Preparation method and application of ferric sodium phosphate pyrophosphate composite material
Through spray drying and ultrasonic dispersion technology, calcining titanium compound coated with sodium ferro pyrophosphate composite material in Ar-H2 mixed atmosphere, the problem of unstable electrochemical performance of titanium doped materials is solved, and conductivity and cyclic stability are achieved The improvement is suitable for sodium ion battery positive electrode material.
Patent Information
- Application Number
- CN202411411591.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing preparation method of titanium-doped carbon-coated sodium ferric pyrophosphate material cannot effectively control the proportion of titanium in the body phase and the surface layer, resulting in unstable electrochemical performance of the material and poor uniformity of the titanium dioxide layer coating, affecting product performance.
The Na4Fe3(PO4)2P2O7 precursor was prepared by spray drying, and the solution was added dropwise by ultrasonic dispersion and liquid titanium source, and then calcined in an Ar-H2 mixed atmosphere to form a sodium ferric pyrophosphate composite material to ensure the titanium compound Coat evenly and control the thickness of the cladding to avoid material agglomeration and sintering.
It improves the conductivity and cyclic stability of the material, ensures the consistency of the product and the stability of electrochemical properties, reduces the loss of active transition metals and the side reaction of electrolyte decomposition, and improves the application performance of the material.
Smart Images

Figure CN118929616A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion battery electrode material preparation, and in particular to a preparation method and application of a sodium iron phosphate pyrophosphate composite material. Background Art
[0002] Fossil fuels are non-renewable resources, and their reserves are decreasing. During the combustion of fossil fuels, a large amount of CO2 is produced, which exacerbates the global greenhouse effect and is not conducive to ecological balance. With the development of human civilization, people's demand for energy is increasing, so the effective use of clean energy is very urgent. Wind energy, solar energy, etc. are renewable resources, but they are intermittent and require supporting energy storage equipment to store them, so as to ensure a stable supply of energy. At present, energy storage technologies are emerging in an endless stream, such as compressed air energy storage, flywheel energy storage, pumped water energy storage and electrochemical energy storage.
[0003] Electrochemical energy storage is widely used in energy storage devices due to its flexible power and capacity configuration and high conversion efficiency. Sodium-ion batteries have developed rapidly in recent years due to their abundant resources, stable high and low temperature performance, and low cost. Currently, the positive electrode materials of sodium-ion batteries are layered oxides, Prussian blue, and polyanions. Polyanions are widely used in research due to their open framework structure, thermal stability, and cycle stability.
[0004] Among polyanionic materials, the Fe-based material Na4Fe3(PO4)2P2O7 has attracted much attention due to its advantages such as environmental friendliness, low cost, and high theoretical specific capacity. However, the larger PO4 and P2O7 groups are not conducive to the transmission of electrons and ions, resulting in low conductivity and poor rate performance of Na4Fe3(PO4)2P2O7. Researchers have modified it in various ways to improve its electrochemical performance.
[0005] The Chinese patent document with publication number CN116750741A discloses a preparation method and application of a titanium-doped carbon-coated sodium iron phosphate pyrophosphate material. The slurry formed by mixing a sodium source, a phosphorus source, a carbon source, an iron source and a titanium source is first ground with a sand mill, then spray-dried, and finally calcined to obtain a titanium-doped carbon-coated sodium iron phosphate pyrophosphate material. In this patent, the conductivity of the material is modified by introducing titanium doping and partial titanium dioxide coating. Titanium doping and titanium dioxide coating are introduced by forming a mixed slurry by ball milling. First, the ratio of the amount of titanium in the bulk phase and the surface layer of the material cannot be controlled, and the thickness of the titanium dioxide layer protecting the surface of the material cannot be controlled. The product quality of different batches of materials is unstable and the consistency is poor, resulting in unstable electrochemical performance of the material. Second, the uniformity of the titanium dioxide layer coating is poor. In the subsequent calcination process, material sintering is likely to occur, affecting product performance. Summary of the invention
[0006] The invention aims to provide a preparation method and application of a sodium iron phosphate pyrophosphate composite material. The prepared sodium iron phosphate pyrophosphate composite material has good electrical conductivity and cycle stability and is suitable for a positive electrode material of a sodium ion battery.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a method for preparing a sodium iron phosphate pyrophosphate composite material, comprising the following steps: (1) dissolving an inorganic salt containing sodium and phosphorus, an inorganic strong acid iron salt, and an organic acid carbon source in deionized water, spray drying the reaction solution to obtain a Na4Fe3(PO4)2P2O7 precursor; adding the Na4Fe3(PO4)2P2O7 precursor and ammonia water into ethanol for ultrasonic dispersion, and then adding a liquid titanium source dropwise under stirring to form a solution A; (2) placing solution A in a water bath or an oil bath and heating and stirring to form a suspension B; filtering solution B, washing the solid with ethanol, and drying the solid to obtain a Na4Fe3(PO4)2P2O7 precursor coated with a titanium compound; (3) The titanium compound is coated on the Na4Fe3(PO4)2P2O7 precursor and calcined in an Ar-H2 mixed atmosphere to obtain a sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7@H-TiO2).
[0008] Furthermore, in the step (1), the inorganic salt containing sodium and phosphorus is sodium dihydrogen phosphate or sodium hypophosphite; the inorganic strong acid iron salt is ferric nitrate or ferric chloride; the organic acid carbon source is citric acid or ascorbic acid; the molar ratio of the inorganic salt containing sodium and phosphorus, the inorganic strong acid iron salt, and the organic acid carbon source sodium is 0.4-0.45 mol: 0.3 mol: 0.05-0.1 mol; the spray drying temperature is 110-150°C; and the flow rate is 200-300 mL / h -1 ; The liquid titanium source is one of tetrabutyl titanate, titanium tetraisopropoxide or titanium tetrachloride; the mass volume ratio of Na4Fe3(PO4)2P2O7 precursor and liquid titanium source is 0.2g:0.2mL~0.4mL; the concentration of ammonia water is 25~28wt%; the volume ratio of ammonia water and ethanol is 0.1mL~0.2mL:50mL.
[0009] Furthermore, in the step (2), the heating temperature is 45°C to 60°C; and the stirring time is 8 to 24 hours.
[0010] Furthermore, in the step (3), the calcination process is to first increase the temperature to 300°C-400°C and keep it at that temperature for 1-3 hours; then increase the temperature to 550°C-600°C and keep it at that temperature for 5-8 hours.
[0011] The present invention also provides the application of the sodium iron phosphate pyrophosphate composite material obtained by the above preparation method, which is applied to the positive electrode material of sodium ion battery.
[0012] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: (1) The technical solution of the present invention adds Na4Fe3(PO4)2P2O7 precursor, ammonia water and liquid titanium source into ethanol to dissolve and form solution A, so that the Na4Fe3(PO4)2P2O7 precursor and the titanium source are in contact with each other through the liquid phase, thereby improving the diffusion efficiency and compatibility of molecules between the two liquid phases of the Na4Fe3(PO4)2P2O7 dispersion and the titanium source liquid. By using ethanol as a solvent and adding the liquid titanium source dropwise to reduce the hydrolysis rate of the titanium source, the titanium compound can be more effectively coated on the surface of the Na4Fe3(PO4)2P2O7 sphere in the liquid phase. Compared with solid phase contact coating, firstly, the amount of coated titanium compound and the thickness of the titanium coating layer are controllable, thereby improving the consistency of the target material and stabilizing the electrochemical performance of the product; secondly, the uniformity of the titanium compound coating is improved, which not only effectively avoids the problems of material agglomeration and sintering during the calcination process; but also the uniform coating layer on the surface can effectively reduce the loss of active transition metals, avoid side reactions such as electrolyte decomposition, and improve the cyclic stability of the material.
[0013] (2) When using the spray drying method to prepare the precursor, a flow rate that is too fast will cause incomplete drying of the material and nozzle clogging, and a high drying temperature will lead to increased energy consumption. The technical solution of the present invention achieves the goal of low energy consumption and high efficiency sample preparation by matching the appropriate drying temperature and flow rate. The sodium iron phosphate pyrophosphate composite material is formed by calcining in an Ar-H2 mixed atmosphere. H2 can not only prevent the iron ions from having multiple valence states that affect the purity and specific capacity of the target material, but also dope H into the titanium dioxide during the calcination process to form defects on the surface of the material - a hydrogen-doped titanium dioxide coating layer. There are some Ti 4+ and Ti 2+ , local charge flow is formed between ions of different valence states. The material has a carbon network structure inside the bulk phase and a defective titanium dioxide layer on the surface, which can effectively improve the conductivity of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a SEM morphology image of the Na4Fe3(PO4)2P2O7 precursor obtained in Example 1 at an electron microscope magnification of 6390 times; Figure 2 This is a SEM morphology image of the sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7@H-TiO2) prepared in Example 1 at an electron microscope magnification of 7670 times; Figure 3This is the SEM morphology of the Na4Fe3(PO4)2P2O7 material obtained in the comparative example at 2250 times; Figure 4 This is the XRD diffraction pattern of the sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7@H-TiO2) obtained in Example 1; Figure 5 This is a long cycle performance diagram of the sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7@H-TiO2) obtained in Example 1 used as a positive electrode material in a sodium ion battery at a current density of 0.5C. DETAILED DESCRIPTION
[0015] The present invention is further described in detail below in conjunction with the embodiments. The drawings and embodiments of the specification are only used to explain the present invention and do not constitute an improper limitation of the present invention. Example 1
[0016] (1) Add 0.4 mol sodium dihydrogen phosphate, 0.3 mol ferric nitrate, and 0.05 mol citric acid to 1 L of deionized water and stir for 3 h. -1 The Na4Fe3(PO4)2P2O7 precursor was obtained by spray drying under the following conditions; 0.2 g of the Na4Fe3(PO4)2P2O7 precursor and 0.2 mL of 25-28 wt% ammonia water were added to 50 mL of ethanol and ultrasonically dispersed for 15 min; 0.2 mL of tetrabutyl titanate was added dropwise during stirring to form solution A; (2) placing solution A in an oil bath and heating and stirring at 45°C for 12 hours to form a suspension B; filtering the suspension B, washing the solid with ethanol, and then drying to obtain a Na4Fe3(PO4)2P2O7 precursor coated with a titanium compound; (3) The titanium compound-coated Na4Fe3(PO4)2P2O7 precursor was calcined in an Ar-H2 mixed atmosphere, first at 300°C for 3 h and then at 550°C for 8 h to obtain a sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7@H-TiO2).
[0017] like Figure 1 As shown, the surface of the Na4Fe3(PO4)2P2O7 precursor spheres prepared by spray drying is relatively rough; Figure 2As shown, the surface of the Na4Fe3(PO4)2P2O7 precursor sphere is coated with a smooth hydrogen-doped titanium dioxide layer. In the technical solution of the present invention, the Na4Fe3(PO4)2P2O7 precursor is in liquid phase contact with the titanium source, which improves the diffusion efficiency and compatibility of molecules between the two liquid phases of the Na4Fe3(PO4)2P2O7 dispersion and the titanium source liquid, so that the titanium compound is evenly coated on the surface of the Na4Fe3(PO4)2P2O7 sphere. Compared with the traditional solid phase contact coating, the amount of coated titanium compound and the thickness of the titanium coating layer are controllable, which improves the consistency of the target material and stabilizes the electrochemical performance of the product; in addition, the coating of the hydrogen-doped titanium dioxide layer can effectively avoid the problems of material agglomeration and sintering; Figure 3 As shown, the surface of the Na4Fe3(PO4)2P2O7 material obtained in the comparative example is not coated with a hydrogen-doped titanium dioxide layer, and the material is adhered and sintered to a certain extent during the calcination process. The XRD diffraction test of the material obtained in Example 1 is performed, as shown in FIG. Figure 4 As shown in the figure, it can be seen that sodium iron pyrophosphate composite material (Na4Fe3(PO4)2P2O7@H-TiO2) was prepared.
[0018] The titanium compound coated Na4Fe3(PO4)2P2O7 precursor prepared in Example 1 is calcined in an Ar-H2 mixed atmosphere to form a sodium iron phosphate pyrophosphate composite material. The material has a carbon network structure inside the bulk phase and good conductivity. A hydrogen-doped titanium dioxide coating layer, i.e., a defective titanium dioxide layer, is formed on the external interface of the material. Part of Ti 4+ and Ti 2+ , local charge flow is formed between ions of different valence states, which effectively improves the conductivity of the material. Uniformly coating the defective titanium dioxide layer on the surface of the material can reduce the loss of active transition metals, avoid side reactions such as electrolyte decomposition, and thus improve the cycle stability of the material. The obtained sodium iron phosphate pyrophosphate composite material is used as a positive electrode material in sodium ion batteries, and the electrochemical performance test is carried out using the LAND battery test system (CT2100A), such as Figure 5 As shown in Figure 2, the reversible specific capacity can still be maintained at 92.63 mAh g after 1500 cycles at a current density of 0.5 C. -1 . Example 2
[0019] (1) Add 0.43 mol sodium hypophosphite, 0.3 mol ferric nitrate, and 0.08 mol ascorbic acid to 1 L of deionized water and stir for 3 h. -1The Na4Fe3(PO4)2P2O7 precursor was obtained by spray drying under the following conditions. 0.2g of the Na4Fe3(PO4)2P2O7 precursor and 0.1mL of 25-28wt% ammonia water were added to 50mL of ethanol and ultrasonically dispersed for 15min; 0.3mL of titanium tetraisopropoxide was added dropwise during stirring to form solution A; (2) placing solution A in a water bath and heating and stirring at 60° C. for 8 h to form a suspension B; filtering the suspension B, washing the solid with ethanol, and then drying to obtain a Na4Fe3(PO4)2P2O7 precursor coated with a titanium compound; (3) The titanium compound-coated Na4Fe3(PO4)2P2O7 precursor was calcined in an Ar-H2 mixed atmosphere, first at 400°C for 1 h and then at 600°C for 5 h to obtain a sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7@H-TiO2). Example 3
[0020] (1) Add 0.45 mol sodium dihydrogen phosphate, 0.3 mol ferric chloride, and 0.1 mol citric acid into 1 L of deionized water and stir for 3 h. The reaction solution is heated at 110 °C for 300 mL / min. -1 The Na4Fe3(PO4)2P2O7 precursor was obtained by spray drying under the following conditions. 0.2 g of the Na4Fe3(PO4)2P2O7 precursor and 0.2 mL of 25-28 wt% ammonia water were added to 50 mL of ethanol and ultrasonically dispersed for 15 min; 0.4 mL of titanium tetrachloride was added dropwise during stirring to form solution A; (2) placing solution A in an oil bath and heating and stirring at 45°C for 24 hours to form a suspension B; filtering the suspension B, washing the solid with ethanol, and then drying to obtain a Na4Fe3(PO4)2P2O7 precursor coated with a titanium compound; (3) The titanium compound-coated Na4Fe3(PO4)2P2O7 precursor was calcined in an Ar-H2 mixed atmosphere, first at 300°C for 3 h and then at 550°C for 8 h to obtain a sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7@H-TiO2). Comparative Example
[0021] (1) Add 0.4 mol sodium dihydrogen phosphate, 0.3 mol ferric nitrate, and 0.05 mol citric acid into 1 L of deionized water and stir for 3 h. -1 The Na4Fe3(PO4)2P2O7 precursor was obtained by spray drying under the following conditions; (2) The Na4Fe3(PO4)2P2O7 precursor was calcined in an Ar atmosphere, first at 300°C for 3 h, and then heated to 550°C for 8 h to obtain sodium iron phosphate pyrophosphate material (Na4Fe3(PO4)2P2O7).
[0022]
[0023] The materials prepared in the examples and comparative examples were used as positive electrodes in sodium ion batteries. From the data in Table 1, it can be seen that the electrochemical performance of the material obtained in Example 1 is the best. From the comparative example results, it can be seen that coating the surface of the material with a defective titanium dioxide layer has a significant effect on the cycle stability and capacity retention rate of the battery, proving that part of the TiO2 in the defective titanium dioxide layer 4+ and Ti 2+ , local charge flow is formed between ions of different valence states, which effectively improves the conductivity of the material; and uniformly coating the defective titanium dioxide layer on the surface of the material can reduce the loss of active transition metals, avoid side reactions such as electrolyte decomposition, and improve the cycle stability of the material, such as Figure 5 As shown, the target material in Example 1 is applied to a sodium ion battery and the reversible specific capacity can still be maintained at 92.62 mAh g after 1500 cycles at a current density of 0.5 C. -1 .
Claims
1. A method for preparing a sodium iron phosphate pyrophosphate composite material, characterized in that: The steps include: (1) dissolving an inorganic salt containing sodium and phosphorus, an inorganic strong acid iron salt, and an organic acid carbon source in deionized water and stirring the mixture for reaction, spray drying the reaction solution to obtain a Na4Fe3(PO4)2P2O7 precursor; adding the Na4Fe3(PO4)2P2O7 precursor and ammonia water into ethanol for ultrasonic dispersion, and then adding a liquid titanium source dropwise under stirring to form a solution A; (2) placing solution A in a water bath or an oil bath, heating and stirring to form a suspension B; filtering the suspension B, washing the solid with ethanol, and drying the solid to obtain a Na4Fe3(PO4)2P2O7 precursor coated with a titanium compound; (3) The titanium compound-coated Na4Fe3(PO4)2P2O7 precursor is calcined in an Ar-H2 mixed atmosphere to obtain a sodium iron phosphate pyrophosphate composite material.
2. The method for preparing the sodium iron phosphate pyrophosphate composite material according to claim 1, characterized in that: In the step (1), the inorganic salt containing sodium and phosphorus is sodium dihydrogen phosphate or sodium hypophosphite; the inorganic strong acid iron salt is ferric nitrate or ferric chloride; the organic acid carbon source is citric acid or ascorbic acid; the molar ratio of the inorganic salt containing sodium and phosphorus, the inorganic strong acid iron salt, and the organic acid carbon source is 0.4-0.45 mol:0.3 mol:0.05-0.1 mol; the spray drying temperature is 110-150°C; and the flow rate is 200-300 mL / h -1 ; The liquid titanium source is one of tetrabutyl titanate, titanium tetraisopropoxide or titanium tetrachloride; the mass volume ratio of Na4Fe3(PO4)2P2O7 precursor and liquid titanium source is 0.2g:0.2mL~0.4mL; the concentration of ammonia water is 25~28wt%; the volume ratio of ammonia water and ethanol is 0.1mL~0.2mL:50mL.
3. The method for preparing the sodium iron phosphate pyrophosphate composite material according to claim 1, characterized in that: In the step (2), the heating temperature is 45-60° C. and the stirring time is 8-24 hours.
4. The method for preparing the sodium iron phosphate pyrophosphate composite material according to claim 1, characterized in that: In the step (3), the calcination process is to first raise the temperature to 300°C-400°C and keep it at that temperature for 1-3 hours; then raise the temperature to 550°C-600°C and keep it at that temperature for 5-8 hours.
5. An application of the sodium iron pyrophosphate composite material prepared by the method according to any one of claims 1 to 4, characterized in that: The sodium iron phosphate pyrophosphate composite material is used as a positive electrode material for sodium ion batteries.
Citation Information
Patent Citations
Titanium sub-oxide coated and modified lithium iron phosphate composite material and preparation method thereof
CN105489864A
Preparation method of iron manganese phosphate
CN108306003A
Oxygen-deficient titanium dioxide-coating tin-doped manganese oxide lithium ion battery negative electrode material, preparation method thereof and lithium battery
CN110289404A
Preparation method of sodium ion negative electrode material MoP-coated TiO2
CN115275158A
Preparation method and application of hydrogenated titanium dioxide modified core-shell structure porous ferroferric oxide and nickel oxide
CN115472801A
Cited By
A sodium titanium phosphate-coated sodium iron pyrophosphate composite material and a preparation method thereof
CN122930864A