Aerogel and preparation method thereof
By combining paraaramid, dopamine and chitosan/organic acids, multifunctional aerogels are prepared, which solves the problem of difficulty in separation and single adsorption after adsorption in the prior art, and achieves efficient adsorption of heavy metals and dyes and recycled, with various physical and chemical mechanism adsorption capabilities, low production costs and environmentally friendly.
Patent Information
- Application Number
- CN202411273126.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-08
AI Technical Summary
The existing para-aramid aerogels are difficult to separate after adsorption and have a single adsorption capacity, which cannot effectively adsorb heavy metals and dyes, and are difficult to recycle.
By combining para-aramid with dopamine and chitosan/organic acids, a multifunctional aerogel is prepared, utilizing the chelating ability of chitosan and organic acids, solvent resistance and high specific surface area of aramid, Achieve efficient adsorption of heavy metals and dyes, and improve the recyclability of materials through specific preparation methods.
The adsorption rate of heavy metals and dyes has reached 80-90%, and it still maintains high adsorption after multiple desorptions. The material has the adsorption capacity of various physical and chemical mechanisms, and is low in production costs and environmentally friendly.
Smart Images

Figure CN118904221A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of environmentally friendly treatment materials, and in particular to an aerogel, in particular to a multifunctional aerogel containing para-aramid / dopamine / chitosan / organic acid and a preparation method thereof. Background Art
[0002] As a new type of aerogel, para-aramid aerogel has excellent mechanical properties, high thermal stability, solvent resistance, and also exhibits excellent high specific surface area and surface activity, high aspect ratio and other characteristics. Therefore, aramid aerogel can be used as an excellent reinforcing building unit / matrix for the extensive construction of various new aerogels and high-performance nanocomposites.
[0003] Based on the excellent performance of para-aramid aerogel, it can be used as an adsorbent in sewage treatment. However, the existing para-aramid aerogel adsorbent has the problems of single adsorption capacity and difficult separation after adsorption. CN112403447A discloses an aerogel based on aramid nanofibers. A PAPAM / aramid nanofiber composite hydrogel is obtained by compounding Kevlar fibers with polyamide amine dendrimers (PAPAM) in an alkaline DMSO solution. The composite hydrogel can be used for the adsorption of organic dyes and metal ions, but its chemical adsorption is mainly through hydrogen bonding forces, and does not support the adsorption of organic dyes or metal ions in the form of chelation.
[0004] Therefore, whether it is possible to combine para-aramid aerogel to provide a multifunctional aerogel has become one of the problems that technicians in this field need to solve urgently. Summary of the invention
[0005] In view of the many problems existing in the existing para-aramid aerogel, the present invention provides an aerogel and a preparation method thereof. The aerogel contains para-aramid, dopamine, and chitosan / organic acid. The preparation method comprises the following steps: subjecting the para-aramid to alkali treatment, solvent exchange, and freeze drying to obtain an aerogel, and then subjecting the para-aramid to dopamine treatment to obtain an aramid / dopamine aerogel, and then impregnating the aerogel with a chitosan / organic acid composite liquid, and subjecting the aerogel to washing, solvent exchange, and freeze drying to obtain a multifunctional aerogel. The obtained aerogel combines the stability and high specific surface area of the aramid aerogel with the chelating and adsorption capabilities of chitosan and organic acid, and the adsorption rate of waste liquid for heavy metals and dyes can reach 80-90%, and the aerogel still has high adsorption after multiple desorptions, and can be recycled.
[0006] The main idea of the present invention is:
[0007] Chitosan is obtained by deacetylation of natural polymer chitin. Chitosan comes from the shells and cell walls of animals such as shrimps and crabs in nature. Its annual output is second only to cellulose, and its production process is simple. The adsorption advantage of chitosan is that it contains hydroxyl and amino groups, and its special functional groups have a certain chelating effect on hexavalent chromium. Organic acids are also taken from natural plants. The natural acquisition method makes organic acids widely used. Its unique carboxyl and hydroxyl groups also have a certain chelating effect and adsorption capacity on heavy metals and dyes. The combination of chitosan and organic acids makes the composite material have the special properties of chitosan and organic acids at the same time, which greatly plays the role of raw materials. At present, the para-aramid aerogel adsorbent on the market has the problem of single adsorption capacity and difficult separation after adsorption. This application finally organically integrates para-aramid aerogel and chitosan / organic acid, which not only combines the advantages of para-aramid solvent resistance, stability and high specific surface area, but also includes the chelating ability and adsorption capacity of chitosan / organic acid. The aerogel finally obtained is a multifunctional adsorption composite material.
[0008] The specific technical solutions of the present invention are as follows:
[0009] An aerogel, wherein the aerogel contains para-aramid, dopamine, and chitosan / organic acid, wherein the mass ratio of para-aramid:dopamine:chitosan / organic acid is (9.4-9.65):(0.08-0.15):
[0010] (0.2-0.52), the specific surface area of aerogel is (80-200) m 2 / g.
[0011] The above-mentioned aerogel is a new material with a large specific surface area. Its pore structure is honeycomb-like, light, porous, and extremely light, with a density only about three times that of air. With para-aramid nanofibers as the main body, a high-strength and high-toughness material is finally obtained, and the addition of dopamine can increase the functional groups on the surface of aramid, which is conducive to the attachment of chitosan / organic acid, and the attachment of chitosan / organic acid can make the whole material have chelating properties and recyclable properties.
[0012] In addition, the inventors also provide a method for preparing the above-mentioned aerogel, comprising the following steps:
[0013] 1) dissolving aramid and alkali in a solvent, stirring evenly and removing excess alkali, standing to remove bubbles; washing the residual solvent, exchanging solvents, and freeze-drying to obtain aramid aerogel;
[0014] 2) placing the aramid aerogel obtained in step 1) in a dopamine solution and mixing well, washing to remove the dopamine remaining on the surface, thereby obtaining an aramid / dopamine aerogel;
[0015] 3) dissolving chitosan in acetic acid, adding an organic acid after the chitosan is dissolved, adding potassium persulfate after the chitosan is dissolved, and reflux heating to react to obtain chitosan / organic acid;
[0016] 4) The aramid / dopamine aerogel obtained in step 2) is mixed with the chitosan / organic acid obtained in step 3), and the target aerogel is obtained by washing, solvent exchange, pre-freezing, and freeze-drying.
[0017] More specifically, the step 1) is:
[0018] First, the long linear aramid yarn is cut into small segments, the yarn segments and KOH are weighed, added to DMSO, and magnetically stirred at room temperature for one week until the solution is dissolved and turns dark red; the excess KOH particles in the liquid are removed by centrifugation, and then the liquid is kept at a constant temperature for a certain period of time to remove bubbles; the aramid DMSO solution is then transferred to deionized water and soaked for a certain period of time to remove the residual solvent to obtain an ANFs solution; the ANFs solution from which the residual solvent has been removed is soaked in a mixed solution of tert-butanol and water for solvent exchange, and finally the ANFs solution after solvent exchange is transferred to a refrigerator for pre-freezing, and then the aramid aerogel is obtained by a freeze dryer.
[0019] The aramid is para-aramid, the aramid is a small yarn segment with a length of 4-6 mm, the alkali is granular KOH, the solvent is DMSO, the mass ratio of aramid to KOH is (0.3-0.8):1, and the mass ratio of aramid to DMSO is 0.5-1:100; the dissolution temperature is 20-25°C, the magnetic rotation speed is 1000-2000rpm, the solution is dissolved until it turns dark red, and the dissolution time is at least 1 week.
[0020] In this step, excess alkali is removed by centrifugation at a speed of 1000-2000 rpm for 30-60 min; the bubbles are removed by standing for 4-6 h; and the residual solvent is then removed by soaking in deionized water for 24-48 h, during which the deionized water is replaced by centrifugation every 6 h.
[0021] Then, a mixed solution of tert-butanol and water is used for solvent exchange, the mass ratio of tert-butanol to water is 0.8-1.5:1, and the solvent exchange time is 24-48 hours; the refrigerator is pre-frozen at -18°C for 5-8 hours, and then freeze-dried in a freeze dryer at -55°C to -45°C for 12-24 hours to obtain aramid aerogel.
[0022] The aramid aerogel obtained at this time has an extremely large specific surface area, and its pore structure is shaped like a honeycomb. It is light, porous, and extremely light, with a density only about three times that of air.
[0023] Furthermore, in step 2), the concentration of the dopamine solution is 2-8 mg / mL, the concentration of the aramid aerogel is 0.5-2 g / 100 ml, the pH is adjusted to 8.5, and the aramid aerogel and the dopamine solution are mixed by oscillation, the oscillation rate is 65-70 rpm, the oscillation temperature is 20-25° C., and the oscillation time is 24-48 h; the liquid for washing the aerogel is selected from ethanol or water or used alternately to ensure that the dopamine particles remaining on the surface are rinsed clean; the aramid / dopamine aerogel obtained at this time has significantly more surface attachment points than the aramid aerogel in the previous step.
[0024] Furthermore, in the step 3), the volume concentration of acetic acid is 2%, chitosan g: acetic acid mL = 1: 2-5, and the time for chitosan to completely dissolve is 3-5h; the dissolved chitosan solution is transparent; chitosan g: organic acid mL / g = 3-5: 1; the organic acid used is selected from a mixture of one or more of oxalic acid, citric acid, tartaric acid, oxalic acid, malonic acid, lactic acid, and malic acid, wherein the organic acid is directly measured in mL when it is liquid; it is measured in g when it is solid, and when used, it is dissolved or diluted to a solution with a mass concentration of 1% and then added to the system; the amount of potassium persulfate is 0.05-0.1 mol per 100 ml of solution; the reflux temperature is 70-80°C, and the reflux time is 7-10h.
[0025] Organic acid can modify chitosan, diversifying the functional groups on the surface of chitosan and providing more adsorption sites, which are conducive to adsorption. A single chitosan functional group is single and inactive, and a single organic acid has no effect on aerogel. The combined effect of the two achieves the above-mentioned effect of the present application.
[0026] Furthermore, in the step 4), the weight ratio of aramid to chitosan is 10-15:1; the aramid / dopamine aerogel and chitosan / organic acid are mixed by shaking at a speed of 50-65 rpm for 24-48 hours;
[0027] A mixed solution of tert-butyl alcohol and water is used for solvent exchange, the mass ratio of tert-butyl alcohol to water is 0.8-1.5:1, and the solvent exchange time is 24-48 hours; the refrigerator is pre-frozen at -18℃ for 5-10 hours, and then freeze-dried in a freeze dryer at -55℃ to -45℃ for 12-24 hours to obtain the target aerogel. At this time, the surface energy groups of the aerogel increase, and it has chelating and adsorption properties, which can solve the problems of single adsorption and poor adsorption cycle, and the production process is simple and easy to use.
[0028] The aramid / dopamine / chitosan / organic acid multifunctional aerogel prepared by the method can be used for the adsorption and removal of heavy metals and dyes in wastewater.
[0029] The present invention can achieve the following technical effects:
[0030] 1) The aramid / dopamine / chitosan / organic acid multifunctional aerogel obtained by this scheme combines the advantages of aramid such as solvent resistance, stability and high specific surface area, and combines the chelation and adsorption capacity of chitosan and organic acid. Chitosan itself has a certain pore structure, but the overall surface tends to be smoother, and the combination form of organic acid and chitosan will affect the morphology of chitosan, presenting a honeycomb shape, which is conducive to adhesion.
[0031] 2) The aramid / dopamine / chitosan / organic acid multifunctional aerogel obtained by this scheme has increased attachment points due to dopamine, which is beneficial to the combination of other functional groups, and the combination of chitosan and organic acid increases the functional group density of amino, hydroxyl and carboxyl in the material. Its special functional group dyes and heavy metals, especially hexavalent chromium, have obvious chelation and adsorption capacity, thus giving the material the property of adsorbing pollutants by multiple physical and chemical mechanisms, so that the composite material has the special properties of chitosan and organic acid at the same time.
[0032] 3) Chitosan is a low-cost, high-yield, and environmentally friendly raw material. It is a product of deacetylation of natural high-molecular chitosan. Chitosan comes from the shells of animals such as shrimps and crabs. It has a large annual output and a simple production process. The present invention uses chitosan as a raw material, which significantly reduces the production cost and has good environmental compatibility;
[0033] 4) The aramid / dopamine / chitosan / organic acid multifunctional aerogel obtained by this scheme can be recycled and reused, and still has a high adsorption capacity after multiple desorptions. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a morphology picture of the aramid aerogel obtained in step (1) of Example 1. It can be seen that the obtained aramid aerogel has an ultra-large specific surface area, and its pore structure is honeycomb-shaped, light and porous.
[0035] Figure 2 This is a morphology image of the aramid / dopamine aerogel obtained in step (2) of Example 1. It can be seen that the surface attachment points of the obtained aramid / dopamine aerogel are significantly increased compared with the aramid aerogel.
[0036] Figure 3 This is the morphology of the aramid / dopamine / chitosan / organic acid aerogel obtained in step (4) of Example 1. It can be seen that the pores on the surface of the aerogel are increased, and it has an ultra-large specific surface area. DETAILED DESCRIPTION
[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments. These embodiments are only used to illustrate the technical solution of the present invention in more detail and should not be construed as limiting the protection scope of the present invention.
[0038] The sources of the materials and reagents used in the examples are as follows: aramid is long-line para-aramid purchased from Shandong Jufang New Materials Co., Ltd., with specifications of 6500D, 650F; dopamine was purchased from Shanghai Myrel Biochemical Technology Co., Ltd.; chitosan was purchased from Shandong Haiyihua Biotechnology Co., Ltd., with specifications of deacetylation degree 85% and molecular weight 5000; tartaric acid was purchased from Anhui Aibo Biotechnology Co., Ltd.; oxalic acid was purchased from Jinan Guocheng Chemical Co., Ltd.; other materials or reagents, unless otherwise specified, are general commercial products.
[0039] Example 1
[0040] An aerogel, the aerogel contains para-aramid, dopamine, chitosan / organic acid, wherein the mass ratio of para-aramid: dopamine: chitosan / organic acid is 9.5: 0.1: 0.4, and the specific surface area is 185m 2 / g, and the organic acid is oxalic acid.
[0041] The preparation method of the above-mentioned aerogel comprises the following specific steps:
[0042] (1) Preparation of pure aramid aerogel: First, cut the long linear aramid yarn into 4 mm small segments, weigh 2 g of yarn segments, grind the flake KOH into fine particles with a mortar, take 4 g of KOH fine particles, measure 200 ml of DMSO and add them to a beaker together, stir at room temperature 20 ° C, magnetic speed 1000 rpm until the solution turns dark red; centrifuge to remove excess KOH particles in the liquid, the centrifugal KOH speed is 1000 rpm, time 30 min, then keep it at room temperature for a certain time, keep it at a constant temperature of 20 ° C, time 4 h, and remove bubbles. Then, transfer the aramid solution to deionized water and soak it for a certain time, the soaking time is 24 h (the deionized water is replaced every 6 h during this period) to remove the residual solvent; soak the prepared ANFs gel in 400 ml of a mixed solution of tert-butyl alcohol and water (the mass ratio of tert-butyl alcohol to water is 1:1) to perform complete solvent exchange, and the full solvent exchange time is 24 h. Finally, the ANFs were transferred to a refrigerator for pre-freezing (-18 °C) for 5 h, and then freeze-dried (-45 °C) for 12 h to obtain the ANFs aerogel.
[0043] (2) Preparation of aramid / dopamine aerogel: ANFs aerogel was immersed in 100 ml of dopamine (PDA) solution, with pH = 8.5 and concentration of 2 mg / mL, and oscillated evenly at 20 °C, 65 rpm, and 24 h. The prepared aramid / dopamine was rinsed twice with 50 ml of ethanol and 100 ml of water to ensure that the PDA particles remaining on the surface were rinsed clean.
[0044] (3) Preparation of chitosan / oxalic acid: Dissolve 0.2 g of chitosan in 50 ml of acetic acid solution in a conical flask. The volume concentration of the acetic acid solution is 2%. After the chitosan is completely dissolved and becomes transparent (3 h), add it dropwise to 4 ml of 1 wt% oxalic acid solution prepared in advance. When the two are dissolved evenly, add 0.05 mol of KPS and heat at reflux temperature of 70°C for 7 h. The final solution is yellow.
[0045] (4) Preparation of aramid / dopamine / chitosan / oxalic acid multifunctional aerogel: The aramid / dopamine aerogel was oscillated in chitosan / oxalic acid for a certain period of time at a temperature of 25°C, a rotation speed of 65 rpm, and an oscillation time of 48 h; it was rinsed with deionized water and then transferred to 400 ml of a mixed solution of tert-butanol and water, with a mass ratio of tert-butanol to water of 0.8:1, and a complete solvent exchange was performed for 48 h; finally, the material after solvent exchange was transferred to a refrigerator for pre-freezing at a refrigerator temperature of -18°C for a pre-freezing time of 5 h, and then freeze-dried in a freeze dryer (-45°C) for 12 h to obtain the aramid / dopamine / chitosan / oxalic acid multifunctional aerogel.
[0046] The mass ratio of para-aramid fiber: dopamine: chitosan / oxalic acid in the aerogel was 9.5: 0.1: 0.4, and its specific surface area was 185 m 2 / g.
[0047] like Figure 1-3 As shown: the morphology of the aramid aerogel obtained in step (1) of Example 1 shows that the obtained aramid aerogel has an ultra-large specific surface area, and its pore structure is honeycomb-shaped, light and porous; the morphology of the aramid / dopamine aerogel obtained in step (2) shows that the surface attachment points of the obtained aramid / dopamine aerogel are significantly increased compared with the aramid aerogel; the morphology of the aramid / dopamine / chitosan / organic acid aerogel obtained in step (4) shows that the pores on the aerogel surface are increased, and it has an ultra-large specific surface area.
[0048] Example 2
[0049] An aerogel, the aerogel contains para-aramid, dopamine, chitosan / organic acid, wherein the mass ratio of para-aramid: dopamine: chitosan / organic acid is 9.6: 0.12: 0.28, and the surface area is 170m 2 / g, and the organic acid is tartaric acid.
[0050] The preparation method of the above-mentioned aerogel comprises the following specific steps:
[0051] (1) Preparation of pure aramid aerogel: First, cut the long linear aramid yarn into 6 mm small segments, weigh 3.2 g of yarn segments, 4 g of KOH fine particles, grind the flake KOH into fine particles with a mortar, measure 400 ml of DMSO and add it to a beaker together with the above substances, stir at room temperature 25 ° C, and stir at a magnetic speed of 2000 rpm until the solution turns dark red. Centrifuge to remove excess KOH particles in the liquid, the centrifugal KOH speed is 2000 rpm, the time is 60 min, and then stand at room temperature for a certain time, the constant temperature is 25 ° C, the time is 6 hours, and the bubbles are removed. Then, the aramid solution is transferred to deionized water and soaked for a certain time, the soaking time is 48 hours (the deionized water is replaced every 6 hours during this period) to remove the residual solvent; the prepared ANFs gel is soaked in a mixed solution of tert-butyl alcohol and water (the mass ratio of tert-butyl alcohol to water is 1.5:1) for complete solvent exchange, and the full solvent exchange time is 48 hours. Finally, the ANFs were transferred to a refrigerator for pre-freezing (-18 °C) for 8 h, and then freeze-dried in a freeze dryer for 24 h to obtain the ANFs aerogel.
[0052] (2) Preparation of aramid / dopamine aerogel: ANFs aerogel was then immersed in 200 ml of dopamine (PDA) solution, with a pH of 8.5 and a concentration of 8 mg / mL, and the aerogel was shaken evenly at a temperature of 25°C, a speed of 70 rpm, and a shaking time of 48 h. The prepared aramid-dopamine was rinsed twice with 30 ml of ethanol and 150 ml of water to ensure that the PDA particles remaining on the surface were washed clean.
[0053] (3) Preparation of chitosan / tartaric acid: Dissolve 0.3 g of chitosan in 75 ml of acetic acid solution in a conical flask with a volume concentration of 2%. After the chitosan is completely dissolved and becomes transparent (5 h), add 10 ml of 1 wt% tartaric acid prepared in advance dropwise. When the two are evenly dissolved, add 0.06 mol of KPS and heat at reflux temperature of 80°C for 10 h. The final solution is yellow.
[0054] (4) Preparation of aramid / dopamine / chitosan / tartaric acid multifunctional aerogel: All (2) aramid / dopamine aerogels were oscillated in chitosan / tartaric acid for a certain period of time, at an oscillation temperature of 20°C, a rotation speed of 50 rpm, and an oscillation time of 24 h. Finally, they were rinsed with deionized water and then transferred to a tert-butyl alcohol mixed solution, with a mass ratio of tert-butyl alcohol to water of 0.8:1 and a mixed solution volume of 300 ml, for complete solvent exchange, and the complete solvent exchange lasted for 24 h. Finally, the solvent-exchanged material was transferred to a refrigerator for pre-freezing, at a refrigerator temperature of -18°C, for a pre-freezing time of 5 h, and then freeze-dried (-50°C) for 12 h in a freeze dryer to obtain aramid / dopamine / chitosan / tartaric acid multifunctional aerogel.
[0055] The mass ratio of para-aramid: dopamine: chitosan / tartaric acid in the aerogel was 9.6: 0.12: 0.28, and its surface area was 170 m 2 / g.
[0056] Comparative Example 1
[0057] An aramid / dopamine aerogel, wherein the mass ratio of aramid to dopamine is 9.71:0.29 and the surface area is 57 m 2 / g.
[0058] The preparation method of the above-mentioned aerogel comprises the following specific steps:
[0059] (1) Preparation of pure aramid aerogel: First, cut the long linear aramid yarn into 4 mm small segments, weigh 2 g of yarn segments, 4 g of KOH fine particles, grind the flake KOH into fine particles with a mortar, measure 200 ml of DMSO and add it to a beaker together with the above substances, stir at room temperature 20 ° C, and stir at a magnetic speed of 1000 rpm until the solution turns dark red. Centrifuge to remove excess KOH particles in the liquid, the centrifugal KOH speed is 1000 rpm, the time is 30 min, and then stand at room temperature for a certain time, the constant temperature is 20 ° C, the time is 4 hours, and the bubbles are removed. Then, the aramid solution is transferred to deionized water and soaked for a certain time, the soaking time is 24 hours (the deionized water is replaced every 6 hours during this period) to remove the residual solvent; the prepared ANFs gel is soaked in a mixed solution of tert-butyl alcohol and water (the mass ratio of tert-butyl alcohol to water is 1:1) for complete solvent exchange, and the full solvent exchange time is 24 hours. Finally, the ANFs were transferred to a refrigerator for pre-freezing (-18 °C) for 5 h, and then freeze-dried in a freeze dryer for 12 h to obtain the ANFs aerogel.
[0060] (2) Preparation of aramid / dopamine aerogel: ANFs aerogel was then immersed in 100 ml of dopamine (PDA) solution, with a pH of 8.5 and a concentration of 2 mg / mL, and the aerogel was shaken evenly at a temperature of 20°C, a speed of 65 rpm, and a shaking time of 24 h. The prepared aramid / dopamine was rinsed twice with 50 ml of ethanol and 200 ml of water to ensure that the PDA particles remaining on the surface were rinsed clean.
[0061] The mass ratio of aramid to dopamine in the aerogel was 9.71:0.29, and its surface area was 57m 2 / g.
[0062] Comparative Example 2
[0063] An aerogel, the aerogel contains para-aramid, dopamine, and chitosan, wherein the mass ratio of para-aramid: dopamine: chitosan is 9.8: 0.07: 0.13, and the surface area is 101m2 / g.
[0064] The preparation method of the above-mentioned aerogel comprises the following specific steps:
[0065] (1) Preparation of pure aramid aerogel: First, cut the long linear aramid yarn into 6 mm small segments, weigh 3.2 g of yarn segments, 4 g of KOH fine particles, grind the flake KOH into fine particles with a mortar, measure 400 ml of DMSO and add them to a beaker together with the above substances, stir at room temperature 25 ° C, and stir at a magnetic speed of 2000 rpm until the solution turns dark red. Centrifuge to remove excess KOH particles in the liquid, the centrifugal KOH speed is 2000 rpm, the time is 60 min, and then stand at room temperature for a certain time, the constant temperature is 25 ° C, the time is 6 hours, and the bubbles are removed. Then, the aramid solution is transferred to deionized water and soaked for a certain time, the soaking time is 48 hours (the deionized water is replaced every 6 hours during this period) to remove the residual solvent; the prepared ANFs gel is soaked in a mixed solution of tert-butyl alcohol and water (the mass ratio of tert-butyl alcohol to water is 1.5:1), the mixed solution volume is 300 ml, and a complete solvent exchange is carried out, and the full solvent exchange time is 48 hours. Finally, the ANFs were transferred to a refrigerator for pre-freezing (-18 °C) for 8 h, and then freeze-dried in a freeze dryer (-50 °C) for 24 h to obtain ANFs aerogel.
[0066] (2) Preparation of aramid / dopamine aerogel: ANFs aerogel was then immersed in 200 ml of dopamine (PDA) solution, with a pH of 8.5 and a concentration of 8 mg / mL, and the aerogel was shaken evenly at a temperature of 25°C, a speed of 70 rpm, and a shaking time of 48 h. The prepared aramid-dopamine was rinsed twice with 30 ml of ethanol and 150 ml of water to ensure that the PDA particles remaining on the surface were washed clean.
[0067] (3) Preparation of chitosan: 0.3 g of chitosan was dissolved in 75 ml of acetic acid solution in a conical flask. The volume concentration of acetic acid was 2%. After the chitosan was completely dissolved and became transparent (5 h), the final solution was yellow.
[0068] (4) Preparation of aramid / dopamine / chitosan multifunctional aerogel: All (2) aramid / dopamine aerogels were oscillated in chitosan for a certain period of time, at an oscillation temperature of 20°C, a rotation speed of 50 rpm, and an oscillation time of 24 h. Finally, they were rinsed with deionized water and then transferred to a tert-butanol mixed solution, with a mass ratio of tert-butanol to water of 0.8:1 and a mixed solution volume of 300 ml, for complete solvent exchange, and the complete solvent exchange lasted for 24 h. Finally, the solvent-exchanged material was transferred to a refrigerator for pre-freezing, at a refrigerator temperature of -18°C, for a pre-freezing time of 5 h, and then freeze-dried (-50°C) for 12 h in a freeze dryer to obtain aramid / dopamine / chitosan multifunctional aerogel.
[0069] The aerogel contains para-aramid, dopamine and chitosan, wherein the mass ratio of para-aramid: dopamine: chitosan is 9.8: 0.07: 0.13, and the surface area is 101m 2 / g.
[0070] Comparative Example 3
[0071] An aerogel, the aerogel contains para-aramid, dopamine, cellulose / organic acid, wherein aramid: dopamine: cellulose / organic acid = 9.66: 0.12: 0.22, and the surface area is 73m 2 / g, and the organic acid is tartaric acid.
[0072] The preparation method of the above-mentioned aerogel comprises the following specific steps:
[0073] (1) Preparation of pure aramid aerogel: First, cut the long linear aramid yarn into 6 mm small segments, weigh 3.2 g of yarn segments, 4 g of KOH fine particles, grind the flake KOH into fine particles with a mortar, measure 400 ml of DMSO and add them to a beaker together with the above substances, stir at room temperature 25 ° C, and stir at a magnetic speed of 2000 rpm until the solution turns dark red. Centrifuge to remove excess KOH particles in the liquid, the centrifugal KOH speed is 2000 rpm, the time is 60 min, and then stand at room temperature for a certain time, the constant temperature is 25 ° C, the time is 6 hours, and the bubbles are removed. Then, the aramid solution is transferred to deionized water and soaked for a certain time, the soaking time is 48 hours (the deionized water is replaced every 6 hours during this period) to remove the residual solvent; the prepared ANFs gel is soaked in a mixed solution of tert-butyl alcohol and water (the mass ratio of tert-butyl alcohol to water is 1.5:1), the mixed solution volume is 300 ml, and a complete solvent exchange is carried out, and the full solvent exchange time is 48 hours. Finally, the ANFs were transferred to a refrigerator for pre-freezing (-18 °C) for 8 h, and then freeze-dried in a freeze dryer (-50 °C) for 24 h to obtain ANFs aerogel.
[0074] (2) Preparation of aramid / dopamine aerogel: ANFs aerogel was then immersed in 200 ml of dopamine (PDA) solution, with a pH of 8.5 and a concentration of 8 mg / mL, and the aerogel was shaken evenly at a temperature of 25°C, a speed of 70 rpm, and a shaking time of 48 h. The prepared aramid-dopamine was rinsed twice with 30 ml of ethanol and 150 ml of water to ensure that the PDA particles remaining on the surface were washed clean.
[0075] (3) Preparation of cellulose / tartaric acid: 0.3 g of cellulose was dissolved in 75 ml of acetic acid solution in a conical flask with a volume concentration of 2%. After the cellulose was completely dissolved and became transparent (5 h), 10 ml of 1 wt% tartaric acid prepared in advance was added dropwise. When the two were evenly dissolved, 0.06 mol of KPS was added and heated at reflux temperature of 80°C for 10 h. The final solution was yellow.
[0076] (4) Preparation of aramid / dopamine / cellulose / tartaric acid multifunctional aerogel: All (2) aramid / dopamine aerogels were shaken in cellulose / tartaric acid for a certain period of time, with an oscillation temperature of 20°C, a rotation speed of 50 rpm, and an oscillation time of 24 h. Finally, they were rinsed with deionized water and then transferred to a tert-butyl alcohol mixed solution, with a mass ratio of tert-butyl alcohol to water of 0.8:1 and a mixed solution volume of 300 ml, for complete solvent exchange, and the complete solvent exchange lasted for 24 h. Finally, the solvent-exchanged material was transferred to a refrigerator for pre-freezing, with a refrigerator temperature of -18°C and a pre-freezing time of 5 h, and then freeze-dried (-50°C) by a freeze dryer for 12 h to obtain aramid / dopamine / cellulose / tartaric acid multifunctional aerogel.
[0077] After testing, the aerogel contains para-aramid, dopamine, cellulose / organic acid, wherein aramid: dopamine: cellulose / organic acid = 9.66: 0.12: 0.22, and its surface area is 73m 2 / g.
[0078] Experimental example
[0079] 100 g of the aerogels obtained in Examples 1-2 and Comparative Examples 1-3 were taken respectively, and solution adsorption studies were performed on them:
[0080] Taking the adsorption of hexavalent chromium as the starting point, its adsorption mechanism is explored. Taking the aerogel of Example 1 as an example, its first-order kinetic correlation coefficient is relatively low, and the second-order kinetic correlation coefficient is above 0.999, which shows that the adsorption of chromium is more in line with the second kinetic equation. In terms of the equilibrium adsorption amount, there is a large gap between the equilibrium adsorption amount obtained by the first-order kinetics and the equilibrium adsorption amount obtained by the experiment, and the equilibrium adsorption amount obtained by the second-order kinetics is very small. Once again, it shows that the second-order kinetic equation is consistent with the adsorption behavior of aerogel on chromium. In terms of the adsorption model, the correlation coefficient of the Langmuir model for the adsorption of chromium is 0.9993, while the correlation coefficient of the Freundlich isotherm adsorption model is 0.9952. Under the comparison of correlation coefficients, the adsorption of chromium is more in line with the Langmuir model. The activation energy of adsorption of chromium is between 40 and 800, indicating that the combination of the aerogel of Example 1 and chromium may be chemically combined. In terms of free energy, the Gibbs free energy value is less than 0, which indicates that the adsorption of chromium by aerogel is feasible and spontaneous, while its enthalpy value is greater than 0, indicating that the adsorption process is an endothermic reaction, and its entropy value is also greater than 0, indicating that the degree of free disorder increases accordingly during the adsorption process.
[0081] The aerogels obtained in the above Examples 1-2 and Comparative Examples 1-3 are used for adsorption and removal of heavy metals and dyes in wastewater, taking the treatment of mixed wastewater of hexavalent chromium and methylene blue as an example:
[0082] Prepare polluted water of a certain concentration, record the initial concentration, the initial concentration of hexavalent chromium is 600 mg / L, the initial concentration of methylene blue is 200 ppm, place 100 grams of aerogel in 100L of sewage, continue stirring for 24 hours, measure the first adsorption concentration, and finally filter, wash with deionized water, use 0.1M sodium hydroxide solution as a remover, soak for 10-12 hours, and dry; then perform the second adsorption, the solution concentration is consistent with the initial concentration, and the other processes are the same as the first adsorption; finally, perform the third adsorption in the same way, and the adsorption effect is shown in Table 1 below:
[0083] Table 1
[0084]
[0085]
[0086] The detection method of chromium adopts the diphenylamino urea (D) method, and real-time monitoring is performed using a spectrophotometer at a wavelength of 540nm, and methylene blue is directly detected using a spectrophotometer at a wavelength of 664nm.
[0087] Compared with Example 1, Comparative Example 1 has no chitosan / organic acid attached, and the adsorption effect is greatly weakened, which shows that the presence of chitosan / organic acid greatly increases the adsorption of the material. Compared with Example 2, Comparative Example 2 has no modification of chitosan by organic acid, and the adsorption effect is significantly weakened, which shows that the modification of chitosan by organic acid is crucial. Compared with Example 2, the adsorption effect of Comparative Example 3 is weakened, which further shows the superiority of chitosan. It can be seen that the adsorption effect of the embodiment is obviously better than that of the comparative example. The increase in specific surface area will increase the adsorption of the material, and the presence of chitosan increases the desorption and then increases the desorption adsorption rate, so that it can be reused.
[0088] The embodiments described above are merely descriptions of preferred implementation modes of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary engineering technicians in the field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. An aerogel, Features: The aerogel contains para-aramid, dopamine, and chitosan / organic acid, wherein the mass ratio of para-aramid:dopamine:chitosan / organic acid is (9.4-9.65):(0.08-0.15):(0.2-0.52), and the specific surface area of the aerogel is (80-200) m 2 / g.
2. The method for preparing the aerogel according to claim 1, It is characterized in that The following steps are involved: 1) dissolving aramid and alkali in a solvent, stirring evenly and removing excess alkali, standing to remove bubbles; washing the residual solvent, exchanging solvents, and freeze-drying to obtain aramid aerogel; 2) placing the aramid aerogel obtained in step 1) in a dopamine solution and mixing well, washing to remove the dopamine remaining on the surface, thereby obtaining an aramid / dopamine aerogel; 3) dissolving chitosan in acetic acid, adding an organic acid after the chitosan is dissolved, adding potassium persulfate after the chitosan is dissolved, and reflux heating to react to obtain chitosan / organic acid; 4) The aramid / dopamine aerogel obtained in step 2) is mixed with the chitosan / organic acid obtained in step 3), and the target aerogel is obtained by washing, solvent exchange, pre-freezing, and freeze-drying.
3. The method for preparing aerogel according to claim 2, It is characterized in that Step 1) is: cutting the long linear aramid yarn into small segments, weighing the yarn segments and KOH, adding them to DMSO, and magnetically stirring at room temperature for one week until it becomes a dark red aramid DMSO solution; centrifuging to remove excess KOH particles in the liquid, and then keeping it at room temperature for a certain period of time to remove bubbles; then transferring the aramid DMSO solution to deionized water to remove the solvent DMSO to obtain an ANFs solution; soaking the ANFs solution from which the residual solvent has been removed in a mixed solution of tert-butyl alcohol and water to perform solvent exchange, and finally transferring the ANFs solution after solvent exchange to a refrigerator for pre-freezing, and then obtaining the aramid aerogel through a freeze dryer.
4. The method for preparing the aerogel according to claim 2 or 3, It is characterized in that The aramid is para-aramid, the aramid is a small yarn segment with a length of 4-6 mm, the KOH is granular, the mass ratio of aramid to KOH is (0.3-0.8):1, and the mass ratio of aramid to DMSO is 0.5-1:100; the dissolving temperature is 20-25°C, the magnetic speed is 1000-2000rpm, and the solution is dissolved until it turns dark red.
5. The method for preparing the aerogel according to claim 2 or 3, It is characterized in that Excess alkali is removed by centrifugation at a speed of 1000-2000 rpm for 30-60 min; the bubbles are removed by standing for 4-6 h; and the residual solvent is removed by soaking in deionized water for 24-48 h, during which the deionized water is replaced by centrifugation every 6 h.
6. The method for preparing the aerogel according to claim 2 or 3, It is characterized in that In step 1), a mixed solution of tert-butanol and water is used for solvent exchange, the mass ratio of tert-butanol to water is 0.8-1.5:1, and the solvent exchange time is 24-48 hours; the refrigerator is pre-frozen at -18°C for 5-8 hours, and then freeze-dried at -55°C to -45°C in a freeze dryer for 12-24 hours to obtain the aramid aerogel.
7. The method for preparing aerogel according to claim 2, It is characterized in that In the step 2), the concentration of the dopamine solution is 2-8 mg / mL, the concentration of the aramid aerogel is 0.5-2 g / 100 ml, the pH is adjusted to 8.5, and the aramid aerogel and the dopamine solution are mixed by oscillation, the oscillation rate is 65-70 rpm, the oscillation temperature is 20-25° C., and the oscillation time is 24-48 h; the liquid for washing the aerogel is selected from ethanol or water or used alternately.
8. The method for preparing aerogel according to claim 2, It is characterized in that In the step 3), the volume concentration of acetic acid is 2%, chitosan g: acetic acid mL = 1: 2-5, and the chitosan is completely dissolved in 3-5 hours; the dissolved chitosan solution is transparent; chitosan g: organic acid mL / g = 3-5: 1; the organic acid used is selected from a mixture of one or more of oxalic acid, citric acid, tartaric acid, oxalic acid, malonic acid, lactic acid, and malic acid; the amount of potassium persulfate used is 0.05-0.1 mol per 100 ml of solution; the reflux temperature is 70-80° C., and the reflux time is 7-10 hours.
9. The method for preparing aerogel according to claim 2, It is characterized in that In the step 4), the weight ratio of aramid to chitosan is 10-15:1; the aramid / dopamine aerogel and chitosan / organic acid are mixed by shaking at a speed of 50-65 rpm for 24-48 hours.
10. The method for preparing aerogel according to claim 2, It is characterized in that In step 4), the solvent exchange is carried out using a mixed solution of tert-butanol and water, the mass ratio of tert-butanol to water is 0.8-1.5:1, and the solvent exchange time is 24-48 hours; the refrigerator is pre-frozen at -18°C for 5-10 hours, and then freeze-dried in a freeze dryer at -55°C to -45°C for 12-24 hours to obtain the target aerogel.