Post-treatment method of reverse osmosis membrane and reverse osmosis dry membrane

By using inorganic salts such as potassium chloride, magnesium chloride, and calcium chloride as moisturizers, the oxidation and airtightness of the reverse osmosis membrane are solved, the membrane performance is maintained and glycerol is replaced, and a more efficient and environmentally friendly membrane preparation is achieved.

CN118904095APending Publication Date: 2024-11-08BEIJING BISHUIYUAN SEPARATION MEMBRANE TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411262480.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing reverse osmosis membranes have problems such as oxidation and blackening, which are prone to microorganisms and are not resistant to low temperatures. The shrinkage of porous structures after heat treatment leads to reduced performance, and the use of glycerol as a moisturizer in commercial membranes leads to chemical dissolution. High, affects health and airtightness.

Method used

Inorganic salts such as potassium chloride, magnesium chloride, and calcium chloride are used as moisturizing agents. Through soaking and drying, the membrane pore structure does not shrink and improves airtightness, and replaces glycerin to reduce chemical dissolution.

Benefits of technology

The reverse osmosis performance is maintained, the airtightness and use efficiency are improved, and the inorganic salts are easy to flush, shortening the time for membrane elements to achieve stable performance, and is greener and more environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904095A_ABST
    Figure CN118904095A_ABST
Patent Text Reader

Abstract

The invention provides a post-treatment method of a reverse osmosis membrane and a reverse osmosis dry membrane, and particularly relates to the technical field of separation membrane preparation. The post-treatment method comprises the following steps: soaking the reverse osmosis membrane in an aqueous solution of a humectant, removing the redundant aqueous solution of the humectant, and drying to obtain a reverse osmosis dry membrane; the humectant is inorganic salt. According to the post-treatment method, inorganic salt rapidly enters interfacial film pores through soaking, in the heat treatment process, the inorganic salt plays a good supporting role, the pore channel structure does not shrink, and the reverse osmosis performance is kept. Meanwhile, inorganic salt exists in the obtained reverse osmosis dry membrane, the reverse osmosis dry membrane has extremely high hygroscopicity, water molecules in air are extremely easily adsorbed to be in a liquid state and are distributed in cavities of the polyamide leaves or pore channels of the porous supporting layer, gas is effectively isolated from passing through, and it is guaranteed that the membrane has good air tightness. In addition, the inorganic salt is extremely easy to wash away by water in the subsequent use process of the membrane element, so that the time for the membrane element to achieve stable performance is shortened, and the use efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of separation membrane preparation, in particular to a reverse osmosis membrane post-treatment method and a reverse osmosis dry membrane. Background Art

[0002] Reverse osmosis membrane is a special chemical membrane that can intercept solutes and ions in water under pressure and only allow water molecules to pass through. This technology is widely used in seawater desalination, drinking water purification and other fields.

[0003] Reverse osmosis dry membrane and wet membrane are two commonly used models in membrane separation technology. They both use the reverse osmosis principle to filter the salt content in the water through the special structure of the membrane. The working principles of reverse osmosis dry membrane and wet membrane are basically the same. The special structure of the membrane allows the salt and impurities in the water to be trapped on the membrane surface, thereby achieving the process of separating water and salt.

[0004] Wet membrane refers to the reverse osmosis membrane that has been tested with water during the production process, and a certain amount of protective liquid needs to be added when it is stored. Dry membrane refers to the reverse osmosis membrane that has not been tested with water, and is in a dry state. It does not require protective liquid for storage and can be stored in a vacuum.

[0005] In the process of preparing reverse osmosis membrane, after the polymerization reaction at the water-oil interface, a large amount of unreacted monomers, such as m-phenylenediamine, will remain in the primary reverse osmosis membrane. The residual m-phenylenediamine will oxidize, causing the membrane to turn yellow and black, which has a great impact on the appearance and performance of the membrane product. Therefore, the membrane needs to be rinsed. The rinsed membrane is called a wet membrane. The components rolled from wet membranes have low dissolution and can achieve stable performance in a short time. However, wet membranes are prone to microbial growth and are not resistant to low temperatures. They require additional protective liquid, which has an adverse effect on transportation and storage. In addition, using wet membranes to roll components is also a huge technical challenge.

[0006] During the preparation of dry membranes, if the wet membrane is directly heat-treated, the water production and desalination rate of the obtained dry membrane will be significantly reduced. This is because during the heat treatment, the porous structure of the reverse osmosis membrane physically shrinks, resulting in changes in the performance of the membrane. In order for the reverse osmosis dry membrane to maintain the original performance of the wet membrane, the wet membrane needs to be post-treated with a moisturizer and then dried. After the obtained dry membrane is rolled into a component, the component needs to be gas-tested to ensure that the glue line does not leak, which puts forward requirements for the gas permeability of the membrane itself. Currently, commercial reverse osmosis membranes mostly use glycerin as a humectant to protect the pore structure while ensuring the airtightness of the membrane element during use. In order to meet the airtightness requirements, a higher concentration of glycerin is usually used, which leads to high chemical dissolution during use and harms health.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] One of the purposes of the present invention is to provide a post-treatment method for a reverse osmosis membrane, aiming to solve at least one of the above-mentioned technical problems in the prior art.

[0009] A second object of the present invention is to provide a reverse osmosis dry membrane.

[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0011] A first aspect of the present invention provides a post-treatment method for a reverse osmosis membrane, wherein the reverse osmosis membrane is immersed in an aqueous solution of a moisturizing agent, and after completion, excess aqueous solution of the moisturizing agent is removed, and then dried to obtain a reverse osmosis dry membrane;

[0012] The humectant is an inorganic salt.

[0013] Furthermore, the inorganic salt includes at least one of potassium chloride, magnesium chloride, calcium chloride and magnesium sulfate.

[0014] Furthermore, the inorganic salt is magnesium chloride and / or calcium chloride.

[0015] Preferably, the magnesium chloride is anhydrous magnesium chloride.

[0016] Preferably, the calcium chloride is anhydrous calcium chloride.

[0017] Furthermore, the mass concentration of the aqueous solution is 4% to 12%, preferably 5% to 10%.

[0018] Furthermore, the temperature of the aqueous solution is 35°C to 45°C.

[0019] Furthermore, the soaking time is 60s to 120s.

[0020] Further, excess moisturizing agent aqueous solution was removed using a pressure roller.

[0021] Furthermore, the drying temperature is 60° C. to 90° C., and the drying time is 3 min to 10 min.

[0022] Furthermore, the reverse osmosis membrane comprises a polyamide composite reverse osmosis membrane.

[0023] The second aspect of the present invention provides a reverse osmosis dry membrane, which is obtained by using the post-treatment method described in the first aspect.

[0024] Compared with the prior art, the present invention has at least the following beneficial effects:

[0025] The post-treatment method of the reverse osmosis membrane provided by the present invention allows the inorganic salt to quickly enter the interface membrane pores of the reverse osmosis membrane polyamide and the porous support layer through immersion. During the heat treatment process, the inorganic salt plays a good supporting role, the pore structure does not shrink, and the good reverse osmosis performance is maintained. At the same time, during the air tightness test process, the inorganic salt uses hygroscopicity to absorb water molecules in the air to present a liquid state, which is distributed in the cavities of the polyamide blades or the pores of the porous support layer, effectively isolating the gas from passing through, and ensuring that the membrane has good air tightness. In addition, during the subsequent use of the membrane element, the inorganic salt is easily washed away by water, which shortens the time taken for the membrane element to reach stable performance and improves the use efficiency.

[0026] The reverse osmosis dry membrane provided by the present invention has inorganic salts in the membrane structure, which replaces alcohol moisturizers such as glycerin, improves the pore-preserving effect and has no chemical dissolution, is more environmentally friendly, and is suitable for large-scale promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 It is a schematic diagram of the principle of the post-processing method of the present invention;

[0029] Figure 2 This is a surface electron microscope image of the reverse osmosis dry membrane obtained in Example 1;

[0030] Figure 3 This is a cross-sectional electron micrograph of the reverse osmosis dry membrane obtained in Example 1. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0032] Hereinafter, the terms "including", "having" and their cognates, which may be used in various embodiments of the present invention, are intended only to indicate specific features, numbers, steps, operations, elements, components or combinations of the foregoing items, and should not be understood as first excluding the existence of one or more other features, numbers, steps, operations, elements, components or combinations of the foregoing items or adding the possibility of one or more features, numbers, steps, operations, elements, components or combinations of the foregoing items.

[0033] A first aspect of the present invention provides a post-treatment method for a reverse osmosis membrane, wherein the reverse osmosis membrane is immersed in an aqueous solution of a moisturizing agent, and after completion, excess aqueous solution of the moisturizing agent is removed, and then dried to obtain a reverse osmosis dry membrane;

[0034] The humectant is an inorganic salt.

[0035] The post-treatment method of the reverse osmosis membrane provided by the present invention allows the inorganic salt to quickly enter the interface membrane pores between the reverse osmosis membrane polyamide and the porous support layer by soaking. Figure 1 As shown in the figure, during the heat treatment process, the inorganic salt plays a good supporting role, the pore structure does not shrink, and the good reverse osmosis performance is maintained. At the same time, during the air tightness test, the inorganic salt uses its hygroscopicity to absorb water molecules in the air and presents a liquid state, which is distributed in the cavities of the polyamide blades or the pores of the porous support layer, effectively isolating the gas from passing through and ensuring that the membrane has good air tightness. In addition, during the subsequent use of the membrane element, the inorganic salt is easily washed away by water, which shortens the time it takes for the membrane element to reach stable performance and improves its use efficiency.

[0036] Furthermore, the inorganic salt includes at least one of potassium chloride, magnesium chloride, calcium chloride and magnesium sulfate.

[0037] Furthermore, the inorganic salt is magnesium chloride and / or calcium chloride.

[0038] Preferably, the magnesium chloride is anhydrous magnesium chloride.

[0039] Preferably, the calcium chloride is anhydrous calcium chloride.

[0040] Anhydrous calcium chloride has strong hygroscopicity. When it comes into contact with air, it will undergo a water absorption reaction as shown in the following formula (1):

[0041] CaCl2+6H2O=CaCl2·6H2O

[0042] Formula (1)

[0043] During the water absorption process, calcium chloride hexahydrate gradually turns into liquid and then completely dissolves in the absorbed water.

[0044] Similarly, magnesium chloride has a strong ability to absorb water, and the water absorption reaction that occurs is shown in the following formula (2):

[0045] MgCl2+6H2O=MgCl2·6H2O

[0046] Formula (2)

[0047] The small droplets formed by magnesium chloride will be dispersed in the micropores at the interface between the polyamide and the porous support layer, thereby having the effect of blocking gas.

[0048] Furthermore, the mass concentration of the aqueous solution is 4% to 12%, preferably 5% to 10%.

[0049] When the mass concentration of the inorganic salt aqueous solution is lower than 4%, the content of the introduced inorganic salt is low, which will lead to insufficient inorganic salt support during the heat treatment process, shrinkage of the pore structure, and reduction of the performance of the reverse osmosis membrane. At the same time, during the air tightness test, due to the insufficient droplet content after the inorganic salt absorbs moisture, the droplets cannot be evenly distributed in the cavities of the polyamide blades or the pores of the porous support layer, the gas isolation ability is reduced, and the air tightness of the membrane becomes worse; when the mass concentration of the inorganic salt aqueous solution is higher than 12%, the content of the introduced inorganic salt is too high, which will increase the difficulty of flushing the inorganic salt in the membrane. Before the membrane element is used, more water and longer flushing are required. In addition, when the solubility of the inorganic salt is too high, the reverse osmosis membrane will absorb too much water, making the membrane sticky, which is not conducive to the rolling of the membrane element.

[0050] Typically but not limiting, the mass concentration of the aqueous solution of inorganic salt can be, for example, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11% or 12%, or any value within the range of 4% to 12%.

[0051] Furthermore, the temperature of the aqueous solution is 35°C to 45°C.

[0052] When the temperature of the inorganic salt aqueous solution is lower than 35°C, the migration speed of the inorganic salt solution into the pores slows down during the immersion process, resulting in insufficient inorganic salt content in the pores, which is insufficient to maintain the pore structure during the heating process, and cannot effectively isolate the air and maintain good air tightness. When the temperature of the inorganic salt aqueous solution is higher than 45°C, the temperature is too high, which will have a negative impact on the original structure of the reverse osmosis membrane and reduce the performance of the reverse osmosis membrane.

[0053] Typically but not limiting, the temperature of the aqueous solution of inorganic salt can be, for example, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C or 45°C, or any value within the range of 35°C to 45°C.

[0054] Furthermore, the soaking time is 60s to 120s.

[0055] When the immersion time is less than 60 seconds, the inorganic salts that enter the pore structure of the reverse osmosis membrane are not sufficient to maintain the integrity of the pore structure and good air tightness; when the immersion time is 120 seconds, the migration of inorganic salts into the pores reaches equilibrium. When the immersion time is longer than 120 seconds, the production efficiency will be reduced.

[0056] Typically but not limiting, the soaking time may be, for example, 60 s, 70 s, 80 s, 90 s, 100 s, 110 s or 120 s, or any value within the range of 60 s to 120 s.

[0057] Further, excess moisturizing agent aqueous solution was removed using a pressure roller.

[0058] Furthermore, the drying temperature is 60° C. to 90° C., and the drying time is 3 min to 10 min.

[0059] Typically but not limitatively, the drying temperature can be, for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C, or any value within the range of 60°C to 90°C; the drying time can be, for example, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, or any value within the range of 3 min to 10 min.

[0060] Furthermore, the reverse osmosis membrane comprises a polyamide composite reverse osmosis membrane.

[0061] The second aspect of the present invention provides a reverse osmosis dry membrane, which is obtained by using the post-treatment method described in the first aspect.

[0062] The reverse osmosis dry membrane provided by the present invention has inorganic salts in the membrane structure, which replaces alcohol moisturizers such as glycerin, improves the pore-preserving effect and has no chemical dissolution, is more environmentally friendly, and is suitable for large-scale promotion and use.

[0063] The present invention is further described below by specific examples and comparative examples, but it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form. The raw materials used in the examples and comparative examples of the present invention, if no specific conditions are specified, are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0064] The reverse osmosis membranes used in the following examples and comparative examples are all polyamide composite reverse osmosis membranes, model XLP, produced by Beijing OriginWater Membrane Technology Co., Ltd.

[0065] Example 1

[0066] This embodiment provides a reverse osmosis dry membrane, and the specific preparation steps are as follows:

[0067] 1. Soak the polyamide composite reverse osmosis membrane in a calcium chloride solution for 60 seconds. The mass concentration of the calcium chloride solution is 5% and the temperature is 35°C.

[0068] 2. Use a roller to remove the calcium chloride solution remaining on the surface of the polyamide composite reverse osmosis membrane, and then place it in a 70°C oven for 5 minutes to obtain a reverse osmosis dry membrane.

[0069] Example 2

[0070] This embodiment provides a reverse osmosis dry membrane, and the specific preparation steps are as follows:

[0071] 1. Soak the polyamide composite reverse osmosis membrane in a magnesium chloride solution for 70 seconds. The mass concentration of the magnesium chloride solution is 8% and the temperature is 40°C.

[0072] 2. Use a roller to remove the magnesium chloride solution remaining on the surface of the polyamide composite reverse osmosis membrane, and then place it in an oven at 80°C for 4 minutes to obtain a reverse osmosis dry membrane.

[0073] Example 3

[0074] This embodiment provides a reverse osmosis dry membrane, and the specific preparation steps are as follows:

[0075] 1. Soak the polyamide composite reverse osmosis membrane in a composite solution for 80 seconds. The composite solution includes magnesium chloride and calcium chloride. The mass concentration of the magnesium chloride solution is 3%, the mass concentration of the calcium chloride solution is 3%, and the temperature of the composite solution is 45°C.

[0076] 2. Use a roller to remove the residual composite solution on the surface of the polyamide composite reverse osmosis membrane, and then place it in an oven at 80°C for 5 minutes to obtain a reverse osmosis dry membrane.

[0077] Example 4

[0078] This embodiment provides a reverse osmosis dry membrane. The difference from Embodiment 2 is that potassium chloride is used instead of magnesium chloride. The remaining raw materials and methods are the same as those in Embodiment 2 and will not be described again.

[0079] Example 5

[0080] This embodiment provides a reverse osmosis dry membrane. The difference from Embodiment 2 is that magnesium sulfate is used instead of magnesium chloride. The remaining raw materials and methods are the same as those in Embodiment 2 and will not be described again.

[0081] Example 6

[0082] This embodiment provides a reverse osmosis dry membrane. The difference from Embodiment 2 is that the mass concentration of the magnesium chloride solution is 4%. The remaining raw materials and methods are the same as those in Embodiment 2 and will not be described again.

[0083] Example 7

[0084] This embodiment provides a reverse osmosis dry membrane. The difference from Embodiment 2 is that the mass concentration of the magnesium chloride solution is 12%. The remaining raw materials and methods are the same as those in Embodiment 2 and will not be described again.

[0085] Example 8

[0086] This embodiment provides a reverse osmosis dry membrane. The difference from Embodiment 2 is that the mass concentration of the magnesium chloride solution is 2%. The remaining raw materials and methods are the same as those in Embodiment 2 and will not be described again.

[0087] Example 9

[0088] This embodiment provides a reverse osmosis dry membrane. The difference from Embodiment 2 is that the mass concentration of the magnesium chloride solution is 15%. The remaining raw materials and methods are the same as those in Embodiment 2 and will not be described again.

[0089] Example 10

[0090] This embodiment provides a reverse osmosis dry membrane. The difference from Embodiment 2 is that the polyamide composite reverse osmosis membrane is immersed in a magnesium chloride solution for 10 seconds. The remaining raw materials and methods are the same as those in Embodiment 2 and will not be described again.

[0091] Embodiment 11

[0092] This embodiment provides a reverse osmosis dry membrane. The difference from Embodiment 2 is that the polyamide composite reverse osmosis membrane is immersed in a magnesium chloride solution for 300 seconds. The remaining raw materials and methods are the same as those in Embodiment 2 and will not be described again.

[0093] Comparative Example 1

[0094] This comparative example provides a reverse osmosis membrane, which is the polyamide composite reverse osmosis membrane used in the embodiments and comparative examples, and the membrane is in a wet membrane state.

[0095] Comparative Example 2

[0096] This comparative example provides a reverse osmosis dry membrane. The polyamide composite reverse osmosis membrane is placed in an oven at 80° C. for 4 minutes to obtain a reverse osmosis dry membrane.

[0097] Comparative Example 3

[0098] This comparative example provides a reverse osmosis dry membrane, and the specific preparation steps are as follows:

[0099] 1. Soak the polyamide composite reverse osmosis membrane in a glycerol aqueous solution for 1 minute; the mass percentage of glycerol is 12% and the temperature is room temperature.

[0100] 2. Use a squeeze roller to remove excess water solution on the surface of the soaked membrane, and then dry the membrane at 80°C for 4 minutes to obtain a reverse osmosis dry membrane.

[0101] Characterization example

[0102] The reverse osmosis dry membrane obtained in Example 1 was subjected to a scanning electron microscope, and the surface electron microscope image of the reverse osmosis dry membrane was obtained as follows: Figure 2 As shown, the cross-sectional electron micrograph is Figure 3 shown.

[0103] from Figure 2 and Figure 3 It can be seen that the polyamide layer and the porous support layer of the reverse osmosis dry membrane have complete structures, the surface presents a large leaf morphology, and the cross-section shows that the leaves have a certain thickness and no collapse occurs, indicating that calcium chloride has good pore retention ability.

[0104] Test Example 1

[0105] The membranes provided in the embodiments and comparative examples were subjected to membrane performance tests, including membrane flux, salt rejection, air tightness and chemical dissolution content tests.

[0106] Diaphragm performance test conditions: 72.5 psi pressure, 500 mg / L NaCl solution, pre-pressing for 30 min.

[0107] Diaphragm airtightness: tested by airtight test bench, the effective area of ​​diaphragm is 36.34cm 2 Compressed air is blown into the membrane pool through a vacuum pump with a pressure of 0.4MPa. The gas that passes through the membrane enters the water through the pipe connected to the upper end of the membrane pool. The air tightness of the membrane is determined based on the number of bubbles in the water.

[0108] The obtained data are shown in Table 1 below.

[0109] Table 1

[0110]

[0111] As can be seen from Table 1, the performance flux of the wet membrane of Comparative Example 1 is 50LMH, and the desalination rate is 99.2%; Calcium chloride and magnesium chloride are used as humectants in Example 1 and Example 2, respectively. After heat treatment, the performance of the membrane is less different from that of the wet membrane, and no organic matter is dissolved, and it has good air tightness. Implementation Case 3 uses calcium chloride and magnesium chloride as a humectant, and the performance is equivalent to that of the wet membrane, and there are no bubbles. The composite inorganic salt has good pore and air tightness. Examples 4 and 5 illustrate that potassium chloride and magnesium sulfate can also be used as pore retainers for reverse osmosis membranes, and the performance after drying is not attenuated compared to wet membranes. Implementation Cases 6 and 7 use magnesium chloride as a humectant at concentrations of 4% and 12%, respectively. After drying, they have excellent flux and desalination performance, and good air tightness. When the solubility is reduced to 2% (Example 8), the flux and air tightness of the membrane are both attenuated. When the concentration was increased to 15% (Example 9), the desalination performance of the membrane decreased. This was because the inorganic salt concentration was too high, resulting in residual inorganic salts in the membrane for the same flushing time, resulting in a decrease in desalination rate. When the immersion time was 10s, the inorganic salt content in the membrane pores was low, resulting in a decrease in flux and air tightness. In Comparative Example 3, glycerol was used as a moisturizer, and TOC dissolution reached 5.92g / m 2 In the case of no moisturizing agent, the comparative example 2 has no water permeability when the membrane is dried.

[0112] Test Example 2

[0113] The reverse osmosis dry membranes obtained in the examples and comparative examples were subjected to stability tests. Specifically, the reverse osmosis dry membranes were stored in sealed bags, and the membrane performance and air tightness were tested every 30 days. The obtained data are shown in Table 2 below.

[0114] Table 2

[0115]

[0116] As can be seen from Table 2, the membranes of Examples 1, 2, 3, 4, 5, 6, 7, 9 and 11 were stored for 90 days, and there was no downward trend in flux, desalination and air tightness. The membranes with different storage times were rolled into components for air tightness detection. The component air tightness detection adopted a vacuum test method to detect the air tightness of the reverse osmosis membrane element. The principle is to judge whether there are defects by the decay rate of the pressure in the water bag of the membrane element under a certain air pressure value. The main test process is to connect the water outlet of the reverse osmosis element to the vacuum system, the vacuum degree is controlled at -80kPa, the pressure holding time is specified to be 5s, and the pressure drop value is <3kPa, then the element is qualified and there is no leak.

[0117] The test results are shown in Table 3.

[0118] Table 3

[0119]

[0120] As can be seen from Table 3, the pressure drop values ​​of the components made of the diaphragms of Examples 1, 2, 3, 4, 5, 6, 7, 9 and 11 are all less than 3 kPa. When an inorganic salt moisturizer is used, the concentration is greater than 4%, and the immersion time is greater than 60 s. The diaphragms have good stability during long-term storage, and inorganic salt moisturizers have broad application prospects.

[0121] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A post-treatment method for a reverse osmosis membrane, characterized in that: The reverse osmosis membrane is immersed in an aqueous solution of a moisturizer, and after completion, the excess aqueous solution of the moisturizer is removed, and then dried to obtain a reverse osmosis dry membrane; The humectant is an inorganic salt.

2. The post-processing method according to claim 1, characterized in that: The inorganic salt includes at least one of potassium chloride, magnesium chloride, calcium chloride and magnesium sulfate.

3. The post-processing method according to claim 1, characterized in that: The inorganic salt is magnesium chloride and / or calcium chloride; Preferably, the magnesium chloride is anhydrous magnesium chloride; Preferably, the calcium chloride is anhydrous calcium chloride.

4. The post-processing method according to any one of claims 1 to 3, characterized in that: The mass concentration of the aqueous solution is 4% to 12%, preferably 5% to 10%.

5. The post-processing method according to any one of claims 1 to 3, characterized in that: The temperature of the aqueous solution is 35°C to 45°C.

6. The post-processing method according to any one of claims 1 to 3, characterized in that: The soaking time is 60s to 120s.

7. The post-processing method according to any one of claims 1 to 3, characterized in that: Use a roller to remove excess moisturizer solution.

8. The post-processing method according to any one of claims 1 to 3, characterized in that: The drying temperature is 60° C. to 90° C., and the drying time is 3 min to 10 min.

9. The post-processing method according to any one of claims 1 to 3, characterized in that: The reverse osmosis membrane comprises a polyamide composite reverse osmosis membrane.

10. A reverse osmosis dry membrane, characterized in that: The product is obtained by the post-processing method according to any one of claims 1 to 9.

Citation Information

Cited By

  • High-flux reverse osmosis membrane and preparation method thereof

    CN119951353A