Polyimide mixed matrix membrane as well as preparation method and application thereof
By using a polyimide mixed matrix membrane with fluoropolymer matrix combined with MOF glass in the helium separation membrane, the problem of insufficient selectivity and permeability of the existing helium separation membrane is solved, and high-efficiency helium is achieved The effect of separation.
Patent Information
- Application Number
- CN202411000758.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The existing helium separation membrane has low selectivity and poor gas permeability, making it difficult to meet the needs of efficient helium separation.
A polyimide mixed matrix film with a fluoropolyimide matrix bonded with MOF glass (ZIF-62 and ZIF-8) was prepared by mold compression and heat treatment, and the spherical MOF glass was prepared with fluoropolyimide. The amine matrix is dissolved and dispersed in DMF to form a film structure, which improves the selectivity and permeability of helium.
High helium flux and good helium selectivity were achieved, the helium flux reached 351GPU, and the He/CH4, He/N2 and He/CO2 selectivity reached 390.0, 292.5 and 234.0 respectively, which significantly improved the helium separation performance. .
Smart Images

Figure CN118904120A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of gas separation membranes, and in particular to a polyimide mixed matrix membrane and a preparation method and application thereof. Background Art
[0002] Helium is a strategic special gas with low density, low boiling point and inert properties. It plays an important role in high-tech industries and scientific research. Helium is widely distributed on the earth as trace components, but helium extraction from helium-containing natural gas is still the only way to produce helium industrially. With the development of the economy, my country's demand for helium has grown rapidly. China's helium natural gas has the characteristics of many types and good resource prospects, but the overall research level of helium resources is very low. In order to meet the demand for helium resources, it is urgent to develop a method for preparing high-purity helium with low energy consumption.
[0003] In recent years, membrane separation has gradually been applied in the field of helium purification. The membrane separation method is driven by the pressure difference on both sides of the membrane, and uses the difference in permeability of each component in the gas during the dissolution, diffusion, and desorption process to achieve the separation effect. The membrane separation method is simple to operate, has low energy consumption, low equipment construction and operation costs, and is highly competitive. Designing a helium separation membrane with high helium selectivity and high gas flux is of great strategic significance for achieving economic helium extraction from natural gas, reducing dependence on helium imports, and achieving autonomy in helium production and use.
[0004] The preparation of high permeability and high selectivity gas separation membrane materials is the key to achieving efficient separation. In the study of hybrid mechanism membranes, there are generally problems of poor compatibility between materials and low selectivity. In order to improve the compatibility between the matrix and the filler, the literature [ACS Sustain. Chem. Eng., 2021, 9, 1814] coated polydopamine (PDA) on the surface of ZIF-8 to improve the MOF-polymer interface compatibility and He separation performance. Existing MMMs materials all take the modification of MOF to affect the selective permeability of mixed matrix membranes, ignoring the modification of the matrix structure to improve the comprehensive performance of MMMs. MOF glass membrane is an isotropic MOF material without grain boundaries. Patent CN202110640619.9 provides a method for preparing a self-supporting glass ZIF 62MOF membrane for CH4 / N2 separation. The glass MOF membrane prepared by this method has no grain boundaries and defects, and has good gas separation selectivity, but poor gas permeability. The glassy porosity is inevitably reduced, which is not conducive to membrane performance optimization.
[0005] Therefore, how to improve gas separation selectivity and gas permeability is still a problem that needs to be solved for helium separation membranes. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a polyimide mixed matrix membrane and a preparation method and application thereof, so as to at least solve the problems of low selectivity and poor gas permeability of existing gas separation membranes when used for helium separation.
[0007] The present invention solves the above technical problems by the following technical means:
[0008] In a first aspect, the present invention provides a polyimide mixed matrix membrane, comprising 5 to 20 wt % of a fluorine-containing polyimide matrix and 80 to 95 wt % of MOF glass.
[0009] In combination with the first aspect, in some embodiments, the MOF glass includes 40 to 70 wt % of ZIF-62 and 30 to 60 wt % of ZIF-8.
[0010] In a second aspect, the present invention provides a method for preparing a polyimide mixed matrix membrane, comprising the following steps:
[0011] In an argon atmosphere, ZIF-62 and ZIF-8 were mixed and pressed using a mold, then heated to 440-450°C for 6-12 minutes and cooled naturally to obtain a spherical mixture MOF glass.
[0012] Under nitrogen protection, diamine monomer, m-cresol and 4,4'-(hexafluoroisopropylene) diphthalic anhydride are mixed, isoquinoline is added dropwise, the temperature is raised to 80-180°C for reaction for 9-10 hours, and then the temperature is 190-200°C for reaction for 12-15 hours. After the reaction is completed, the temperature is cooled to 55-60°C, the obtained reaction solution is poured into methanol for drawing precipitation, washed and filtered, and then dried to obtain the FPI matrix;
[0013] According to 5-25wt% of fluorinated polyimide matrix and 80-95wt% of MOF glass, the FPI matrix is added to DMF, stirred and dissolved to obtain an FPI solution, the MOF glass is stirred and dispersed in DMF to obtain a MOF glass solution, the MOF glass solution is added to the FPI solution under stirring, stirred and ultrasonically dispersed, and then allowed to stand for degassing, coated on a smooth glass plate to be cast into a film, dried, demolded, and activated to obtain a MOF glass / FPI mixed matrix membrane.
[0014] In combination with the second aspect, in some embodiments, in the MOF glass, the mass fraction of ZIF-62 is 40 to 70 wt %, and the mass fraction of ZIF-8 is 30 to 60 wt %.
[0015] In conjunction with the second aspect, in some embodiments, the preparation method of ZIF-62 is as follows:
[0016] Zn(NO3)2·6H2O and imidazole were added to N,N-dimethylformamide and stirred respectively, and then the two solutions were mixed and stirred, and then benzimidazole was added and stirred, and the obtained mixed solution was heated to 130-140°C for reaction for 48-50h, cooled to room temperature, vacuum filtered, and the precipitate was washed with N,N-dimethylformamide and dichloromethane, and then dried at 150-155°C to obtain ZIF-62;
[0017] The molar ratio of Zn(NO3)2·6H2O to imidazole is (0.070-0.080):(1.60-1.80), and the molar ratio of Zn(NO3)2·6H2O to benzimidazole is 1:1.
[0018] In conjunction with the second aspect, in some embodiments, the preparation method of ZIF-8 is as follows:
[0019] ZnCl2 and 2-methylimidazole were added to methanol respectively and stirred, and then the two solutions were mixed and stirred, and allowed to stand at room temperature for 4 to 5 hours, centrifuged and filtered, and the precipitate was washed with methanol, and then dried in a vacuum oven at 110 to 120°C for 12 to 15 hours to obtain ZIF-8.
[0020] In conjunction with the second aspect, in some embodiments, the molar ratio of the diamine monomer to 4,4'-(hexafluoroisopropylene) diphthalic anhydride is 1:1.
[0021] In combination with the second aspect, in some embodiments, the diamine monomer is one of 4-(3-fluoro-4-trifluoromethylphenyl)-2,6-bis-(4-aminophenyl)-pyridine, 4,4'-((perfluoropropane-2,2-diyl)bis(4,1-phenylsulfonyl))diphenylamine, 4,4'-diaminodiphenyl ether, and 4,6-diaminoresorcinol hydrochloride.
[0022] In combination with the second aspect, in some embodiments, the activation condition is maintained in a vacuum environment at 160-180° C. for 24-36 hours.
[0023] In a third aspect, the present invention provides use of the polyimide mixed matrix membrane described in the first aspect or the polyimide mixed matrix membrane prepared by the preparation method described in the second aspect in helium separation.
[0024] The polyimide mixed matrix membrane of the present invention, on the one hand, has good hydrophobic properties by introducing a fluorinated polyimide matrix, and can improve the helium permeability of the mixed matrix membrane; on the other hand, by utilizing the good compatibility of ZIF-62 and ZIF-8 in MOF glass, the prepared MOF glass mixed matrix membrane has almost no interface defects, and the thermal stability of the mixed matrix membrane is improved. At the same time, the pore structure characteristics of ZIF-8 ensure high gas flux, thereby constructing a polyimide mixed matrix membrane with an ideal interface structure, high flux and good selectivity for helium.
[0025] According to experiments, the helium flux of the polyimide mixed matrix membrane of the present invention is as high as 351GPU, and the He / CH4, He / N2 and He / CO2 selectivities are 390.0, 292.5 and 234.0 respectively. Both the helium flux and the helium selectivity are excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the process of preparing a polyimide mixed matrix membrane. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The raw materials, equipment or instruments used, if no manufacturer is specified, are all conventional products that can be purchased on the market.
[0029] The English letters in the present invention are interpreted as follows:
[0030] FTPPA: 4-(3-fluoro-4-trifluoromethylphenyl)-2,6-bis-(4-aminophenyl)-pyridine;
[0031] ODA: 4,4'-diaminodiphenyl ether;
[0032] DAR: 4,6-diaminoresorcinol hydrochloride;
[0033] 6FDA: 4,4'-(hexafluoroisopropylene) diphthalic anhydride;
[0034] DMF: N,N-dimethylformamide;
[0035] DCM: dichloromethane;
[0036] BASA: 4,4'-((perfluoropropane-2,2-diyl)bis(4,1-phenylsulfonyl))diphenylamine, its chemical structure is as follows:
[0037]
[0038] The present invention provides a polyimide mixed matrix membrane and a preparation method and application thereof. The comprehensive performance of a polyimide polymer matrix is improved by molecular design, and the good compatibility of ZIF-62 and ZIF-8 in MOF glass is utilized to make the prepared MOF glass mixed matrix membrane almost free of interface defects. At the same time, the pore structure characteristics of ZIF-8 ensure high gas flux, thereby constructing a polyimide mixed matrix membrane with an ideal interface structure, high flux and good selectivity.
[0039] The polyimide mixed matrix membrane of the present invention comprises 5-20wt% of a fluorinated polyimide matrix and 80-95wt% of MOF glass, wherein the fluorinated polyimide matrix is one of 6FDA-FTPPA, 6FDA-BASA, 6FDA-ODA and 6FDA-DAR, and the MOF glass comprises 40-70wt% of ZIF-62 and 30-60wt% of ZIF-8.
[0040] Please refer to Figure 1 The method for preparing the polyimide mixed matrix membrane of the present invention comprises the following steps:
[0041] In an argon atmosphere, ZIF-62 and ZIF-8 were mixed and pressed using a mold, then heated to 440-450°C for 6-12 minutes and cooled naturally to obtain a spherical mixture MOF glass.
[0042] Under nitrogen protection, diamine monomer, m-cresol and 4,4'-(hexafluoroisopropylene) diphthalic anhydride are mixed, isoquinoline is added dropwise, the temperature is raised to 80-180°C for reaction for 9-10 hours, and then the temperature is 190-200°C for reaction for 12-15 hours. After the reaction is completed, the temperature is cooled to 55-60°C, the obtained reaction solution is poured into methanol for drawing precipitation, washed and filtered, and then dried to obtain the FPI matrix;
[0043] According to 5-25wt% of fluorinated polyimide matrix and 80-95wt% of MOF glass, the FPI matrix is added to DMF, stirred and dissolved to obtain an FPI solution, the MOF glass is stirred and dispersed in DMF to obtain a MOF glass solution, the MOF glass solution is added to the FPI solution under stirring, stirred and ultrasonically dispersed, and then allowed to stand for degassing, coated on a smooth glass plate to be cast into a film, dried, demolded, and activated to obtain a MOF glass / FPI mixed matrix membrane.
[0044] For details, please refer to Examples 1-7:
[0045] Example 1
[0046] The polyimide mixed matrix membrane of this embodiment includes 5 wt % of a fluorine-containing polyimide matrix and 95 wt % of MOF glass.
[0047] In the present embodiment, the preparation method of ZIF-62 is as follows:
[0048] Zn(NO3)2·6H2O was added to N,N-dimethylformamide and stirred to obtain a metal salt solution with a Zn(NO3)2·6H2O concentration of 0.075 mol / L. Imidazole was added to N,N-dimethylformamide and stirred to obtain a ligand solution with an imidazole concentration of 1.75 mol / L. The two solutions were then mixed in equal volumes and stirred to mix. An equal amount of benzimidazole to Zn(NO3)2·6H2O was added and stirred. The obtained mixed solution was heated to 135°C and reacted for 48 hours. The mixture was cooled to room temperature and vacuum filtered. The precipitate was washed with equal amounts of N,N-dimethylformamide and dichloromethane and then dried at 150-155°C overnight to obtain ZIF-62.
[0049] The preparation method of ZIF-8 is as follows:
[0050] ZnCl2 was added to methanol and stirred to obtain a metal salt solution with a ZnCl2 concentration of 0.13 mol / L, 2-methylimidazole was added to methanol and stirred to obtain a ligand solution with a 2-methylimidazole concentration of 2.1 mol / L, and the two solutions were then mixed and stirred, allowed to stand at room temperature for 5 h, centrifuged and filtered, the precipitate was washed with methanol, and then dried in a vacuum oven at 110-120°C for 15 h to obtain ZIF-8.
[0051] The preparation method of the polyimide mixed matrix membrane of this embodiment is as follows:
[0052] (1) Preparation of ZIF-62@ZIF-8MOF glass
[0053] Under an argon atmosphere, 70 wt% of ZIF-62 and 30 wt% of ZIF-8 were mixed together, pressed using a mold, and then heated to 440°C for 6 min and cooled naturally to obtain a spherical mixture, thereby obtaining MOF glass.
[0054] (2) Preparation of FPI (6FDA-DAR) matrix
[0055] Under nitrogen protection, m-cresol (33.6 mL) containing DAR (6.0 mmol, 1.18 g) was added to a 100 mL three-necked flask to obtain a diamine monomer solution. Under continuous stirring, 6FDA (5.9 mmol, 2.66 g) was added to the diamine monomer solution, stirred and heated to 50 ° C to fully dissolve, and 5 drops of isoquinoline were added. The temperature was raised to 80 ° C for reaction for 3 h, then raised to 120 ° C for reaction for 3 h, then raised to 180 ° C for reaction for 3 h, and finally raised to 200 ° C for reaction for 12 h. After the reaction was completed, it was cooled to 55 ° C, and the viscous solution was poured into 500 mL of methanol for drawing precipitation. After multiple washing and filtration, it was placed in an oven to dry to obtain the FPI matrix.
[0056] (3) Preparation of MOF glass / fluorinated polyimide mixed matrix membrane
[0057] The FPI matrix prepared in step (2) is added to DMF, stirred and dissolved to obtain an FPI solution, the MOF glass is stirred and dispersed in DMF to obtain a MOF glass solution, the MOF glass solution is added to the FPI solution while stirring, and after stirring and ultrasonic dispersion, it is allowed to stand for 5 hours to degas to form a casting liquid, and the casting liquid is evenly coated on a glass plate by a casting method to form a film, and the solvent is removed and dried in a vacuum oven at 80°C for 12 hours. The formed mixed film is placed in an oven for evacuation, and maintained at 170°C for 24 hours to remove the solvent and reactivate to obtain a ZIF-62@ZIF-8MOF glass / 6FDA-DAR mixed matrix membrane.
[0058] Example 2
[0059] The polyimide mixed matrix membrane of this embodiment includes 5wt% of a fluorine-containing polyimide matrix and 95wt% of MOF glass. The preparation method of the polyimide mixed matrix membrane of this embodiment is as follows:
[0060] In the present embodiment, the preparation method of ZIF-62 is as follows:
[0061] Zn(NO3)2·6H2O was added to N,N-dimethylformamide and stirred to obtain a metal salt solution with a Zn(NO3)2·6H2O concentration of 0.070 mol / L. Imidazole was added to N,N-dimethylformamide and stirred to obtain a ligand solution with an imidazole concentration of 1.70 mol / L. The two solutions were then mixed in equal volumes and stirred to mix. An equal amount of benzimidazole to Zn(NO3)2·6H2O was added and stirred. The obtained mixed solution was heated to 130°C for reaction for 50 hours, cooled to room temperature, vacuum filtered, and the precipitate was washed with equal amounts of N,N-dimethylformamide and dichloromethane. It was then dried at 150-155°C overnight to obtain ZIF-62.
[0062] The preparation method of ZIF-8 is as follows:
[0063] ZnCl2 was added to methanol and stirred to obtain a metal salt solution with a ZnCl2 concentration of 0.13 mol / L. 2-Methylimidazole was added to methanol and stirred to obtain a ligand solution with a 2-methylimidazole concentration of 2.1 mol / L. The two solutions were then mixed in equal volumes and stirred to mix well. The mixture was allowed to stand at room temperature for 4 h, filtered by centrifugation, and the precipitate was washed with methanol. The mixture was then dried in a vacuum oven at 110-120°C for 12 h to obtain ZIF-8.
[0064] (1) Preparation of MOF glass
[0065] In an argon atmosphere, 40 wt% of ZIF-62 and 60 wt% of ZIF-8 were mixed together, pressed using a mold, and then heated to 445°C for 12 min and cooled naturally to obtain a spherical mixture, thereby obtaining MOF glass.
[0066] (2) Preparation of FPI (6FDA-BASA) matrix
[0067] In a 50mL three-necked flask equipped with a stirrer, N2 inlet, condenser and oil bath, BASA (1.00g, 1.63mmol), 6FDA (0.68g, 1.63mmol), m-cresol (19.00mL) and isoquinoline (3 drops) were added in sequence, heated to 60°C to completely dissolve the reactants, then heated to 80°C for 3h, then heated to 120°C for 3h, then heated to 180°C for 3h, and finally heated to 200°C for 14h. The product obtained by the reaction was cooled to room temperature, slowly poured into 300mL methanol for wire drawing precipitation, filtered, and then dried, dissolved, wire drawing, and purified. The final product was vacuum dried at 160°C for 12h to obtain FPI (6FDA-BASA) substrate.
[0068] (3) Preparation of MOF glass / fluorinated polyimide mixed matrix membrane
[0069] The FPI matrix prepared in step (2) is added to DMF, stirred and dissolved to obtain an FPI solution, the MOF glass is stirred and dispersed in DMF to obtain a MOF glass solution, the MOF glass solution is added to the FPI solution while stirring, and after stirring and ultrasonic dispersion, it is allowed to stand for 5 hours to degas to form a casting liquid, and the casting liquid is evenly coated on a glass plate by a casting method to form a film, and the solvent is removed and dried in a vacuum oven at 80°C for 12 hours. The formed mixed film is placed in an oven for evacuation, and maintained at 180°C for 30 hours to remove the solvent and reactivate to obtain a ZIF-62@ZIF-8MOF glass / 6FDA-BASA mixed matrix membrane.
[0070] Example 3
[0071] The polyimide mixed matrix membrane of this embodiment includes 5wt% of a fluorine-containing polyimide matrix and 95wt% of MOF glass. The preparation method of the polyimide mixed matrix membrane of this embodiment is as follows:
[0072] The preparation method of ZIF-62 and ZIF-8 in this example is the same as that in Example 1.
[0073] (1) Preparation of MOF glass
[0074] The preparation method of MOF glass is the same as that in Example 1 without any changes.
[0075] (2) Preparation of fluorinated polyimide FPI
[0076] Under nitrogen protection, FTPPA (6.0mmol, 2.4g) and m-cresol (17mL) were added to a 50mL three-necked flask. When FTPPA was completely dissolved, 6FDA (5.9mmol, 3.0g), m-cresol (17mL) and isoquinoline (6 drops) were added to the three-necked flask, stirred and heated to 60℃ for full dissolution, then heated to 80℃ for 3h, 120℃ for 4h, 180℃ for 3h, and finally 190℃ for 15h. After the reaction was completed, it was cooled to room temperature, and the viscous product solution was poured into 500mL methanol for drawing precipitation. After washing and filtering, it was placed in an oven to dry to obtain fibrous polyimide. The polyimide was then redissolved in DMF, purified by secondary precipitation, and dried to obtain the FPI (6FDA-FTPPA) substrate.
[0077] (3) Preparation of MOF glass / fluorinated polyimide mixed matrix membrane
[0078] The FPI matrix prepared in step (2) is added to DMF, stirred and dissolved to obtain an FPI solution, the MOF glass is stirred and dispersed in DMF to obtain a MOF glass solution, the MOF glass solution is added to the FPI solution while stirring, and after stirring and ultrasonic dispersion, it is allowed to stand for 5 hours to degas to form a casting liquid, and the casting liquid is evenly coated on a glass plate by a casting method to form a film, and the solvent is removed and dried in a vacuum oven at 80°C for 12 hours. The formed mixed film is placed in a vacuum oven and evacuated, and maintained at 160°C for 36 hours to remove the solvent and reactivate to obtain a ZIF-62@ZIF-8MOF glass / 6FDA-FTPPA mixed matrix membrane.
[0079] Example 4
[0080] The polyimide mixed matrix membrane of this embodiment includes 10 wt % of a fluorine-containing polyimide matrix and 90 wt % of MOF glass. The steps and conditions of the preparation method thereof are the same as those of Example 3.
[0081] Example 5
[0082] The polyimide mixed matrix membrane of this embodiment includes 15 wt % of a fluorine-containing polyimide matrix and 85 wt % of MOF glass. The steps and conditions of the preparation method thereof are the same as those of Example 3.
[0083] Example 6
[0084] The polyimide mixed matrix membrane of this embodiment includes 20 wt % of a fluorine-containing polyimide matrix and 80 wt % of MOF glass. The steps and conditions of the preparation method thereof are the same as those of Example 3.
[0085] Example 7
[0086] The polyimide mixed matrix membrane of this embodiment includes 5wt% of fluorine-containing polyimide matrix and 95wt% of MOF glass. The preparation method of the polyimide mixed matrix membrane of this embodiment is as follows:
[0087] In the present embodiment, the preparation method of ZIF-62 is as follows:
[0088] Zn(NO3)2·6H2O was added to N,N-dimethylformamide and stirred to obtain a metal salt solution with a Zn(NO3)2·6H2O concentration of 0.080 mol / L. Imidazole was added to N,N-dimethylformamide and stirred to obtain a ligand solution with an imidazole concentration of 1.80 mol / L. The two solutions were then mixed in equal volumes and stirred to mix. An equal amount of benzimidazole to Zn(NO3)2·6H2O was added and stirred. The obtained mixed solution was heated to 140°C and reacted for 48 hours. The mixture was cooled to room temperature and vacuum filtered. The precipitate was washed with equal amounts of N,N-dimethylformamide and dichloromethane and then dried at 150-155°C overnight to obtain ZIF-62.
[0089] The preparation method of ZIF-8 is as follows:
[0090] ZnCl2 was added to methanol and stirred to obtain a metal salt solution with a ZnCl2 concentration of 0.13 mol / L. 2-Methylimidazole was added to methanol and stirred to obtain a ligand solution with a 2-methylimidazole concentration of 2.1 mol / L. The two solutions were then mixed in equal volumes and stirred to mix well. The mixture was allowed to stand at room temperature for 5 h, filtered by centrifugation, and the precipitate was washed with methanol. The mixture was then dried in a vacuum oven at 110-120°C for 15 h to obtain ZIF-8.
[0091] (1) Preparation of MOF glass
[0092] The preparation method of MOF glass is the same as that in Example 1 without any changes.
[0093] (2) Preparation of FPI (6FDA-ODA) matrix
[0094] Under nitrogen protection, m-cresol (33.6 mL) containing ODA (6.0 mmol, 1.2 g) was added to a 100 mL three-necked flask. Under continuous stirring, 6FDA (5.9 mmol, 2.66 g) was added to the solution, stirred and heated to 50 °C for full dissolution. After adding 6 drops of isoquinoline, the temperature was raised to 80 °C for 3 h, 120 °C for 4 h, 180 °C for 3 h, and finally 200 °C for 14 h. After the reaction was completed, it was cooled to 60 °C, and the viscous solution was poured into 500 mL of methanol for drawing precipitation. After multiple washing and filtration, it was placed in an oven to dry for 12 h to obtain the FPI (6FDA-ODA) matrix.
[0095] (3) Preparation of MOF glass-polyimide mixed matrix membrane
[0096] The FPI matrix prepared in step (2) is added to DMF, stirred and dissolved to obtain an FPI solution, the MOF glass is stirred and dispersed in DMF to obtain a MOF glass solution, the MOF glass solution is added to the FPI solution while stirring, and after stirring and ultrasonic dispersion, it is allowed to stand for 5 hours to degas to form a casting liquid, and the casting liquid is evenly coated on a glass plate by a casting method to form a film, and the solvent is removed and dried in a vacuum oven at 80°C for 12 hours. The formed mixed film is placed in an oven for evacuation, and maintained at 170°C for 30 hours to remove the solvent and reactivate to obtain a ZIF-62@ZIF-8MOF glass / 6FDA-ODA mixed matrix membrane.
[0097] Comparative Example 1
[0098] The gas separation membrane of this embodiment is 100 wt % MOF glass.
[0099] The preparation method of the gas separation membrane of this embodiment is as follows:
[0100] (1) Preparation of ZIF-62@ZIF-8MOF glass
[0101] Under an argon atmosphere, 70 wt% of ZIF-62 and 30 wt% of ZIF-8 were mixed together, pressed using a mold, and then heated to 440°C for 6 min and cooled naturally to obtain a spherical mixture, thereby obtaining MOF glass.
[0102] (2) Preparation of gas separation membranes
[0103] The MOF glass was stirred and dispersed in DMF to obtain a MOF glass solution. After stirring and ultrasonic dispersion, the solution was allowed to stand for 5 hours for degassing to form a casting liquid. The casting liquid was evenly coated on a glass plate by a casting method to form a film. The solution was removed by solvent and dried in a vacuum oven at 80°C for 12 hours. The formed mixed film was placed in an oven for evacuation and maintained at 170°C for 24 hours for removal of solvent and reactivation to obtain a ZIF-62@ZIF-8MOF glass gas separation membrane.
[0104] Comparative Example 2
[0105] The polyimide gas separation membrane of this embodiment includes 100 wt % of a fluorine-containing polyimide matrix.
[0106] The preparation method of the polyimide gas separation membrane of this embodiment is as follows:
[0107] (1) Preparation of FPI (6FDA-FTPPA) matrix
[0108] Under nitrogen protection, FTPPA (6.0mmol, 2.4g) and m-cresol (17mL) were added to a 50mL three-necked flask. When FTPPA was completely dissolved, 6FDA (5.9mmol, 3.0g), m-cresol (17mL) and isoquinoline (6 drops) were added to the three-necked flask, stirred and heated to 60℃ for full dissolution, then heated to 80℃ for 3h, 120℃ for 4h, 180℃ for 3h, and finally 190℃ for 15h. After the reaction was completed, it was cooled to room temperature, and the viscous product solution was poured into 500mL methanol for drawing precipitation. After washing and filtering, it was placed in an oven to dry to obtain fibrous polyimide. The polyimide was then redissolved in DMF, purified by secondary precipitation, and dried to obtain the FPI (6FDA-FTPPA) substrate.
[0109] (2) Preparation of gas separation membranes
[0110] The FPI matrix prepared in step (1) was added to DMF, stirred and dissolved to obtain an FPI solution, and allowed to stand for 5 hours to degas to form a casting liquid. The casting liquid was evenly coated on a glass plate by a casting method to form a film, and the film was removed by solvent and dried in a vacuum oven at 80°C for 12 hours. The formed mixed film was placed in an oven for evacuation and maintained at 170°C for 24 hours to remove the solvent and reactivate to obtain a 6FDA-DAR gas separation membrane.
[0111] The performance tests of the polyimide mixed matrix membranes prepared in Examples 1-7 and the gas separation membranes prepared in Comparative Examples 1-2 were performed as follows:
[0112] The polyimide mixed matrix membranes prepared in Examples 1-7 and the gas separation membranes prepared in Comparative Examples 1-2 were respectively encapsulated in components, and their performances were tested under conditions of a pressure of 1 MPa and a room temperature. The test gases included CH4, CO2, He, and N2. The test results are shown in Table 1.
[0113]
[0114] Table 1
[0115] It can be seen from the data in Table 1 that the helium flux and selectivity of MOF glass membrane and fluorinated polyimide (FPI) used alone are poor, while the helium flux and selectivity of the mixed matrix membrane prepared by MOF glass membrane and fluorinated polyimide (FPI) are greatly improved, with the maximum helium flux reaching 351GPU, and the He / CH4, He / N2 and He / CO2 selectivities reaching 390.0, 292.5 and 234.0 respectively. Compared with Comparative Example 1, the reason for the improvement of helium flux is that the polyfluorine introduction in the fluorinated polyimide structure and the hydrogen bonding of imide make the MOF glass membrane and polyimide more fully combined. The poor effect of Comparative Example 1 is mainly due to the low porosity of the glassy MOF. Compared with Comparative Example 2, the pore size of the simple polyimide does not match the gas molecules, and the separation effect is poor. Therefore, the introduction of MOF glass membrane greatly improves the helium mass transfer resistance and improves the helium selectivity by utilizing its own pore structure characteristics. MOF glass retains a certain porosity, with an average pore size between CO2 and N2, and has the ability to adsorb a variety of gases.
[0116] Therefore, the polyimide mixed matrix membrane of the present invention can be used in the separation of helium.
[0117] The hydrophobicity of the mixed matrix membrane can be tested by a contact angle tester. The larger the contact angle, the better the hydrophobicity. The polyimide mixed matrix membranes of Examples 3-6, ordinary Kapton membranes purchased from the market, and the gas separation membrane of Comparative Example 2 were used as samples, and the hydrophobicity was tested to detect their water contact angles. The test results are shown in Table 2. In the table, (5) in MOF glass / FPI (5) represents an FPI filler content of 5wt%, (15) in MOF glass / FPI (15) represents an FPI filler content of 15wt%, (10) in MOF glass / FPI (10) represents an FPI filler content of 10wt%, and (20) in MOF glass / FPI (20) represents an FPI filler content of 20wt%.
[0118]
[0119] Table 2
[0120] The data in Table 2 show that the contact angles of the 6FDA-FTPPA matrix and the polyimide mixed matrix membranes of Examples 3-6 are 93.1°, 92.2°, 91.0°, 90.3° and 89.6°, respectively, all of which are maintained at around 90°, indicating that the polyimide mixed matrix membrane of the present invention has good hydrophobic properties.
[0121] The polyimide mixed matrix membranes of Examples 3-6 and the gas separation membrane of Comparative Example 2 were used as samples, and their thermal properties were tested by thermogravimetric method. The test results are shown in Table 3.
[0122]
[0123] Table 3
[0124] The data in Table 3 show that in a nitrogen atmosphere, the initial decomposition temperature of the MOF glass / FPI mixed matrix membrane of the present invention is about 500°C, T 10% At 506-553°C, the carbon residue rate of the MOF glass / FPI mixed matrix membrane is higher than 45%. Although the carbon residue rate of the MOF glass / FPI mixed matrix membrane decreases with the increase of the filler FPI doping amount, the decline range is limited, and the mixed matrix membrane still has excellent thermal stability.
[0125] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it should be understood by those skilled in the art that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention. The techniques, shapes, and structural parts not described in detail in the present invention are all known technologies.
Claims
1. A polyimide mixed matrix membrane, characterized in that The invention comprises 5-20 wt % of a fluorine-containing polyimide matrix and 80-95 wt % of MOF glass.
2. The polyimide mixed matrix membrane according to claim 1, characterized in that The MOF glass comprises 40-70 wt % of ZIF-62 and 30-60 wt % of ZIF-8.
3. A method for preparing a polyimide mixed matrix membrane, characterized in that: The steps include: In an argon atmosphere, ZIF-62 and ZIF-8 were mixed and pressed using a mold, then heated to 440-450°C for 6-12 minutes and cooled naturally to obtain a spherical mixture MOF glass. Under nitrogen protection, diamine monomer, m-cresol and 4,4'-(hexafluoroisopropylene) diphthalic anhydride are mixed, isoquinoline is added dropwise, the temperature is raised to 80-180°C for reaction for 9-10 hours, and then the temperature is 190-200°C for reaction for 12-15 hours. After the reaction is completed, the temperature is cooled to 55-60°C, the obtained reaction solution is poured into methanol for drawing precipitation, washed and filtered, and then dried to obtain the FPI matrix; According to 5-25wt% of fluorinated polyimide matrix and 80-95wt% of MOF glass, the FPI matrix is added to DMF, stirred and dissolved to obtain an FPI solution, the MOF glass is stirred and dispersed in DMF to obtain a MOF glass solution, the MOF glass solution is added to the FPI solution under stirring, stirred and ultrasonically dispersed, and then allowed to stand for degassing, coated on a smooth glass plate and cast into a film, dried, demolded, and activated to obtain a MOF glass / FPI mixed matrix membrane.
4. The method for preparing a polyimide mixed matrix membrane according to claim 3, characterized in that: In the MOF glass, the mass fraction of ZIF-62 is 40-70wt%, and the mass fraction of ZIF-8 is 30-60wt%.
5. The method for preparing a polyimide mixed matrix membrane according to claim 3, characterized in that: The preparation method of the ZIF-62 is as follows: Zn(NO3)2·6H2O and imidazole were added to N,N-dimethylformamide and stirred respectively, and then the two solutions were mixed and stirred, and then benzimidazole was added and stirred, and the obtained mixed solution was heated to 130-140°C for reaction for 48-50h, cooled to room temperature, vacuum filtered, and the precipitate was washed with N,N-dimethylformamide and dichloromethane, and then dried at 150-155°C to obtain ZIF-62; The molar ratio of Zn(NO3)2·6H2O to imidazole is (0.070-0.080):(1.60-1.80), and the molar ratio of Zn(NO3)2·6H2O to benzimidazole is 1:
1.
6. The method for preparing a polyimide mixed matrix membrane according to claim 3, characterized in that: The preparation method of the ZIF-8 is as follows: ZnCl2 and 2-methylimidazole were added to methanol respectively and stirred, and then the two solutions were mixed and stirred, and allowed to stand at room temperature for 4 to 5 hours, centrifuged and filtered, and the precipitate was washed with methanol, and then dried in a vacuum oven at 110 to 120°C for 12 to 15 hours to obtain ZIF-8.
7. The method for preparing a polyimide mixed matrix membrane according to claim 3, characterized in that: The molar ratio of the diamine monomer to 4,4'-(hexafluoroisopropylene) diphthalic anhydride is 1:
1.
8. The method for preparing a polyimide mixed matrix membrane according to claim 7, characterized in that: The diamine monomer is one of 4-(3-fluoro-4-trifluoromethylphenyl)-2,6-bis-(4-aminophenyl)-pyridine, 4,4'-((perfluoropropane-2,2-diyl)bis(4,1-phenylsulfonyl))diphenylamine, 4,4'-diaminodiphenyl ether, and 4,6-diaminoresorcinol hydrochloride.
9. The method for preparing a polyimide mixed matrix membrane according to claim 3, characterized in that: The activation condition is to maintain the temperature at 160-180° C. in a vacuum environment for 24-36 hours.
10. Use of the polyimide mixed matrix membrane according to claim 1 or 2 or the polyimide mixed matrix membrane prepared by the preparation method according to any one of claims 3 to 9 in helium separation.
Citation Information
Cited By
Composite MOF (Metal Organic Framework) membrane for gas separation and preparation method of composite MOF membrane
CN119345918A
A composite MOF membrane for gas separation and preparation method thereof
CN119345918B
MOF glass film and preparation method and application thereof
CN120305850A