Layered double hydroxide composite chitosan modified magnetic carbon as well as preparation method and application thereof

Through the preparation of layered double hydroxide composite chitosan modified magnetic carbon, the problems of low removal efficiency and material stability of nanoscale microplastics are solved, and the effect of efficient adsorption and reusability in a wide pH range is achieved.

CN118904295APending Publication Date: 2024-11-08NINGBO INST OF TECH ZHEJIANG UNIV ZHEJIANG

Patent Information

Application Number
CN202410947940.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently remove nanoscale microplastics, the traditional adsorption method is inefficient, and the material's performance is unstable in different pH environments, and it is difficult to achieve reusable material.

Method used

Layered double hydroxide composite chitosan modified magnetic charcoal (LDHs-CTS@MBC) was prepared by peanut shell, sodium hydroxide, FeCl3·6H2O and ZnCl2 solutions and other raw materials, combined with high-temperature pyrolysis and co-precipitation method. Modified magnetic carbon with multiple adsorption mechanism was prepared, which can efficiently adsorb nanoscale microplastics over a wide pH range.

Benefits of technology

It has achieved efficient adsorption of nanoscale microplastics in the pH range of 5-11, with a maximum removal rate of 87.95%. The material is super paramagnetic, can be separated by magnets, and has good reusable properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904295A_ABST
    Figure CN118904295A_ABST
Patent Text Reader

Abstract

The invention discloses layered double hydroxide composite chitosan modified magnetic carbon as well as a preparation method and application thereof. The modified magnetic carbon is prepared from the following main raw materials: peanut shells, sodium hydroxide, FeCl3. 6H2O, chitosan, a ZnCl2 solution and an AlCl3 solution. The peanut shells are used for preparing magnetic biochar; the chitosan is used for modifying the magnetic charcoal, and the ZnCl2 solution and the AlCl3 solution are used for preparing the final modified magnetic charcoal; the magnetic carbon prepared by the scheme of the invention can effectively adsorb nano-scale micro-plastics, is relatively strong in reusability, and still keeps good adsorption capacity in a relatively wide pH environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of water treatment, and in particular to a layered double hydroxide composite chitosan modified magnetic carbon (LDHs-CTS@MBC, magnetic carbon), a preparation method and application thereof. Background Art

[0002] Plastics smaller than 5 mm are considered microplastics (MPs). S ), plastics smaller than 1μm are considered nanoplastics (NPs). Plastics have the characteristics of low production cost and wide application, so the global plastic production has increased dramatically, but problems also arise. When plastics enter the environment, they are decomposed into micro-nano plastics under the action of weathering, photooxidation, and biological decomposition. Micro-nano plastics continue to spread in the ecological environment, posing a serious threat to life. Due to the small particle size of micro-nano plastics, traditional adsorption removal methods have little effect. It is necessary to improve the traditional adsorption removal method to improve the adsorption removal efficiency of micro-nano plastics and improve the reusability of materials.

[0003] Biochar (BC) has great potential in the adsorption and removal of micro-nano plastics. The magnetic carbon material (MBC) improved on the basis of BC solves the problem that BC is difficult to separate from aqueous solution. On this basis, the modification of MBC can improve the adsorption performance of micro-nano plastics and shorten the corresponding separation time. In addition, the modification will also increase the adsorption mechanism of MBC, and the adsorption and removal efficiency of micro-nano plastics will also be greatly improved.

[0004] At present, the existing technology for treating micro-nano plastics with magnetic carbon materials is not common. Several application patents for treating microplastics with magnetic carbon materials are as follows: 1. The patent document with publication number CN 111117814A adopts a persulfate-based advanced oxidation technology, and uses magnetic carbon materials to activate persulfate, but it can only treat the organic layer on the surface of microplastics, and simultaneously remove the surface of microplastics and released pollutants, and separate the magnetic carbon material from the solution through an external magnetic field; the oxidation technology using persulfate in this document can only achieve the treatment of pollutants on the surface of microplastics, and although the diameter of microplastics that can be removed is <5mm, it is difficult to remove nanoscale (less than 1μm) microplastics, and the residual amount of microplastics is still large; 2. In the invention patent CN 115321657 B, a device for removing microplastics from polluted water bodies using the electrical properties of particles is used. The device uses the electrical properties of microplastic particles to set a metal mesh to achieve electric field enrichment of microplastic particles, and removes microplastic particles through a scum removal device to achieve sewage treatment. This patent uses physical methods to remove microplastics. The process of processing microplastics consumes a lot of electricity and the size of the removed microplastic particles is limited, which is not conducive to responding to national policies; 3. The patent document with publication number CN116196899A cultivates white rot fungi to form fungal balls, and uses the porous structure of the mycelium to adsorb microplastics. However, the fungal balls prepared in this document are significantly affected by the pH value of the water environment and are only suitable for water environments with pH = 3-7. They are easy to fall off after adsorption and the adsorption is not firm. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present application provides a layered double hydroxide composite chitosan modified magnetic carbon which can effectively adsorb nano-scale microplastics, has strong reusability, and maintains good adsorption capacity in a wide pH environment.

[0006] In order to solve the above technical problems, the technical solution adopted in this application is: a layered double hydroxide composite chitosan modified magnetic carbon (magnetic carbon), the main raw materials for the preparation of the modified magnetic carbon include: peanut shells, sodium hydroxide, FeCl 3 6H 2 O, chitosan, ZnCl 2 Solution, AlCl 3 solution; the peanut shell is used to prepare magnetic biochar; the chitosan is used to modify magnetic biochar, and the ZnCl 2 Solution and AlCl 3 The solution was used to prepare the final modified magnetic carbon (LDHs-CTS@MBC, layered double hydroxide composite chitosan modified magnetic carbon).

[0007] Furthermore, the specific preparation process of the magnetic biochar includes: calcining peanut shells at 400-600°C for 0.5-3h under the protection of nitrogen, and then sieving with a 50-200 mesh screen to obtain carbonized peanut shells; then adding the carbonized peanut shells and sodium hydroxide in a weight ratio of 3-5:1 into a reactor and adding deionized water to mix, and then stirring and reacting for 20-30h; balancing the solution after stirring and reacting to pH=7; then adding an equal volume of 1-1.2 mol / L FeCl 3 6H 2 O (the amount added here is related to magnetism. Generally speaking, the larger the addition, the greater the magnetism of the subsequent synthesized product. The equal volume here is FeCl 3 6H 2 The aqueous solution of O is added (the volume of the solution to be added is equivalent to the volume of the solution adjusted to pH=7 in the above stirring reaction), stirred for 20-40 minutes, and then vacuum dried. After drying, it is placed under nitrogen conditions and pyrolyzed at a temperature of 500-600° C. for 20-40 minutes to obtain magnetic biochar.

[0008] Furthermore, the preparation of the chitosan-modified magnetic biochar includes the following specific preparation processes: dissolving chitosan in an acetic acid solution with a mass concentration of 1-3%, adding the prepared magnetic biochar, wherein the mass ratio of chitosan to magnetic carbon is 1:4-6; then stirring at 30-50°C for 20-40 minutes, then adding a NaOH solution with a mass concentration of 1-3%, until the pH value is 8-9 and continuously stirring for 05-1.5 hours, and then washing until the solution is neutral; filtering, and drying the filtered solid in a vacuum oven to obtain chitosan-modified magnetic biochar.

[0009] Furthermore, the preparation process of the modified magnetic carbon comprises: ZnCl 2 Solution with AlCl 3 The solution was added to the reaction vessel and mixed, wherein ZnCl 2 With AlCl 3 The molar concentration ratio is 1-3:1; then chitosan modified magnetic biochar is added, stirred evenly, sodium hydroxide solution is added to adjust the pH, the reaction is stopped when the pH of the solution is 9.5-10.5, and then the solution is centrifuged to obtain a mixture that is washed to neutrality and dried to obtain modified magnetic carbon.

[0010] Furthermore, the present application also provides a method for preparing layered double hydroxide composite chitosan modified magnetic carbon, the specific preparation steps of the method comprising:

[0011] (1) Preparation of magnetic biochar: Peanut shells were calcined at 400-600°C for 0.5-3 h under nitrogen protection, and then sieved with a 50-200 mesh screen to obtain carbonized peanut shells; the carbonized peanut shells and sodium hydroxide were added to a reactor at a weight ratio of 3-5:1 and deionized water was added to mix, and the mixture was stirred for 20-30 h; the stirred solution was balanced to pH = 7; then, FeCl was added to the aqueous solution. 3 6H 2 O, stirring for 20-40 minutes, then vacuum drying, and after drying, pyrolyzing at 500-600°C for 20-40 minutes under nitrogen conditions to obtain magnetic biochar;

[0012] (2) Preparation of chitosan-modified magnetic biochar: dissolve chitosan in an acetic acid solution with a mass concentration of 1-3%, add the prepared magnetic biochar, wherein the mass ratio of chitosan to magnetic carbon is 1:4-6; then stir at 30-50°C for 20-40 minutes, then add a NaOH solution with a mass concentration of 1-3% until the pH is 8-9 and continue stirring for 05-1.5 hours, then wash until the solution is neutral; filter, and put the filtered solid into a vacuum oven for drying to obtain chitosan-modified magnetic biochar;

[0013] (3) Preparation of modified magnetic carbon: ZnCl 2 Solution with AlCl 3 The solution was added to the reaction vessel and mixed, wherein ZnCl 2 With AlCl 3 The molar concentration ratio is 1-3:1; then chitosan modified magnetic biochar is added, stirred evenly, sodium hydroxide solution is added to adjust the pH, the reaction is stopped when the pH of the solution is 9.5-10.5, and then the solution is centrifuged to obtain a mixture that is washed to neutrality and dried to obtain modified magnetic carbon.

[0014] Furthermore, the vacuum drying mentioned above in the present application specifically involves placing the material in a vacuum oven and drying it at 75-85° C. for 10-15 hours.

[0015] The present application also provides an application of the layered double hydroxide composite chitosan modified magnetic carbon prepared as above, specifically, it is used for the adsorption and separation of micro-nano plastics in water environment.

[0016] Furthermore, the micro-nano plastic is polystyrene (PS-NPs, polystyrene nanoplastic).

[0017] Furthermore, the pH of the adsorption water environment is 5-11.

[0018] Furthermore, the optimal reaction conditions of the adsorption water environment are: layered double hydroxide composite chitosan modified magnetic carbon (LDHs-CTS@MBC) dosage 30 mg, polystyrene (PS-NPs) initial concentration 200 mg / L, pH = 11, oscillation intensity 150 rpm, NaCl concentration in the solution 0 mM; the adsorption process conforms to the Langmuir adsorption isotherm, and the maximum saturated adsorption capacity can reach 309.09 mg / g.

[0019] Furthermore, after the layered double hydroxide composite chitosan modified magnetic carbon is used to adsorb micro-nano plastics, it is subjected to ultrasonic oscillation by an ultrasonic cleaner to remove PS-NPs adsorbed in the pores of the layered double hydroxide composite chitosan modified magnetic carbon (LDHs-CTS@MBC).

[0020] Advantages and beneficial effects of this application:

[0021] 1. This application uses peanut shells as raw materials for the first time to prepare a layered double hydroxide composite chitosan modified magnetic carbon (LDHs-CTS@MBC). The adsorption mechanism of LDHs-CTS@MBC on PS-NPs involves multiple interactions. LDHs-CTS@MBC first aggregates PS-NPs in the aqueous solution through aggregation, and then adsorbs PS-NPs in the aqueous solution through electrostatic interactions and van der Waals forces, thereby achieving the adsorption of nano-scale microplastic particles.

[0022] 2. The layered double hydroxide composite chitosan modified magnetic carbon (magnetic carbon) of the present application can have good adsorption in a water environment of pH = 5-11. This is because the removal rate of LDHs-CTS@MBC is greatly affected by the pH of the solution, and the pH of the solution has a great influence on the surface charge and oxygen-containing functional groups of the LDHs-CTS@MBC material; under strong acid conditions, the removal rate of LDHs-CTS@MBC is the lowest, only 50.4%, and at this time, the solution turns light yellow after oscillation under strong acid conditions. This may be because the strong acid conditions destroy the molecular structure of LDHs-CTS@MBC, and the chitosan in the material dissolves and precipitates, causing the solution to change color. Under pH = 5-11 conditions, the removal rate of PS-NPs by LDHs-CTS@MBC is improved, especially when pH = 11, the removal rate of PS-NPs by LDHs-CTS@MBC is the highest, reaching 87.95%. This is because under strong alkaline conditions, the amino groups on the surface of LDHs-CTS@MBC have higher reactivity and the electrostatic interaction of LDHs-CTS@MBC is the strongest, which can better remove PS-NPs in the solution.

[0023] 3. The layered double hydroxide composite chitosan modified magnetic carbon of the present application has an irregular surface of ZnAl layered double hydroxide, chitosan existing on the surface of the carbon material and rough Fe3O4 particles. Chitosan and Fe3O4 particles are agglomerated on the surface of the carbon material. The layered double hydroxide has a unique flaky aggregation with a smooth surface, which makes the surface of the composite structure full of dense pores and can provide a large number of adsorption sites for PS-NPs.

[0024] 4. PS-NPs are aggregated and adsorbed in the pores and surface of the material by LDHs-CTS@MBC. The PS-NPs are spherical in shape and of different sizes. Therefore, PS-NPs may first aggregate in the solution and then be adsorbed in the pores and surface by LDHs-CTS@MBC. This shows that LDHs-CTS@MBC has a good adsorption and aggregation effect on PS-NPs, which also proves the successful synthesis of LDHs-CTS@MBC.

[0025] 5. The layered double hydroxide composite chitosan modified magnetic carbon of the present application has superparamagnetism, and the adsorbed PS-NPs can be separated from the solution by a magnet; the present application provides an efficient and reusable method for the removal of micro-nano plastics in aquatic environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 .Comparison chart of the effects of NPS-Ps before and after adsorption of this application.

[0027] Figure 2 . Experimental diagram of the conditions for the removal of micro-nano plastics by magnetic carbon materials in this application, including the effect of the initial concentration of PS-NPs on the removal rate (a); the effect of the dosage of LDHs-CTS@MBC on the removal rate (b); the effect of solution pH on the removal rate (c); the effect of oscillation intensity on the removal rate (d); Cl - Effect of concentration on removal efficiency (e).

[0028] Figure 3 .SEM of LDHs-CTS@MBC prepared in this application.

[0029] Figure 4 .SEM image of LDHs-CTS@MBC prepared in this application after adsorbing PS-NPs. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments and drawings to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only preferred embodiments, not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] (1) Preparation of magnetic biochar: Peanut shells were calcined in a muffle furnace at 500 °C for 1 h under nitrogen protection, and carbonized peanut shells were sieved with a 100-mesh sieve. The carbonized peanut shells were then mixed with sodium hydroxide in a beaker at a weight ratio of 4:1 and deionized water was added. The mixture was stirred for 24 h using a magnetic stirrer, and the solution was balanced to pH 7. Subsequently, an equal volume of 1.1 mol / L FeCl 3 6H 2 O aqueous solution, stirred with a glass rod for 30 minutes, then placed the beaker in a vacuum oven and dried at 80 °C for 12 hours, and the obtained solid was pyrolyzed at 550 °C for 30 minutes under nitrogen to obtain magnetic biochar.

[0033] (2) Preparation of chitosan-modified magnetic biochar: chitosan was dissolved in a 2% acetic acid solution in a beaker, wherein the mass ratio of chitosan to magnetic biochar was 1:5; the prepared magnetic biochar was added to the mixture, stirred at 40°C for 30 min, and then a 3% NaOH solution was added until the pH value was 9 and stirred for 1 h. The obtained precipitate was washed with distilled water until the solution was neutral; the precipitate was filtered with a funnel and a glass rod, and the filtered solid was placed in a vacuum oven and dried at 80°C for 12 h;

[0034] (3) Preparation of LDHs-CTS@MBC: ZnCl 2 The solution and AlCl3 solution were added into a beaker and mixed together, wherein ZnCl 2 With AlCl 3 The molar concentration ratio was 2:1, and it was stirred with a glass rod for 15 minutes; then chitosan-modified magnetic biochar was added, stirred evenly with a glass rod, and sodium hydroxide solution was added to adjust the pH. The reaction was stopped when the pH of the solution was 10. The solution was then centrifuged for 10 minutes, and the obtained mixed solution was washed with deionized water until neutral, and placed in a vacuum oven and dried at 80°C for 12 hours to obtain LDHs-CTS@MBC.

[0035] The LDHs-CTS@MBC modified magnetic carbon material prepared in Example 1 was used to adsorb PS-NPs: temperature 25°C, NaCl 5mM; 200mg / L PS-NPs, solution pH set to 11, the amount of modified magnetic carbon material added was 30mg / L, oscillation at 150rpm for 30min, sampling and testing after adsorption equilibrium, and the PS-NPs concentration in the solution was measured using a fluorescence spectrophotometer, and the removal rate of PS-NPs was 88.17%.

[0036] The dosage of LDHs-CTS@MBC was 30 mg, the initial concentration of PS-NPs was 200 mg / L, pH = 11, the oscillation intensity was 150 rpm, and the NaCl concentration in the solution was 0 mM; the adsorption process conformed to the Langmuir adsorption isotherm, and the maximum saturated adsorption capacity could reach 309.09 mg / g.

[0037] Figure 1 As shown, it is a comparison diagram of the effect before and after the LDHs-CTS@MBC modified magnetic carbon material prepared in Example 1 is used to adsorb PS-NPs (before adsorption on the left, after adsorption on the right). It can be seen from the figure that the left picture does not add the adsorption material, and the solution is relatively turbid. The right picture shows the effect after adding the adsorption material. The solution is relatively clear and a good adsorption effect is achieved.

[0038] Figure 2 As shown, it is the experimental diagram of the conditions for the magnetic carbon material to adsorb and remove micro-nano plastics in this embodiment, the effect of the initial concentration of PS-NPs on the removal rate (a); the effect of the dosage of LDHs-CTS@MBC on the removal rate (b); the effect of solution pH on the removal rate (c); the effect of oscillation intensity on the removal rate (d); the effect of Cl- concentration on the removal rate (e);

[0039] Among them, the removal rate of LDHs-CTS@MBC is greatly affected by the pH of the solution, and the pH of the solution has a great influence on the surface charge and oxygen-containing functional groups of the LDHs-CTS@MBC material. Under strong acid conditions, the removal rate of LDHs-CTS@MBC is the lowest, only 50.4%. At this time, the solution turns light yellow after oscillation under strong acid conditions. This may be because the strong acid conditions destroy the molecular structure of LDHs-CTS@MBC, and the chitosan in the material is dissolved and precipitated, causing the solution to change color. Under pH = 5-11 conditions, the removal rate of PS-NPs by LDHs-CTS@MBC is improved, especially at pH = 11, the removal rate of PS-NPs by LDHs-CTS@MBC is the largest, reaching 87.95%. This is because under strong alkaline conditions, the amino groups on the surface of LDHs-CTS@MBC have high reactivity, and the electrostatic interaction of LDHs-CTS@MBC is the strongest, which can better remove PS-NPs in the solution.

[0040] In addition, temperature has a great influence on the adsorption of PS-NPs by LDHs-CTS@MBC. With the increase of temperature, the adsorption amount of LDHs-CTS@MBC increases to a certain extent. The increase in temperature is beneficial to the removal of PS-NPs in aqueous solution (the maximum adsorption amount of PS-NPs by LDHs-CTS@MBC obtained through adsorption isotherm experiments is 309.09 mg / g (25℃), 311.82 mg / g (35℃), and 320.79 mg / g (45℃)).

[0041] Figure 3 This is the SEM (scanning electron microscope) of the LDHs-CTS@MBC prepared in this example. The SEM image of LDHs-CTS@MBC shows the irregular surface of the composite ZnAl layered double hydroxide; the red frame in the figure indicates the chitosan on the surface of the carbon material and the rough Fe 3 O 4 Particles, chitosan and Fe 3 O 4 The particles agglomerated on the surface of the carbon material; the blue frame in the figure represents the unique lamellar aggregation of the layered double hydroxide with a smooth surface; indicating that the surface of the composite structure prepared in this application has dense pores, which can provide a large number of adsorption sites for PS-NPs.

[0042] Figure 4 .This is the SEM image of the LDHs-CTS@MBC prepared in this example after adsorbing PS-NPs. It can be seen from the figure that the PS-NPs are aggregated and adsorbed by the LDHs-CTS@MBC in the pores and on the surface of the material. The PS-NPs are spherical in shape and of different sizes. Therefore, the PS-NPs may first aggregate in the solution and then be adsorbed in the pores and on the surface by the LDHs-CTS@MBC, indicating that LDHs-CTS@MBC has a good adsorption and aggregation effect on PS-NPs, which also proves the successful synthesis of LDHs-CTS@MBC.

[0043] Example 2

[0044] (1) Preparation of magnetic biochar: Peanut shells were calcined in a muffle furnace at 550 °C for 0.8 h under nitrogen protection and sieved with a 150-mesh sieve to obtain carbonized peanut shells. The carbonized peanut shells were then mixed with sodium hydroxide in a beaker at a weight ratio of 3.5:1 and deionized water was added. The mixture was stirred for 24 h using a magnetic stirrer and the solution was balanced to pH 7. Subsequently, an equal volume of 1.0 mol / L FeCl 3 6H 2O aqueous solution, stirred with a glass rod for 35 minutes, then placed the beaker in a vacuum oven and dried at 80 °C for 12 hours, and the obtained solid was pyrolyzed at 550 °C for 30 minutes under nitrogen to obtain magnetic biochar.

[0045] (2) Preparation of chitosan-modified magnetic biochar: chitosan was dissolved in a 2.5% acetic acid solution in a beaker, wherein the mass ratio of chitosan to magnetic biochar was 1:4.5; the prepared magnetic biochar was added to the mixture, stirred at 45°C for 28 min, and then a 3.5% NaOH solution was added until the pH value was 9 and stirred for 1 h. The precipitate was washed with distilled water until the solution was neutral; the precipitate was filtered with a funnel and a glass rod, and the filtered solid was placed in a vacuum oven and dried at 80°C for 12 h;

[0046] (3) Preparation of LDHs-CTS@MBC: ZnCl 2 Solution with AlCl 3 The solution was added to the beaker and mixed together, where ZnCl 2 With AlCl 3 The molar concentration ratio is 2.5:1, and it is stirred with a glass rod for 20 minutes; then chitosan-modified magnetic biochar is added, stirred evenly with a glass rod, and sodium hydroxide solution is added to adjust the pH. The reaction is stopped when the pH of the solution is 10. The solution is then centrifuged for 10 minutes, and the obtained mixed solution is washed with deionized water until neutral, and placed in a vacuum oven and dried at 80°C for 12 hours to obtain LDHs-CTS@MBC.

[0047] The LDHs-CTS@MBC modified magnetic carbon material prepared in Example 2 was used to adsorb PS-NPs: temperature 25°C, NaCl was 5mM, PS-NPs was 200mg / L, the solution pH was set to 11, the amount of modified magnetic carbon material added was 30mg / L, and it was oscillated at 150rpm for 30min. After adsorption equilibrium, sampling was performed and the PS-NPs concentration in the solution was measured using a fluorescence spectrophotometer. The removal rate of PS-NPs was 83.35%.

[0048] It can be seen from the above examples that layered double hydroxide composite chitosan modified magnetic carbon LDHs-CTS@MBC was prepared by high temperature pyrolysis and coprecipitation using peanut shell powder as raw material. LDHs-CTS@MBC has better adsorption effect on polystyrene (PS-NPs) under most conditions, and the adsorption effect is better under strong alkaline conditions; the optimal reaction conditions are: LDHs-CTS@MBC dosage 30mg, PS-NPs initial concentration 200mg / L, pH=11, oscillation intensity 150rpm, NaCl concentration in solution 0mM; the adsorption process conforms to the Langmuir adsorption isotherm, and the maximum saturated adsorption capacity can reach 309.09mg / g. The material has superparamagnetism, and the adsorbed PS-NPs can be separated from the solution by a magnet. The present application provides an efficient and reusable method for the removal of micro-nano plastics in water environments.

Claims

1. A layered double hydroxide composite chitosan modified magnetic carbon, characterized in that: The main raw materials for preparing the modified magnetic carbon include: peanut shell, sodium hydroxide, FeCl3·6H2O, chitosan, ZnCl2 solution and AlCl3 solution; the peanut shell is used to prepare the magnetic biochar; the chitosan is used to modify the magnetic biochar, and the ZnCl2 solution and AlCl3 solution are used to prepare the final modified magnetic carbon.

2. The layered double hydroxide composite chitosan modified magnetic carbon according to claim 1, characterized in that: The specific preparation process of the magnetic biochar comprises: calcining peanut shells at 400-600°C for 0.5-3h under the protection of nitrogen, and then sieving with a 50-200 mesh screen to obtain carbonized peanut shells; then adding the carbonized peanut shells and sodium hydroxide into a reactor at a weight ratio of 3-5:1 and adding deionized water to mix, and then stirring for 20-30h; balancing the solution after the stirring reaction to pH=7; then, adding an equal volume of 1-1.2mol / L FeCl3·6H2O aqueous solution to the solution, stirring for 20-40min, and then vacuum drying, and after drying, pyrolyzing at 500-600°C for 20-40min under nitrogen conditions to obtain magnetic biochar.

3. The layered double hydroxide composite chitosan modified magnetic carbon according to claim 1, characterized in that: The preparation of the chitosan modified magnetic biochar includes: dissolving chitosan in an acetic acid solution with a mass concentration of 1-3%, adding the prepared magnetic biochar, wherein the mass ratio of chitosan to magnetic carbon is 1:4-6; stirring at 30-50°C for 20-40 minutes, then adding a NaOH solution with a mass concentration of 1-3% until the pH is 8-9 and continuously stirring for 05-1.5 hours, and then washing until the solution is neutral; filtering, and placing the filtered solid into a vacuum oven for drying to obtain the chitosan modified magnetic biochar.

4. The layered double hydroxide composite chitosan modified magnetic carbon according to claim 1, characterized in that: The preparation process of the final modified magnetic carbon includes: adding ZnCl2 solution and AlCl3 solution into a reaction container and mixing, wherein the molar concentration ratio of ZnCl2 to AlCl3 is 1-3:1; then adding chitosan modified magnetic biochar, stirring evenly, adding sodium hydroxide solution to adjust the pH, stopping the reaction when the pH of the solution is 9.5-10.5, then washing the mixture obtained by centrifuging the solution to neutrality, and drying to obtain modified magnetic carbon.

5. A method for preparing the layered double hydroxide composite chitosan modified magnetic carbon according to any one of claims 1 to 4, characterized in that: The specific preparation steps of the method include: (1) Preparation of magnetic biochar: Peanut shells were calcined at 400-600°C for 0.5-3h under nitrogen protection, and then sieved with a 50-200 mesh screen to obtain carbonized peanut shells; the carbonized peanut shells and sodium hydroxide were added to a reactor at a weight ratio of 3-5:1 and deionized water was added and mixed, and the mixture was stirred for 20-30h; the stirred solution was balanced to pH = 7; then, FeCl3·6H2O was added to the aqueous solution, stirred for 20-40min, and then vacuum dried. After drying, the mixture was pyrolyzed at 500-600°C for 20-40min under nitrogen conditions to obtain magnetic biochar; (2) Preparation of chitosan-modified magnetic biochar: dissolve chitosan in an acetic acid solution with a mass concentration of 1-3%, add the prepared magnetic biochar, wherein the mass ratio of chitosan to magnetic carbon is 1:4-6; then stir at 30-50°C for 20-40 minutes, then add a NaOH solution with a mass concentration of 1-3% until the pH is 8-9 and continue stirring for 05-1.5 hours, then wash until the solution is neutral; filter, and put the filtered solid into a vacuum oven for drying to obtain chitosan-modified magnetic biochar; (3) Preparation of the final modified magnetic carbon: ZnCl2 solution and AlCl3 solution are added to a reaction container and mixed, wherein the molar concentration ratio of ZnCl2 to AlCl3 is 1-3:1; then chitosan-modified magnetic biochar is added and stirred evenly, and sodium hydroxide solution is added to adjust the pH. The reaction is stopped when the pH of the solution is 9.5-10.5, and the solution is then centrifuged to obtain a mixture that is washed to neutrality and dried to obtain modified magnetic carbon.

6. The method for preparing layered double hydroxide composite chitosan modified magnetic carbon according to claim 5, characterized in that: The vacuum drying specifically involves placing the material in a vacuum oven and drying it at 75-85° C. for 10-15 hours.

7. An application of the layered double hydroxide composite chitosan modified magnetic carbon according to any one of claims 1 to 4, characterized in that: Specifically, it is used for the adsorption and separation of micro-nano plastics in water environments.

8. The use of layered double hydroxide composite chitosan modified magnetic carbon according to claim 7, characterized in that: The micro-nano plastic is polystyrene; the pH of the adsorption water environment is 5-11.

9. The use of layered double hydroxide composite chitosan modified magnetic carbon according to claim 8, characterized in that: The optimal reaction conditions of the adsorption water environment are: the addition amount of layered double hydroxide composite chitosan modified magnetic carbon is 30 mg, the initial concentration of polystyrene is 200 mg / L, pH=11, the oscillation intensity is 150 rpm, and the NaCl concentration in the solution is 0 mM; the adsorption process conforms to the Langmuir adsorption isotherm, and the maximum saturated adsorption capacity can reach 309.09 mg / g.

10. The use of layered double hydroxide composite chitosan modified magnetic carbon according to claim 8, characterized in that: After the layered double hydroxide composite chitosan modified magnetic carbon is used to adsorb micro-nano plastics, it is subjected to ultrasonic oscillation by an ultrasonic cleaning instrument, so as to remove polystyrene adsorbed in the pores of the layered double hydroxide composite chitosan modified magnetic carbon.

Citation Information

Patent Citations

  • Preparation method of layered double hydroxide-loaded biochar composite material

    CN108837803A

  • Preparation method and application of modified biochar composite modified with magnetic hydrotalcite

    CN109499542A

  • Preparation method and application method of chitosan combined magnetic modified biochar material

    CN109529767A

  • Double-metal hydroxide flocculating agent and nano-plastic-containing wastewater treatment method

    CN112551747A

  • Preparation method and application of LDH modified biomass charcoal material

    CN114307944A

Cited By

  • Device and method for efficiently recycling sewage micro-plastics through cooperation of magnetic porous material and ultrasonic method

    CN120717555A