Process method for maintaining stability of water content of porous support layer in interfacial polymerization process of nanofiltration / reverse osmosis composite membrane

By controlling the water content of the porous support layer of the nanofiltration/reverse osmosis composite membrane and employing water spraying and sponge roller processes, the problem of membrane surface defects was solved, thereby improving the membrane's performance and appearance quality.

CN118904101APending Publication Date: 2024-11-08SHANDONG FUFAN TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118553.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the interfacial polymerization process of nanofiltration/reverse osmosis composite membranes, the unstable water content of the porous support layer leads to defects on the membrane surface, such as yellow spots and yellow patches, which affect the performance and appearance of the composite membrane. Existing processes are unable to effectively solve this problem.

Method used

By combining water spraying technology with sponge roller adsorption and spreading technology, the moisture content on the membrane surface is kept constant, ensuring that the monomers are evenly distributed on the base membrane surface. Excess moisture is removed by stainless steel air knife, and atomizing nozzles and sponge rollers are installed on the membrane surface to maintain the stability of moisture content.

Benefits of technology

This achieved uniform moisture distribution on the membrane surface, avoiding yellow spots and yellow patches, improving the performance stability and uniformity of the composite membrane, and enhancing the desalination rate and flux of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904101A_ABST
    Figure CN118904101A_ABST
Patent Text Reader

Abstract

The invention relates to the field of separation membranes, and discloses a process method for maintaining the stability of the water content of a porous support layer in the interfacial polymerization process of a nanofiltration / reverse osmosis composite membrane, which comprises the following steps: immersing a porous support layer base membrane in a monomer aqueous solution; blowing off most of redundant water solution on the surface of the film in the vertical direction by using an air knife; extruding redundant aqueous solution on the back surface of the film and in film holes by using a rubber extrusion roller; blowing off water drops on the front and back surfaces of the membrane by using air knives arranged on the front and back surfaces of the membrane; an atomizing device on which atomizing nozzles are distributed is mounted on the front surface of the diaphragm for spraying; the front surface of the membrane passes through a stick coated with sponge; and testing the water content and performance of the diaphragm. According to the preparation method, a water spraying process and a sponge roller adsorption spreading process are combined, so that the moisture content of the surface of the membrane is constant before the membrane enters an oil phase, the constancy of the interfacial polymerization reaction speed is ensured, and the membrane defects such as yellow spots are avoided; the performance of the composite membrane is improved, and the industrial application value is very good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of separation membranes, and in particular to a process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane. Background Art

[0002] With the continuous improvement of industrialization level, the problem of industrial wastewater pollution is becoming increasingly serious. In this context, reverse osmosis and nanofiltration have been widely used in the fields of seawater and brackish water desalination, wastewater and drinking water deep treatment. Membrane materials are the core of the entire separation process, and their performance determines the application scope and operating cost of membrane water treatment technology. Reverse osmosis and nanofiltration membranes have similar composite membrane structures, which are composed of a porous support layer, an ultra-thin functional separation layer, a functional modification layer, etc. The porous support layer is generally composed of non-woven fabrics and base membranes, which provide a good interface environment, mechanical strength, chemical and thermal stability for the preparation and application of nanofiltration / reverse osmosis.

[0003] In the past, many literature reports mainly improved the performance of composite membranes by optimizing the ultra-thin functional separation layer, and a small number of reports improved the structure and performance of composite membranes by optimizing the base membrane. The main methods to improve the performance of composite membranes include optimizing the base membrane process, optimizing the interfacial polymerization process, and developing new membrane making processes, including the pore size, porosity, surface hydrophilicity of the base membrane, water-oil phase monomer concentration, temperature, oven temperature, additives, etc. These process methods have more or less improved the performance of nanofiltration / reverse osmosis composite separation membranes to a certain degree of matching, but among these many methods, few people have mentioned the influence of the water content and stability of the porous support layer (base membrane) on the performance of the composite membrane before the membrane enters the oil phase during the interfacial polymerization process. In addition to being closely related to the monomer concentration, the interfacial polymerization reaction time and reaction degree are also related to the water content of the membrane: on the one hand, the water content of the membrane affects the volatilization rate of the solvent during interfacial polymerization. Within a certain range, the more water content, the slower the solvent evaporates, the longer the reaction time, the higher the polymer cross-linking degree, and the increased membrane desalination rate; on the other hand, the high water content of the membrane increases the humidity in the pre-curing stage, and the incompletely reacted acyl chloride groups will be hydrolyzed, which will increase the flux of the membrane to a certain extent. In fact, the surface water content of the porous support layer not only affects the reaction time and reaction degree of the interfacial polymerization, but also affects the generation of defects such as yellow spots and yellow spots in the composite membrane. Because the water content of the membrane is different, there is too little water in some places, and the organic monomer cannot diffuse into the water phase, so it does not react with the water phase monomer. Even if a trace amount of monomer reacts, the desalination layer formed is too thin. After the high-temperature curing of the membrane, the aniline and piperazine substances that do not participate in the reaction will be oxidized and yellowed, forming yellow spots and yellow spots, and the longer the storage time, the yellower the membrane. Many factories encounter defects such as yellow spots and yellow dots during the diaphragm production process. They have made great efforts and adjusted many process parameters, such as formula, reaction temperature, air knife air volume, etc., but none of them have fundamentally solved the problem. Summary of the invention

[0004] In order to overcome the defects of the prior art, the present invention provides a process for maintaining the stable water content of the porous support layer during the interfacial polymerization of the nanofiltration / reverse osmosis composite membrane, and the technical scheme thereof is as follows: A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane, comprising the following steps: (1) Immersing the porous support layer base membrane in a liquid phase tank containing a monomer aqueous solution; (2) Use an air knife to blow off most of the excess aqueous solution on the membrane surface in the vertical direction and make it flow back into the liquid phase tank; (3) Before the membrane enters the horizontal storage rack, use a rubber extrusion roller to squeeze out the excess aqueous solution on the back of the membrane and in the membrane pores. The squeezed solution flows vertically along the membrane into the liquid phase tank. (4) The diaphragm enters the storage rack, and the water droplets on both sides of the diaphragm are blown away by the air knives installed on the front and back sides of the diaphragm to prevent defects from being formed due to water droplets on the membrane surface during the interface reaction; (5) Because the temperature and humidity of the wind blown out by the wind knife are not uniform and constant, and the water content of the base membrane itself is also different in different batches, in order to maintain the constant moisture on the surface of the membrane pores, after the water droplets on the surface of the membrane are blown off, an atomizing device covered with atomizing nozzles is installed on the front of the membrane to ensure that the sprayed water mist is evenly distributed on the surface of the membrane, but not too much; (6) The areas with high water content on the diaphragm may form tiny water droplets after spraying. Therefore, before the diaphragm enters the liquid phase oil tank, the front of the diaphragm is passed through a stick covered with a sponge to allow the sponge to absorb the tiny water droplets, so that the water film is evenly distributed on the surface of the diaphragm to ensure a constant water content; (7) Testing the water content of the membrane after passing through the sponge-coated stick and before entering the oil phase tank; (8) The performance of the membrane is tested after the interfacial reaction in the oil phase tank.

[0005] Furthermore, the air knife in step (2) is a stainless steel air knife.

[0006] Furthermore, the spray width of the atomizing device in step (5) is consistent with the width of the diaphragm.

[0007] Furthermore, the operating pressure of the atomizing device in step (5) is 10-70 kg / cm.

[0008] Furthermore, the spray volume of the atomizing device in step (5) is 10-130cc / min.

[0009] Furthermore, the diameter of the atomizing nozzle in step (5) may be 0.1-0.5 mm.

[0010] Furthermore, the step (7) tests the water content of the membrane at three different operating positions.

[0011] Furthermore, in step (7), the water content of each position of the membrane is tested on both sides and in the middle.

[0012] Furthermore, the step (8) tests the performance of the membrane at three different operating positions corresponding to the water content test.

[0013] Furthermore, in step (8), the performance of the diaphragm is tested at both sides and in the middle of each position.

[0014] Compared with the existing process, the process of the present invention has the following advantages: 1. The present invention combines the water spray process with the sponge roller adsorption and spreading process to ensure that the moisture content of the membrane surface is constant before entering the oil phase, which can not only ensure the constant rate of interfacial polymerization reaction, but also avoid the membrane defect of uneven color on the membrane surface caused by the inconstant moisture content of the membrane due to the front wind knife, environment, and base membrane itself. Yellow spots are the main manifestation of membrane defects; some yellow spots are found to have no desalination layer after staining, which not only affects the appearance of the membrane, but also affects the performance of the membrane.

[0015] 2. The process of the present invention makes the water content of the porous support layer surface constant during the interfacial polymerization of the nanofiltration / reverse osmosis separation composite membrane, and the monomer can be well evenly distributed on the surface of the base membrane, which is conducive to generating a more uniform and smooth skin layer and improving the performance of the composite membrane.

[0016] 3. The present invention only slightly changes the original process to bring into play the unique advantage of stabilizing product performance and has good industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the basic process flow of the present invention. DETAILED DESCRIPTION

[0018] The process of the present invention is described in detail below by taking the production of nanofiltration membrane composite membrane as an example, so that people skilled in the art can more clearly understand the advantages of the present invention.

[0019] First, the flux and rejection rate test of the membrane, the moisture content test of the membrane and the interfacial polymerization time timing method of the present invention are briefly introduced as follows: 1. The composite nanofiltration membrane prepared by the present invention is first rinsed with deionized water and soaked for half an hour, and then pre-pressed for 0.5 hours at a test liquid of 2000ppm magnesium sulfate solution, a solution pH of 7.0±0.5, a temperature of 25.0±0.2, a membrane flow rate of ≥0.45m / s, and an operating pressure of 0.7Mpa, and finally the flux and retention rate of the membrane are tested.

[0020] The membrane flux calculation formula is shown in (1): F= V / (T×A)........................(1) F is the membrane flux (L / m 2 h); V is the volume of the permeable liquid (L); T is the time required to collect V volume of permeate (h); A is the effective membrane area (m 2 ).

[0021] The ion removal rate of the membrane is shown in (2): R = (1-C p ÷C f )×100%.....................(2) R is the removal rate; C p is the content of ions in the permeate, expressed in mg / l; C f is the content of ions in the test solution, in mg / l; 2. The moisture content test of the membrane of the present invention adopts the German Coli M50S non-contact online microwave moisture meter / moisture sensor.

[0022] 3. The interfacial polymerization time is measured by a stopwatch, starting from the time when the base film enters the oil phase and ending when the organic solvent on the membrane surface evaporates.

[0023] Then, the process of the present invention is described in detail in the form of examples, but they should not be understood as specific limitations on the scope of protection of the present invention. Example 1

[0024] The nanofiltration composite membrane is produced according to the following steps and the surface water content of the porous polysulfone support layer is kept constant during the interfacial polymerization reaction. 1) The reverse osmosis membrane production line equipment is started, and the equipment runs at a speed of 2m / min. The unwinding is driven by a servo motor to pull the ultrafiltration base membrane into a 6% piperazine aqueous solution for 30s. 2) The stainless steel air knife blows off most of the excess aqueous solution on the surface in the vertical direction, so that it flows into the liquid phase tank again. 3) Before the membrane enters the horizontal storage rack, the excess aqueous solution on the back of the membrane and the membrane pores is squeezed out with a rubber extrusion roller, and the squeezed solution flows into the liquid phase water tank along the membrane in the vertical direction. 4) Then the membrane enters the storage rack, and air knives are set on both sides of the membrane. The air knives are used to blow off the water droplets on both sides of the membrane. Water droplets on the membrane surface will form defects during the interfacial reaction. 5) An atomization device is installed on the front of the membrane, with the same width as the membrane, and it is covered with atomization nozzles to ensure that the water mist is evenly distributed on the surface of the membrane. The diameter of the atomizing nozzle can be 0.1mm, the operating pressure is 10kg / cm, and the spray volume is 10cc / min. 6) Before entering the oil phase, the front of the diaphragm must pass through a stick covered with a sponge to allow the sponge to absorb tiny water droplets, so that the water film is evenly distributed on the surface of the diaphragm and the water content is constant. When the equipment runs for 10 meters, 100 meters, and 500 meters, the horizontal average sampling is taken 3 times, and the water content on both sides and in the middle of the diaphragm is tested and recorded; the diaphragm enters the 0.3% benzyl chloride oil phase for interfacial reaction, and the interfacial polymerization reaction time is 20s. There are no defects such as yellow spots and yellow spots on the surface of the diaphragm. Finally, the performance of the diaphragms near 10 meters, 100 meters, and 500 meters is tested. Example 2

[0025] The diameter of the atomizing nozzle in Example 1 was changed to 0.3 mm, the operating pressure was 50 kg / cm, the spray volume was 60 cc / min, the interfacial polymerization reaction time was 25 s, and the other process remained unchanged. Example 3

[0026] The diameter of the atomizing nozzle in Example 1 was changed to 0.5 mm, the operating pressure was 70 kg / cm, the spray volume was 100 cc / min, the interfacial polymerization reaction time was 30 s, and the other process remained unchanged.

[0027] Comparative Example The spray device in Example 1 was turned off, the sponge on the last support stick was removed, the interfacial polymerization reaction time was 15 s, and the other processes were the same as in Example 1.

[0028] The water content, corresponding interfacial polymerization time and membrane performance of different lengths and positions of membranes in Examples 1-3 and Comparative Examples were compared, and the results are shown in Tables 1, 2 and 3: Table 1 Comparison of water content of membranes at different lengths and positions ; Table 2 Comparison of interface polymerization time corresponding to different meters and different positions ; Table 3 Comparison of membrane performance at different lengths and positions ; As can be seen from Table 1, the water content of the membranes in Examples 1-3 is different with different spray amounts. The greater the spray amount, the greater the water content of the membrane. Compared with the comparative example, the water content of different positions of the membrane with the spray process added after the air knife is more uniform; the water content of the membrane in the comparative example is not only lower than that of the embodiment, but also the water content of the membrane will change with the increase of local space humidity and the generation of mechanical heat energy of the air knife.

[0029] It can be seen from Table 2 that in Examples 1-3 and the comparative example, the higher the water content of the membrane, the longer the interface reaction time, the higher the water content, the less likely the organic phase solution will evaporate quickly on the surface of the base membrane, and it is easier to maintain the uniformity and integrity of the solution interface.

[0030] It can be seen from Table 3 that: (1) When the reaction time is less than 10s, due to the incomplete reaction of the two-phase monomers, the cross-linking degree is low and the desalination cortex is thin, which will make the flux of the reverse osmosis composite membrane larger and the desalination rate lower. (2) As the reaction time increases, the degree of reaction further deepens, a cortex with a high degree of cross-linking will be formed, and the thickness of the cortex will also increase, resulting in a corresponding decrease in flux and an increase in desalination rate. In addition to the increase in the water content of the base membrane and the increase in the interfacial polymerization time in Example 1-3, the water content also affects the hydrolysis of the incompletely reacted acyl chloride groups. The higher the degree of hydrolysis, the higher the membrane flux. These factors combined make the membrane water content in the range of 20%-30%, and the membrane performance increases with the increase in the water content of the base membrane. (3) In the comparative example, the desalination rate of the membrane on the left side of 200m is too low, only 88.32%. Three or four yellow spots can be seen under the light. The membrane with yellow spots turns red when stained with rhodamine B solution, indicating that the membrane has no desalination layer at this point. Before the base membrane enters the oil phase, the membrane with yellow spots is blown too dry, which affects the diffusion of the water phase monomer into the oil phase and the polymerization reaction is incomplete. This is also one of the reasons why yellow spots appear on the membrane during industrial production.

Claims

1. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane, characterized in that: The following steps are involved: (1) Immersing the porous support layer base membrane in a liquid phase tank containing a monomer aqueous solution; (2) Use an air knife to blow off most of the excess aqueous solution on the membrane surface in the vertical direction and make it flow back into the liquid phase tank; (3) Before the membrane enters the horizontal storage rack, use a rubber extrusion roller to squeeze out the excess aqueous solution on the back of the membrane and in the membrane pores. The squeezed solution flows vertically along the membrane into the liquid phase tank. (4) The diaphragm enters the storage rack, and the water droplets on both sides of the diaphragm are blown away by the wind knives set on the front and back sides of the diaphragm; (5) Install an atomizing device covered with atomizing nozzles on the front of the diaphragm to ensure that the sprayed water mist is evenly distributed on the surface of the diaphragm; (6) Before the membrane enters the oil phase tank, the front of the membrane passes through a stick covered with a sponge to allow the sponge to absorb tiny water droplets, so that the water film is evenly distributed on the surface of the membrane to ensure a constant water content; (7) Testing the water content of the membrane after passing through the sponge-coated stick and before entering the oil phase tank; (8) The performance of the membrane is tested after the interfacial reaction in the oil phase tank.

2. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane according to claim 1, characterized in that: The air knife in step (2) is a stainless steel air knife.

3. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane according to claim 1, characterized in that: The spray width of the atomizing device in step (5) is consistent with the width of the diaphragm.

4. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane according to claim 1, characterized in that: The operating pressure of the atomizing device in step (5) is 10-70 kg / cm.

5. The process for maintaining stable water content of the porous support layer during interfacial polymerization of nanofiltration / reverse osmosis composite membrane according to claim 1, characterized in that: The spray volume of the atomizing device in step (5) is 10-130cc / min.

6. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane according to claim 1, characterized in that: The diameter of the atomizing nozzle in step (5) may be 0.1-0.5 mm.

7. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane according to claim 1, characterized in that: The step (7) tests the water content of the membrane at three different operating positions.

8. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane according to claim 7, characterized in that: The step (7) tests the water content at both sides and the middle of each position of the membrane.

9. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane according to claim 1, characterized in that: The step (8) tests the performance of the membrane at three different operating positions corresponding to the water content test.

10. A process for maintaining stable water content of a porous support layer during interfacial polymerization of a nanofiltration / reverse osmosis composite membrane according to claim 9, characterized in that: The step (8) tests the performance of the diaphragm at both sides and in the middle of each position.