl chloride.
6. The method for preparing the composite nanofiltration membrane with high removal hardness according to claim 4, It is characterized in that The molecular weight of the polyethyleneimine is 1800-70000Da.
7. The method for preparing the composite nanofiltration membrane with high removal hardness according to claim 3, It is characterized in that The oil phase solution is a multifunctional acyl chloride solution; The mass concentration of the oil phase solution is 0.05wt%-0.2wt%; The multifunctional acyl chloride is one of trimesoyl chloride, adipoyl chloride and sebacoyl chloride; The solvent of the oil phase solution is one of n-hexane, cyclohexane and heptane.
8. The method for preparing the composite nanofiltration membrane with high removal hardness according to claim 3, It is characterized in that Specifically, the steps include: opening the second valve and the fourth valve, closing the first valve and the third valve, and utilizing the force generated by the liquid level difference to allow the aqueous phase solution to flow from bottom to top into the tube side of the membrane module; After soaking, close the second valve and the fourth valve, and open the third valve to allow the liquid to flow out of the membrane assembly; Then, use an air compressor to purge the membrane module from top to bottom to remove excess water phase solution. The purge time is 3-7 minutes. Then, open the first valve and the fourth valve, close the third valve, and use the force generated by the liquid level difference to pass the oil phase solution from bottom to top for 30-80 seconds. Finally, the first valve and the fourth valve are closed, and the third valve is opened to allow the oil phase solution to flow out of the membrane assembly to obtain the composite nanofiltration membrane.
9. A composite nanofiltration membrane with high removal hardness obtained by the preparation method according to any one of claims 3 to 8.
Citation Information
Cited By
Device and method for removing urea from water
CN120590000A