Concurrent MOF (Metal Organic Framework) membrane material high-throughput production equipment and production method
Through the high-throughput production equipment of concurrent MOF film materials, the high-throughput preparation and thickness control of MOF films are achieved through electrostatic generators and atomization spraying technology, and the scale and multiple batches of MOF film materials in the existing technology are solved. The production problem has improved the performance and application potential of membrane materials.
Patent Information
- Application Number
- CN202410855322.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-08
AI Technical Summary
The existing MOF film material preparation technology is difficult to achieve large-area and high-throughput concurrent preparation, which limits its scale and multi-batch production in industrial applications. The existing methods usually can only prepare a single type of MOF film, which cannot be met. High throughput requirements for multiple types of MOF membranes.
A high-throughput production equipment for concurrent MOF membrane materials is designed, including electrostatic generators, liquid storage units, liquid mixing units, film growth chambers and atomization spraying units. Through precision control of the mixing and atomization spraying of metal and ligand solutions and displacement control, realize efficient, uniform deposition and continuous growth of MOF films, and can prepare MOF films with controllable thickness.
It realizes high-throughput preparation of MOF films, is simple to operate, is suitable for large-scale industrial production, and controls the crystal plane growth orientation through an alternating electric field, improving the performance of the film material.
Smart Images

Figure CN118904123A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of MOF membrane material preparation, and in particular to a concurrent MOF membrane material high-throughput production device and a production method. Background Art
[0002] Compared with traditional separation technologies such as distillation and extraction, membrane separation technology has the advantages of low energy consumption, high efficiency, and environmental protection. The preparation of high-performance separation membranes is an important issue in realizing the membrane separation process. Especially in the field of gas separation, MOF membrane materials have attracted widespread attention due to their outstanding structural characteristics and gas separation properties. MOF is a porous material constructed by metal clusters as secondary structural units and organic ligands connected by chemical bonds. It has the characteristics of adjustable pore size, high pore volume, large specific surface area, and easy functional group modification. This structural feature enables it to produce different host-guest interactions or screening effects for different gas molecules to achieve the purpose of economical and energy-saving separation of gases.
[0003] However, the current design and preparation of MOF membrane materials face great challenges. The reason is that the existing MOF membrane preparation process is mainly prepared through microwave-assisted synthesis, seed secondary growth, reverse diffusion, chemical vapor deposition and electrochemical methods. However, for these methods, the size and scale of the prepared membrane are limited by the size of the synthesis equipment container. Usually, only a few square centimeters of MOF membrane can be prepared, and the area of the membrane cannot be expanded, which limits its industrial application.
[0004] For the classic hydrothermal or solvent thermal synthesis process, the reaction time is long, the reaction temperature is high, and only a single preparation can be made. The preparation cost is high, and it is difficult to expand this preparation process to a larger size and space, which has become the main obstacle to the commercial application of MOF membrane materials. Therefore, it is urgent to develop a new method for easily scalable preparation of MOF membranes to achieve multi-batch high-throughput concurrent preparation of MOF membrane materials. In addition, the liquid phase epitaxial growth method, that is, the surface of the porous substrate is alternately exposed to the MOF precursor solution, and the excess / unreacted precursor is rinsed in the middle to remove the excess / unreacted precursor. The method of forming the MOF membrane by layer-by-layer (LBL) is applied to the spraying preparation of large-area MOF membranes, but this method is suitable for MOF materials that can be synthesized under mild conditions, and it is almost not feasible for MOF materials with harsh reaction conditions. In addition, this method can only complete the large-area preparation of a single MOF membrane material, and cannot meet the requirements of high-throughput parallel preparation of multiple batches of MOF membrane materials. Another method of preparing MOF membrane materials by spraying is to deposit MOF crystals on a hot substrate by electrostatic spraying and achieve MOF intergrowth through thermal action. However, this method generally produces more grain boundary defects and requires a larger spray liquid concentration and more spraying times to compensate for the grain boundary defects. However, a thicker MOF membrane structure is often obtained, which increases the mass transfer resistance of the gas separation process, is not conducive to the improvement of gas flux, and can only be used for the preparation of a single type or a single batch of MOF membrane materials. Summary of the invention
[0005] In view of the problems existing in the above-mentioned prior art, the present invention provides a concurrent MOF membrane material high-throughput production equipment. The design of this concurrent MOF (metal organic framework material) membrane material high-throughput production equipment is intended to efficiently and accurately manufacture MOF membranes with high-throughput characteristics. These membranes are widely used in gas separation, water purification, catalyst carriers and other fields.
[0006] The concurrent MOF membrane material high-throughput production equipment comprises: an electrostatic generator, a liquid storage unit, a liquid mixing unit, a thin film growth chamber, and an atomizing spray unit and a stage located in the thin film growth chamber; the atomizing spray unit is controlled to move by a displacement control unit;
[0007] The liquid storage unit is divided into two independent parts: the metal solution tank and the ligand solution tank. The two tanks are designed with strict sealing and temperature control mechanisms to ensure that the solutions are stable and not prone to chemical changes. The metal solution usually contains metal ions such as copper, zinc, and iron, while the ligand solution contains organic molecules. Both are the basic units that make up MOF materials. Through the precision pump system, the two solutions are ensured to be supplied to the mixing unit on demand and accurately measured.
[0008] The mixing chamber integrates stirring and temperature control functions to ensure that the metal solution and ligand solution are fully mixed and maintained at a suitable reaction temperature to form a stable MOF precursor solution. The mixed solution is then transported to the atomization spray unit for film deposition.
[0009] The film growth chamber is a highly enclosed space with adjustable environmental parameters (such as temperature, humidity, and pressure) to provide ideal conditions for the growth of MOF films. Fine control of the indoor environment is crucial to obtaining high-quality MOF films.
[0010] The atomizing spray unit includes an atomizing nozzle, which is a key component for atomizing the MOF precursor solution into tiny droplets by high pressure. Combined with the effect of the electrostatic field, these droplets can be very evenly deposited on the growth substrate loaded on the stage. The displacement control unit moves the atomizing spray unit along a predetermined path to ensure uniform coverage on the entire substrate surface, and to achieve large-area, continuous film preparation. In the present invention, the mixed liquid bin implements the output of the newly configured MOF precursor solution, and the MOF precursor solution is deposited on the growth substrate. At this time, the atoms grow in an island-like mode with lower free energy. As the number of spraying increases, adjacent islands contact and combine with each other to form a thin film with a mesh structure, and finally form a continuous MOF film structure. Compared with the existing MOF film preparation method, the in-situ growth of MOF crystals on the substrate can achieve lower thickness MOF film growth, high-throughput preparation of continuous MOF membrane materials, and through the control of precursor concentration and spraying times, the film thickness can be accurately controlled, which is suitable for large-scale industrial preparation of MOF membrane materials.
[0011] The stage is used to load the growth substrate; the growth substrate carried by the stage is the physical basis for the formation of the MOF film, and its material and surface properties directly affect the formation and performance of the MOF film.
[0012] The electrostatic generator is one of the key components. It inputs alternating voltage to the atomizing spray unit to generate an electrostatic field. The role of this electrostatic field is to enhance the atomization effect of the MOF precursor solution, making the sprayed droplets smaller and more evenly distributed, thereby improving the uniformity and coverage of the film layer.
[0013] It should be pointed out that the existing technology for preparing MOF membranes can only prepare MOF membrane materials with randomly grown crystal faces. Studies have shown that oriented growth of the crystal faces of MOF membrane materials is conducive to achieving higher gas separation performance. In the present invention, the alternating voltage output by the electrostatic generator can also promote the oriented arrangement of positive and negative particles in the solution, which is conducive to forming a more regular MOF crystal structure and improving the performance of the membrane material.
[0014] Preferably, the stage is located above the atomizing spray unit, and the atomizing spray unit sprays from bottom to top, thereby enabling better thickness control.
[0015] As a common technical means in this field, the displacement control unit includes an x-axis stepper motor and a y-axis stepper motor.
[0016] Optionally, a heating plate is provided in the stage to heat the growth substrate.
[0017] Optionally, the metal solution tank, the ligand solution tank and the mixed liquid tank are connected by a pipeline, and a flow controller is provided on the pipeline; the mixed liquid tank and the atomizing nozzle are connected by a pipeline, and a peristaltic pump is provided on the pipeline.
[0018] Based on the above production equipment, the present invention provides a concurrent high-throughput production method of MOF membrane materials, comprising the following steps:
[0019] S1: placing the growth substrate on a stage; injecting the metal solution and the ligand solution into the metal solution tank and the ligand solution tank; controlling the speed of injecting the metal solution and the ligand solution into the mixed solution tank, and mixing the metal solution and the ligand solution to form a MOF precursor solution;
[0020] S2: Start the atomizing spray unit, the atomizing nozzle starts to spray the MOF precursor solution onto the growth substrate, and at the same time, the electrostatic generator inputs an alternating voltage to the atomizing nozzle. After at least 2 alternating cycles, one spraying is completed, and the MOF precursor solution is deposited on the growth substrate. At this time, the atoms grow in an island pattern with lower free energy; then the position of the atomizing nozzle is moved to spray the next position; among them, under positive voltage, it is more conducive to the deposition of negatively charged organic ligands on the substrate; under negative voltage, it is more conducive to the deposition of positively charged metal ions on the substrate.
[0021] S3: Perform overall spraying multiple times according to step S2 to obtain continuous MOF membrane material, until the spraying of the entire growth surface is completed, adjacent islands contact and combine with each other to form a thin film with a network structure, and finally form a continuous MOF membrane structure.
[0022] Optionally, the metal solution is Zn 2+ , Cu 2+ 、Co 2+ 、Ni 2+ 、Ti 4+ or Zr 4+ The solvent is one or more of water, DMF, methanol, ethanol, and DMA;
[0023] Optionally, the ligand solution is a solution of terephthalic acid, dimethylimidazole, tris-benzoic acid, dimethylbenzimidazole or benzimidazole; and the solvent is one or more of water, DMF, methanol, ethanol and DMA.
[0024] Optionally, the spray flow rate of the atomizing nozzle is 1 ml / s to 2 ml / s; the positive voltage is 15 V, the duration is 0.5 s; the negative voltage is 15 V, the duration is 0.5 s;
[0025] Optionally, the liquid discharge rate of the mixing chamber is 1ml / min-9ml / min.
[0026] Optionally, the growth substrate adopts a porous substrate, including but not limited to: porous AAO, porous α-Al2O3 ceramic sheet, porous ZrO2 ceramic sheet, etc.
[0027] The beneficial effects of the present invention are:
[0028] (1) The present invention can prepare MOF membranes with controllable thickness at high throughput, is simple to operate, easy to prepare, and suitable for large-scale industrial production;
[0029] (2) By controlling the alternating directional deposition of metal / ligands through an alternating electric field, the crystal growth orientation of the MOF film can be controlled. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings in the specification are an integral part of the present invention and are intended to further illustrate the present invention. The exemplary embodiments and corresponding descriptions therein are intended to assist understanding rather than to unduly limit the scope of the present invention.
[0031] Figure 1 A schematic diagram of a concurrent high-throughput production device for MOF membrane materials of the present invention; wherein, a metal solution tank 1, a ligand solution tank 2, a mixed solution tank 3, a thin film growth chamber 4, a stage 5, an atomizing nozzle 6, an electrostatic generator 7, a displacement control unit 8, a collecting valve 9, and a peristaltic pump 10.
[0032] Figure 2 Example 1 Concurrent MOF membrane material high-throughput equipment preparation NH2-MIL-125 membrane XRD pattern;
[0033] Figure 3 Example 1 Concurrent MOF membrane material high-throughput equipment preparation NH2-MIL-125-1 membrane SEM image;
[0034] Figure 4 Example 1 Concurrent MOF membrane material high-throughput equipment preparation of NH2-MIL-125-1 membrane and NH2-MIL-125-1 membrane gas separation performance diagram;
[0035] Figure 5Comparative Example 1: XRD pattern of NH2-MIL-125 membrane prepared by concurrent MOF membrane material high-throughput equipment;
[0036] Figure 6 Comparative Example 1: SEM image of NH2-MIL-125-1 membrane prepared by concurrent MOF membrane material high-throughput equipment;
[0037] Figure 7 Comparative Example 1: Preparation of NH2-MIL-125-1 membrane by concurrent MOF membrane material high-throughput equipment and gas separation performance diagram of NH2-MIL-125-1 membrane;
[0038] Figure 8 XRD pattern of Zn / Co-ZIF film material of Example 2;
[0039] Fig. 9 SEM image of Zn / Co-ZIF membrane material in Example 2.
[0040] Fig.10 Schematic diagram of another concurrent MOF membrane material high-throughput production equipment of the present invention;
[0041] Fig.11 Example 3 SEM image of NH2-MIL-125 membrane material DETAILED DESCRIPTION
[0042] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In order to make the purpose, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only intended to explain the present application, rather than to limit the present application. For those skilled in the art, the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating the examples of the present application.
[0043] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0044] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0045] It is obvious to those skilled in the art that various modifications and changes can be made in the present application without departing from the spirit or scope of the present application. Therefore, the present application is intended to cover modifications and changes of the present application that fall within the scope of the corresponding claims (technical solutions for protection) and their equivalents. It should be noted that the implementation methods provided in the embodiments of the present application can be combined with each other without contradiction.
[0046] Before describing the technical solutions provided by the embodiments of the present application, in order to facilitate the understanding of the embodiments of the present application, the present application first specifically describes the problems existing in the related art:
[0047] The electrostatic generator described in the present invention is a device specially designed to generate static electricity, which has a wide range of applications in multiple industrial and scientific research fields. As is common knowledge in the field, its basic working principle involves converting the energy provided by a high-voltage power supply into electrostatic energy, thereby causing the target object to be electrostatically charged. In atomized spraying applications, the electrostatic generator can cause the sprayed liquid particles to be electrostatically charged by inputting a voltage to the nozzle. This process regulates the interaction between the substrate and the particles to achieve controllable spraying.
[0048] The film growth chamber of the present invention refers to a chamber constructed in any form, the interior of which generally maintains a very high cleanliness level to prevent dust and other pollutants from affecting the quality of the film. In addition, a vacuum system can be built according to actual needs.
[0049] The displacement control unit of the present invention is an automated control device that is responsible for accurately controlling the position and / or movement distance of the nozzle. As is common knowledge in the art, the displacement control unit generally includes: a sensor, a driver (such as a stepper motor driver, a servo driver), a controller (such as a PLC, a motion controller or an embedded system), etc.
[0050] Figure 1 The concurrent MOF membrane material high-throughput production equipment of the present invention comprises: an electrostatic generator 7, a liquid storage unit, a liquid mixing unit, a thin film growth chamber 4, and an atomizing spray unit and a stage 5 located in the thin film growth chamber 4; the atomizing spray unit is controlled to move by a displacement control unit 8, and the electrostatic generator 7 inputs an alternating voltage to the atomizing spray unit;
[0051] The liquid storage unit includes a metal solution tank 1 and a ligand solution tank 2, which are respectively used to store the metal solution and the ligand solution used for the synthesis of the MOF membrane material;
[0052] The liquid mixing unit includes a liquid mixing chamber 3, which is used to mix the metal solution and the ligand solution to form a MOF precursor solution;
[0053] The loading platform 5 is used to load the growth substrate;
[0054] The atomizing spray unit comprises an atomizing nozzle 6 for spraying the MOF precursor solution onto the growth substrate.
[0055] S1: When in use, the growth substrate is placed on a stage; a metal solution and a ligand solution are injected into the metal solution tank and the ligand solution tank; the speed at which the metal solution and the ligand solution are injected into the mixed solution tank is controlled to mix the metal solution and the ligand solution to form a MOF precursor solution;
[0056] S2: Start the atomizing spray unit, the atomizing nozzle starts to spray the MOF precursor solution onto the growth substrate, and the electrostatic generator inputs an alternating voltage to the atomizing nozzle at the same time, and completes one spraying after at least 2 alternating cycles; then move to the position of the atomizing nozzle, spray again, until the batch growth substrate high-throughput spraying is completed, and the MOF film material is formed on the growth substrate; wherein, under a positive voltage, it is conducive to the deposition of positively and negatively charged organic ligands on the substrate; under a negative voltage, it is conducive to the deposition of positively charged metal ions on the substrate. Those skilled in the art should know that the growth substrate is generally grounded, and the electrostatic generator inputs an alternating voltage to the atomizing nozzle, so that a potential difference is formed between the atomizing nozzle and the growth substrate. The positive voltage described in the present invention refers to the potential difference between the nozzle and the growth substrate being positive, and the negative voltage refers to the potential difference between the nozzle and the growth substrate being negative.
[0057] S3: Repeat the above operation and complete one growth preparation after at least 50 cycles of spraying.
[0058] Optionally, the metal solution is Zn 2+ , Cu 2+ 、Co 2+ 、Ni 2+ 、Ti 4+ or Zr 4+ The solvent is one or more of water, DMF, methanol, ethanol, and DMA;
[0059] Optionally, the ligand solution is a solution of terephthalic acid, dimethylimidazole, tris-benzoic acid, dimethylbenzimidazole or benzimidazole; and the solvent is one or more of water, DMF, methanol, ethanol and DMA.
[0060] Optionally, the spray flow rate of the atomizing nozzle is 1 ml / s to 2 ml / s; the positive voltage is 15 V, the duration is 0.5 s; the negative voltage is 15 V, the duration is 0.5 s;
[0061] Optionally, the liquid discharge rate of the mixing chamber is 1ml / min-9ml / min.
[0062] Optionally, the growth substrate adopts a porous substrate, including but not limited to: porous AAO, porous α-Al2O3 ceramic sheet, porous ZrO2 ceramic sheet, etc.
[0063] Example 1
[0064] The purpose of this embodiment is to quickly and efficiently obtain 64 batches of NH2-MIL-125 membrane materials with a diameter of 18 nm.
[0065] (1) Raw material preparation:
[0066] Dissolve 168 g of 2-aminoterephthalic acid in 6 L of N,N-dimethylformamide to obtain a ligand solution;
[0067] 78 ml of tetrabutyl titanate was fully dissolved in 6 L of methanol / DMF mixed solution (volume ratio was 2:8) to obtain a metal solution;
[0068] The above ligand solution and metal solution are injected into the corresponding ligand solution tank 2 and metal solution tank 1 respectively.
[0069] The growth substrate is a circular porous α-Al2O3 ceramic sheet with a diameter of 18 nm, a thickness of 1 mm, and a pore size of 0.22 μ; 64 growth substrates are arranged in an 8 by 8 array.
[0070] (2) Flow control:
[0071] The flow rate of ligand solution tank 2-mixing liquid tank 3 is 5ml / min;
[0072] The flow rate of metal solution tank 1-mixing liquid tank 3 is 5ml / min;
[0073] The flow rate of the mixing chamber 3-atomizing nozzle 6 is 1 ml / s;
[0074] (3) Film making process
[0075] ① The positive voltage is 15V, the duration is 0.5s; the negative voltage is -15V, the duration is 0.5s; one spraying process goes through 2 cycles;
[0076] ② The spray pressure of the atomizing nozzle 6 is 0.2 MPa, and the distance from the growth substrate is 5 cm.
[0077] ③ The running time of each step of the displacement control unit is 1s, the running interval is 1s, and the running step length is 2.5cm;
[0078] ④The total number of spraying times is 50 times;
[0079] ⑤ The stage 5 has a built-in heating plate with a temperature of 160°C.
[0080] Figure 2 The XRD diagram of the NH2-MIL-125 membrane material prepared by the high-throughput device of the present invention (four samples are selected from 64 samples) shows that it exhibits strong diffraction peaks of the (002) and (004) crystal planes, indicating that it maintains a good c-axis orientation arrangement;
[0081] Figure 3 This is an SEM image of the NH2-MIL-125 membrane material prepared with high throughput using the equipment of the present invention. The left image shows the surface morphology of the NH2-MIL-125 membrane material, indicating that the surface growth of the MOF membrane material is uniform and dense. The right image shows the cross-sectional morphology of the NH2-MIL-125 membrane material, indicating that after 50 cycles, its thickness is 600-800nm, showing a good thickness control effect.
[0082] Figure 4 The gas separation performance of some NH2-MIL-125 membrane materials was studied, and it was found that it exhibited higher gas flux and good separation selectivity.
[0083] Comparative Example 1
[0084] This comparative example is the same as Example 1, except that a DC voltage of 15V is applied.
[0085] (1) Raw material preparation:
[0086] Dissolve 168 g of 2-aminoterephthalic acid in 6 L of N,N-dimethylformamide to obtain a ligand solution;
[0087] 78 ml of tetrabutyl titanate was fully dissolved in 6 L of methanol / DMF mixed solution (volume ratio was 2:8) to obtain a metal solution;
[0088] The above ligand solution and metal solution are injected into the corresponding ligand solution tank 2 and metal solution tank 1 respectively.
[0089] The growth substrate is a circular porous α-Al2O3 ceramic sheet with a diameter of 18 nm, a thickness of 1 mm, and a pore size of 0.22 μm; 64 growth substrates are arranged in an 8 by 8 array.
[0090] (2) Flow control:
[0091] The flow rate of ligand solution tank 2-mixing liquid tank 3 is 5ml / min;
[0092] The flow rate of metal solution tank 1-mixing liquid tank 3 is 5ml / min;
[0093] The flow rate of the mixing chamber 3-atomizing nozzle 6 is 1 ml / s;
[0094] (3) Film making process
[0095] ① The DC voltage is 15V, the duration is 0.5s; the negative voltage is -15V, the duration is 0.5s; one spraying goes through 2 cycles;
[0096] ② The spray pressure of the atomizing nozzle 6 is 0.2 MPa, and the distance from the growth substrate is 5 cm.
[0097] ③ The running time of each step of the displacement control unit is 1s, the running interval is 1s, and the running step length is 2.5cm;
[0098] ④The total number of spraying times is 50 times;
[0099] ⑤ The stage 5 has a built-in heating plate with a temperature of 160°C.
[0100] Figure 5 The XRD diagram of the randomly oriented NH2-MIL-125 film material prepared by the high-throughput device of the present invention (three samples are randomly selected from 64 samples) shows that it exhibits diffraction peaks of all crystal planes of the NH2-MIL-125 material, indicating that its crystal grows in a random orientation and cannot maintain a good c-axis orientation arrangement;
[0101] Figure 6 This is an SEM image of a randomly oriented NH2-MIL-125 membrane material prepared with high throughput using the equipment of the present invention. The left image is the surface morphology of the NH2-MIL-125 membrane material. The surface growth of the MOF membrane material shows a randomly oriented growth arrangement.
[0102] Figure 7 The gas separation performance of the NH2-MIL-125 membrane material was investigated. It was found that it exhibited lower gas flux and separation selectivity compared with the membrane material prepared by applying an alternating electric field.
[0103] Example 2
[0104] This embodiment aims to quickly and efficiently obtain 64 batches of Zn / Co-ZIF membrane materials with a diameter of 18 nm.
[0105] (1) Raw material preparation:
[0106] Dissolve 120 g of benzimidazole in 6 L of ethanol to obtain a ligand solution;
[0107] 125 g of Co(Ac)2·4H2O and 110 g of Zn(Ac)2·2H2O were fully dissolved in 6 L of ethanol to obtain metal solutions;
[0108] The above ligand solution and metal solution are injected into the corresponding ligand solution tank 2 and metal solution tank 1 respectively.
[0109] The growth substrate is a circular porous α-Al2O3 ceramic sheet with a diameter of 18 nm, a thickness of 1 mm, and a pore size of 0.22 μm; 64 growth substrates are arranged in an 8 by 8 array.
[0110] (2) Flow control:
[0111] The flow rate of ligand solution tank 2-mixing liquid tank 3 is 5ml / min;
[0112] The flow rate of metal solution tank 1-mixing liquid tank 3 is 5ml / min;
[0113] The flow rate of the mixing chamber 3-atomizing nozzle 6 is 1 ml / s;
[0114] (3) Film making process
[0115] ① The positive voltage is 15V, the duration is 0.5s; the negative voltage is -15V, the duration is 0.5s; one spraying process goes through 2 cycles;
[0116] ② The spray pressure of the atomizing nozzle 6 is 0.2 MPa, and the distance from the growth substrate is 5 cm.
[0117] ③ The running time of each step of the displacement control unit is 1s, the running interval is 1s, and the running step length is 2.5cm;
[0118] ④The overall spraying times is 20 times;
[0119] ⑤ The stage 5 has a built-in heating plate with a temperature of 100°C.
[0120] Figure 8 The XRD diagram of the Zn / Co-ZIF membrane material prepared by the high-throughput device of the present invention (4 samples are randomly selected from 64 samples), which shows that it exhibits a strong crystal plane directional growth orientation arrangement;
[0121] Fig. 9 This is a SEM image of a Zn / Co-ZIF membrane material prepared by high throughput using the device of the present invention, indicating that the surface growth of the MOF membrane material is uniform and dense.
[0122] Example 3
[0123] The purpose of this embodiment is to change the atomization spraying direction from downward spraying to upward spraying, so as to quickly and high-throughput obtain 64 batches of NH2-MIL-125 membrane materials with a diameter of 18 nm and a lower thickness. Fig.10 This is a schematic diagram of the concurrent MOF membrane material high-throughput production equipment of this embodiment.
[0124] (1) Raw material preparation:
[0125] Dissolve 168 g of 2-aminoterephthalic acid in 6 L of N,N-dimethylformamide to obtain a ligand solution;
[0126] 78 ml of tetrabutyl titanate was fully dissolved in 6 L of methanol / DMF mixed solution (volume ratio was 2:8) to obtain a metal solution;
[0127] The above ligand solution and metal solution are injected into the corresponding ligand solution tank 2 and metal solution tank 1 respectively.
[0128] The growth substrate is a circular porous α-Al2O3 ceramic sheet with a diameter of 18 nm, a thickness of 1 mm, and a pore size of 0.22 μm; 64 growth substrates are arranged in an 8 by 8 array.
[0129] (2) Flow control:
[0130] The flow rate of ligand solution tank 2-mixing liquid tank 3 is 5ml / min;
[0131] The flow rate of metal solution tank 1-mixing liquid tank 3 is 5ml / min;
[0132] The flow rate of the mixing chamber 3-atomizing nozzle 6 is 1 ml / s;
[0133] (3) Film making process
[0134] ① The positive voltage is 15V, the duration is 0.5s; the negative voltage is -15V, the duration is 0.5s; one spraying process goes through 2 cycles;
[0135] ② The spray pressure of the atomizing nozzle 6 is 0.2 MPa, and the distance from the growth substrate is 5 cm.
[0136] ③ The running time of each step of the displacement control unit is 1s, the running interval is 1s, and the running step length is 2.5cm;
[0137] ④The total number of spraying times is 50 times;
[0138] ⑤ The stage 5 has a built-in heating plate with a temperature of 160°C.
[0139] Fig.11This is an SEM image of the NH2-MIL-125 membrane material prepared by high throughput using the equipment of the present invention. The left image shows the surface morphology of the NH2-MIL-125 membrane material, indicating that the surface growth of the MOF membrane material is uniform and dense. The right image shows the cross-sectional morphology of the NH2-MIL-125 membrane material, indicating that after 50 cycles, its thickness is 500-600nm, showing a better thickness control effect compared with downward spraying.
Claims
1. A concurrent MOF membrane material high-throughput production device, characterized in that: At least: An electrostatic generator, a liquid storage unit, a liquid mixing unit, a thin film growth chamber, and an atomizing spray unit and a stage located in the thin film growth chamber; the atomizing spray unit is controlled to move by a displacement control unit, and the electrostatic generator inputs an alternating voltage to the atomizing spray unit; The liquid storage unit includes a metal solution tank and a ligand solution tank, which are used to store the metal solution and ligand solution used for synthesizing the MOF membrane material; The liquid mixing unit includes a liquid mixing chamber for mixing the metal solution and the ligand solution to form a MOF precursor solution; The stage is used to load the growth substrate; The atomizing spray unit comprises an atomizing nozzle for spraying the MOF precursor solution onto the growth substrate.
2. The production equipment according to claim 1, characterized in that: The loading platform is located above the atomizing spraying unit, and the atomizing spraying unit sprays from bottom to top.
3. The production equipment according to claim 1, characterized in that: A heating plate is arranged inside the stage to heat the growth substrate.
4. The production equipment according to claim 1, characterized in that: The metal solution tank, the ligand solution tank and the mixed liquid tank are connected through pipelines, and a flow controller is arranged on the pipelines; the mixed liquid tank and the atomizing nozzle are connected through pipelines, and a peristaltic pump is arranged on the pipelines.
5. A concurrent high-throughput production method for MOF membrane materials, characterized in that: The production is carried out using the equipment described in claim 1.
6. The production method according to claim 5, characterized in that: The steps include: S1: placing the growth substrate on a stage; injecting the metal solution and the ligand solution into the metal solution tank and the ligand solution tank; controlling the speed of injecting the metal solution and the ligand solution into the mixed solution tank, and mixing the metal solution and the ligand solution to form a MOF precursor solution; S2: Start the atomizing spray unit, the atomizing nozzle starts to spray the MOF precursor solution onto the growth substrate, and at the same time, the electrostatic generator inputs an alternating voltage to the atomizing nozzle, and at least two alternating cycles are passed to complete one spraying; then the position of the atomizing nozzle is moved to spray the next position until the entire growth substrate is sprayed; S3: Perform overall spraying multiple times according to step S2 to obtain a continuous MOF membrane material.
7. The production method according to claim 6, characterized in that: The metal solution is Zn 2+ , Cu 2+ 、Co 2+ 、Ni 2+ 、Ti 4+ or Zr 4+ The solvent is one or more of water, DMF, methanol, ethanol, and DMA; The ligand solution is a solution of terephthalic acid, dimethylimidazole, tris-benzoic acid, dimethylbenzimidazole or benzimidazole; the solvent is one or more of water, DMF, methanol, ethanol and DMA.
8. The production method according to claim 6, characterized in that: The spray flow rate of the atomizing nozzle is 1 ml / s to 2 ml / s; the positive voltage is 15V, and the duration is 0.5s; the negative voltage is -15V, and the duration is 0.5s.
9. The production method according to claim 6, characterized in that: The liquid discharge rate of the mixing chamber is 1ml / min-9ml / min.
10. The production method according to claim 6, characterized in that: The growth substrate is a porous substrate.