Preparation method of nano mineral activated carbon

By modifying zircon and beech wood biochar, combining sodium alginate and bismuth salts, nanomineral activated carbon is formed, which solves the problem of poor adsorption effect of traditional biochar on stubborn pollutants, and achieves lead, cadmium and industrial Efficient removal of dyes and improved stability.

CN118904312AInactive Publication Date: 2024-11-08JIUJIANG TIANZE CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197413.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional biochar has poor adsorption effect on stubborn pollutants, and has poor removal of harmful substances such as lead, cadmium, and color, and has poor strength.

Method used

By modifying zircon and beech wood biochar, combining sodium alginate and bismuth salt, ultrasonic treatment and ball milling technology, nanomineral activated carbon is formed to enhance its adsorption capacity and mechanical properties.

Benefits of technology

It significantly improves the adsorption and fixation ability of nanomineral activated carbon to heavy metal ions, enhances the removal effect of pollutants, including the removal ability of industrial dyes and heavy metals, and improves the stability and use time limit of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a preparation method of nano mineral activated carbon, which belongs to the technical field of nano materials, and comprises the following steps: modifying baddeleyite by using sodium alginate; preparing bismuth modified beech biochar; and loading the modified baddeleyite on the bismuth-modified beech biochar, so as to prepare the nano mineral activated carbon. The preparation method comprises the following steps: respectively modifying beech stone and beech charcoal, grinding the beech stone, sodium alginate and a dispersing agent, performing ultrasonic treatment, and sintering, so that a large number of fine pores are formed in the surface of the stone, and the stone has good mechanical properties; the bismuth salt is used for modifying the biochar, so that pore blockage and micropore collapse of the biochar are prevented, and the porosity and the adsorption capacity are improved; and through a ball milling technology, the mesopores and macropores of the nano mineral activated carbon material are enhanced through decomposition of the biochar and extrusion of the bismuth salt, so that the pollutant treatment effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano materials, and in particular, relates to a method for preparing nano mineral activated carbon. Background Art

[0002] Human exposure to cadmium, lead, and arsenic through water circulation and consumption of contaminated food can cause serious health problems in the skin, lungs, kidneys, and brain. In addition, there is organic pollution such as industrial dyes. Since the pollutants are difficult to degrade and stubborn to the physical and chemical properties of the surrounding environment, they are difficult to remove with adsorption scavengers.

[0003] In the work of providing a clean environment for humans, nanomaterials are a good pollution adsorbent. Their high reactivity has become an emerging technology for cleaning soil and water pollutants. Activated carbon is a commonly used carrier for removing pollutants to improve removal efficiency. However, ordinary activated carbon has poor adsorption effect on stubborn pollutants, and has poor removal effect and strength on harmful substances such as lead, cadmium, and color. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing nano mineral activated carbon, by modifying sphene and beech wood biochar respectively, grinding the sphene with sodium alginate and a dispersant, performing ultrasonic treatment, and then sintering, so as to form a large number of fine pores on the surface of the stone with good mechanical properties; using bismuth salt to modify the biochar to prevent pore blockage and micropore collapse of the biochar, increase porosity and adsorption capacity; and then through ball milling technology, the decomposition of the biochar and the extrusion of the bismuth salt enhance the mesopores and macropores of the nano mineral activated carbon material, so that the effect of treating pollutants is improved.

[0005] The technical problem to be solved by the present invention is as follows: The present invention solves the problem that the traditional biochar adsorbent has poor adsorption effect on stubborn pollutants, poor removal effect on harmful substances such as lead, cadmium, and chromaticity, and poor strength.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A method for preparing nano mineral activated carbon comprises the following steps:

[0008] (1) Modification of baddeleyite using sodium alginate;

[0009] The baddeleyite concentrate is washed with deionized water, calcium oxide powder is added, ground for 60 minutes at 40°C and then dried; the mixed powder of baddeleyite and calcium oxide is mixed with sodium alginate, Dol apix-CE-64 dispersant and deionized water, and ultrasonic dispersion is performed at 20kHz in a mode of ultrasonic treatment for 10 seconds and then paused for 50 seconds. After circulating for 20 minutes, the solution is degassed in a vacuum furnace at 25°C and 0.2 bar for 1-2 minutes, and then added dropwise to a 2% calcium chloride suspension, filtered after standing for 10 minutes, washed with distilled water and dried at room temperature for 24 hours, and sintered in a muffle furnace at an air atmosphere of 1000-1300°C at a heating rate of 5°C / min for 1 hour to obtain modified baddeleyite.

[0010] (2) Preparation of bismuth-modified beech wood biochar;

[0011] The beech wood raw material was heated at 500°C at a rate of 5°C / min and carbonized for 5 hours to prepare biochar, which was passed through a 30-mesh sieve for later use; bismuth nitrate pentahydrate was dissolved in 1 mol / L nitric acid solution, diluted with deionized water, and the beech wood biochar was mixed with 5 mmol / L bismuth nitrate pentahydrate and ultrasonically dispersed for 60 minutes, then vigorously stirred at 25°C for 4 hours, and then rinsed with deionized water until the pH value was neutral, and then dried at 105°C to obtain bismuth-modified beech wood biochar.

[0012] (3) Bismuth-modified beech wood biochar was loaded with modified baddeleyite to prepare nano-mineral activated carbon.

[0013] The bismuth-modified beech wood biochar was ground at room temperature, passed through a 100-mesh sieve, mixed with modified baddeleyite, transferred to a ball mill and worked at a rotation speed of 400 rpm for 12 hours, with the rotation direction changed every 1 hour, to obtain nano mineral activated carbon.

[0014] Furthermore, the mass ratio of the mixed powder of baddeleyite and calcium oxide, sodium alginate and Dol apix-CE-64 dispersant is 1:1.5-2:0.05-0.09.

[0015] Furthermore, the mass ratio of bismuth-modified beech wood biochar to modified baddeleyite is 1:2-3.

[0016] Beneficial effects of the present invention:

[0017] (1) In the technical solution of the present invention, the adsorption of pollutants by biochar is enhanced by modifying baddeleyite ore. Baddeleyite concentrate contains more than 95% free zirconium oxide, and also contains SiO2, Al2O3, Fe2O3, TiO2 and other substances. The combination with biochar can reduce the fluid resistance of inorganic nanoparticles, make the particles uniform, enhance chemical stability, and increase the adsorption and fixation capacity of nano-mineral activated carbon for heavy metal ions. In addition, baddeleyite is ground with sodium alginate and a dispersant, ultrasonically treated, and then sintered to form a large number of fine pores on the surface of the stone, which enhances the adsorption capacity and also makes the material have good mechanical properties, increasing the service life of the material.

[0018] (2) In the technical solution of the present invention, beech wood is used as raw material to prepare biochar. Beech wood is a kind of wood used for furniture. However, beech wood over a certain age will have uneven color, cracks and deformation in the wood body, resulting in huge losses. However, beech wood has a uniform texture and many pores. The biochar prepared is environmentally friendly and has strong adsorption capacity compared to other materials. It can be used as a soil additive to improve the fertility and water retention of the soil. Its organic properties and high specific surface area also enhance the soil properties.

[0019] (3) In the technical solution of the present invention, bismuth salt is used to modify biochar, so that the biochar has higher ion exchange capacity, higher porosity and abundant surface groups. The bismuth salt material is low in cost and easy to synthesize. The presence of biochar can also avoid condensation between bismuth salts, provide more pore space for bismuth metal salts, provide more adsorption sites, promote surface complexation, ion exchange and electrostatic attraction processes, so as to increase the adsorption effect on pollutants.

[0020] (4) In the technical scheme of the present invention, the nano-mineral activated carbon prepared by modified beech wood biochar loaded with modified baddeleyite can achieve good removal and fixation effects on colored pollutants such as lead, cadmium and industrial dyes in the soil through chemical adsorption methods such as surface exchange and ion complexation, and can effectively promote the stable transformation of heavy metals in water and soil. The baddeleyite surface carries abundant hydroxyl groups that can coordinate with heavy metal ions, and the good mechanical properties exhibited by the material after modification make it have good corrosion resistance and good stability. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] A method for preparing nano mineral activated carbon comprises the following steps:

[0024] (1) Modification of baddeleyite using sodium alginate;

[0025] 9.8 g of baddeleyite concentrate was washed with deionized water, and 0.2 g of calcium oxide powder was added, ground at 40° C. for 60 minutes, and then dried; the mixed powder of baddeleyite and calcium oxide was mixed with 15 g of sodium alginate, 0.005 g of Dol apix-CE-64 dispersant, and 10 mL of deionized water, and ultrasonically dispersed at 20 kHz in a mode of ultrasonic treatment for 10 seconds and then paused for 50 seconds. After circulating for 20 minutes, the solution was degassed in a vacuum furnace at 25° C. and 0.2 bar for 2 minutes, and then added dropwise to 50 mL of 2% calcium chloride suspension, allowed to stand for 10 minutes, filtered, washed with distilled water, dried at room temperature for 24 hours, and sintered in a muffle furnace at 1000° C. in an air atmosphere at a heating rate of 5° C. / min for 1 hour to obtain modified baddeleyite.

[0026] (2) Preparation of bismuth-modified beech wood biochar;

[0027] 20 g of beech wood raw material was heated at 500 ° C at a rate of 5 ° C / min and carbonized for 5 hours to prepare biochar, which was passed through a 30-mesh sieve for later use; 2.32 g of bismuth nitrate pentahydrate was dissolved in 1 mol / L nitric acid solution, diluted with 20 mL of deionized water, 1.0 g of beech wood biochar was mixed with 100 mL of 5mmol / L bismuth nitrate pentahydrate, and ultrasonically dispersed for 60 minutes, and then vigorously stirred at 25 ° C for 4 hours, then rinsed with deionized water until the pH value was neutral, and then dried at 105 ° C to obtain bismuth-modified beech wood biochar.

[0028] (3) Bismuth-modified beech wood biochar was loaded with modified baddeleyite to prepare nano-mineral activated carbon.

[0029] 5.0 g of bismuth-modified beech wood biochar was ground at room temperature, passed through a 100-mesh sieve, mixed with 10.0 g of modified baddeleyite, transferred to a ball mill and worked at a rotation speed of 400 rpm for 12 hours, with the rotation direction changed every 1 hour, to obtain nano mineral activated carbon.

[0030] Example 2

[0031] A method for preparing nano mineral activated carbon comprises the following steps:

[0032] (1) Modification of baddeleyite using sodium alginate;

[0033] 9.8 g of baddeleyite concentrate was washed with deionized water, and 0.2 g of calcium oxide powder was added, ground at 40° C. for 60 minutes, and then dried; the mixed powder of baddeleyite and calcium oxide was mixed with 17.5 g of sodium alginate, 0.007 g of Dol apix-CE-64 dispersant, and 10 mL of deionized water, and ultrasonically dispersed at 20 kHz in a mode of ultrasonic treatment for 10 seconds and then paused for 50 seconds. After circulating for 20 minutes, the solution was degassed in a vacuum furnace at 25° C. and 0.2 bar for 2 minutes, and then added dropwise to 50 mL of 2% calcium chloride suspension, allowed to stand for 10 minutes, filtered, washed with distilled water, dried at room temperature for 24 hours, and sintered in a muffle furnace at 1200° C. in an air atmosphere at a heating rate of 5° C. / min for 1 hour to obtain modified baddeleyite.

[0034] (2) Preparation of bismuth-modified beech wood biochar;

[0035] 20 g of beech wood raw material was heated at 500 ° C at a rate of 5 ° C / min and carbonized for 5 hours to prepare biochar, which was passed through a 30-mesh sieve for later use; 2.32 g of bismuth nitrate pentahydrate was dissolved in 1 mol / L nitric acid solution, diluted with 20 mL of deionized water, 1.0 g of beech wood biochar was mixed with 100 mL of 5mmol / L bismuth nitrate pentahydrate, and ultrasonically dispersed for 60 minutes, and then vigorously stirred at 25 ° C for 4 hours, then rinsed with deionized water until the pH value was neutral, and then dried at 105 ° C to obtain bismuth-modified beech wood biochar.

[0036] (3) Bismuth-modified beech wood biochar was loaded with modified baddeleyite to prepare nano-mineral activated carbon.

[0037] 5.0 g of bismuth-modified beech wood biochar was ground at room temperature, passed through a 100-mesh sieve, mixed with 12.5 g of modified baddeleyite, transferred to a ball mill and worked at a rotation speed of 400 rpm for 12 hours, with the rotation direction changed every 1 hour, to obtain nano mineral activated carbon.

[0038] Example 3

[0039] A method for preparing nano mineral activated carbon comprises the following steps:

[0040] (1) Modification of baddeleyite using sodium alginate;

[0041] 9.8 g of baddeleyite concentrate was washed with deionized water, and 0.2 g of calcium oxide powder was added, ground at 40° C. for 60 minutes, and then dried; the mixed powder of baddeleyite and calcium oxide was mixed with 20 g of sodium alginate, 0.009 g of Dol apix-CE-64 dispersant, and 10 mL of deionized water, and ultrasonically dispersed at 20 kHz in a mode of ultrasonic treatment for 10 seconds and then paused for 50 seconds. After circulating for 20 minutes, the solution was degassed in a vacuum furnace at 25° C. and 0.2 bar for 2 minutes, and then added dropwise to 50 mL of 2% calcium chloride suspension, allowed to stand for 10 minutes, filtered, washed with distilled water, dried at room temperature for 24 hours, and sintered in a muffle furnace at 1300° C. in an air atmosphere at a heating rate of 5° C. / min for 1 hour to obtain modified baddeleyite.

[0042] (2) Preparation of bismuth-modified beech wood biochar;

[0043] 20 g of beech wood raw material was heated at 500 ° C at a rate of 5 ° C / min and carbonized for 5 hours to prepare biochar, which was passed through a 30-mesh sieve for later use; 2.32 g of bismuth nitrate pentahydrate was dissolved in 1 mol / L nitric acid solution, diluted with 20 mL of deionized water, 1.0 g of beech wood biochar was mixed with 100 mL of 5 mmol / L bismuth nitrate pentahydrate, and ultrasonically dispersed for 60 minutes, and then vigorously stirred at 25 ° C for 4 hours, then rinsed with deionized water until the pH value was neutral, and then dried at 105 ° C to obtain bismuth-modified beech wood biochar.

[0044] (3) Bismuth-modified beech wood biochar was loaded with modified baddeleyite to prepare nano-mineral activated carbon.

[0045] 5.0 g of bismuth-modified beech wood biochar was ground at room temperature, passed through a 100-mesh sieve, mixed with 15.0 g of modified baddeleyite, transferred to a ball mill and worked at a rotation speed of 400 rpm for 12 hours, with the rotation direction changed every 1 hour, to obtain nano mineral activated carbon.

[0046] Comparative Example 1

[0047] A method for preparing an activated carbon adsorbent comprises the following steps:

[0048] 20 g of beech wood raw material was heated at 500 ° C at a rate of 5 ° C / min and carbonized for 5 hours to prepare biochar, which was passed through a 30-mesh sieve for later use; 2.32 g of bismuth nitrate pentahydrate was dissolved in 1 mol / L nitric acid solution, diluted with 20 mL of deionized water, 1.0 g of beech wood biochar was mixed with 100 mL of 5 mmol / L bismuth nitrate pentahydrate, and ultrasonically dispersed for 60 minutes, then vigorously stirred at 25 ° C for 4 hours, then rinsed with deionized water until the pH value was neutral, and then dried at 105 ° C to obtain an activated carbon adsorbent.

[0049] Comparative Example 2

[0050] A method for preparing an activated carbon adsorbent comprises the following steps:

[0051] 20 g of beech wood raw material was heated at 500° C. at a rate of 5° C. / min and carbonized for 5 hours to prepare biochar, which was then passed through a 30-mesh sieve to obtain an activated carbon adsorbent.

[0052] Now test the industrial dye adsorption effect of the activated carbon adsorbent prepared in Examples 1-3 and Comparative Examples 1-2, taking methylene blue dye as an example. After preparing 1 mmol / L of methylene blue standard solution, use a pipette to transfer the methylene blue standard solution into a 100 mL volumetric flask, add 100 mg of the activated carbon adsorbent prepared in Examples 1-3 and Comparative Examples 1-2, respectively, and use labels to distinguish them. After shaking at 25°C for 20 minutes, filter with a neutral qualitative filter paper with a diameter of 12.5 cm. Place the filtrate in a cuvette with a light path of 1 cm, and use a spectrophotometer to measure the absorbance at a wavelength of 665 nm to determine the sample's removal efficiency of the methylene blue dye solution. Five readings are obtained for each sample.

[0053] The average value is taken and the test results are shown in Table 1 below.

[0054] Table 1 Test of the adsorption effect of industrial dyes on activated carbon prepared in Examples 1-3 and Comparative Examples 1-2

[0055] project Removal efficiency (%) Example 1 98.3 Example 2 99.6 Example 3 98.7 Comparative Example 1 78.9 Comparative Example 2 54.1

[0056] As shown in Table 1, the nano-mineral activated carbon synthesized under different conditions in the examples has a certain influence on the methylene

[0057] The adsorption rate of blue dye can reach more than 98%, which is higher than that of untreated beech wood biochar and

[0058] The adsorption effect of activated carbon without mineral loading is significantly increased.

[0059] Now, the activated carbon prepared in Examples 1-3 and Comparative Examples 1-2 is subjected to an adsorption experiment of heavy metal pollutants, taking arsenic, lead and cadmium as examples. 0.1 mol / L heavy metal solutions of arsenic, lead and cadmium are prepared respectively, and 0.5 g of the activated carbon prepared in Examples 1-3 and Comparative Examples 1-2 is added respectively.

[0060] The samples were mixed and shaken for 24 hours, filtered, and then measured by atomic absorption spectrophotometry.

[0061] The content of heavy metals in the filtrate after treatment and the removal rate of heavy metal ions were calculated. Each sample was measured

[0062] The test results are shown in Table 2.

[0063] Table 2 Adsorption experiment of heavy metal pollutants in activated carbon prepared in Examples 1-3 and Comparative Examples 1-2

[0064]

[0065] From the results in Table 2, it can be seen that the activated carbon samples prepared in Examples 1-3 and Comparative Examples 1-2 have a removal effect on heavy metal pollutants, and the removal effect on cadmium is the best. The removal effect of the samples prepared in Examples 1-3 is better than that of the comparative examples.

[0066] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0067] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing nano mineral activated carbon, characterized in that: The following steps are involved: (1) Modification of baddeleyite using sodium alginate; (2) Preparation of bismuth-modified beech wood biochar; (3) Bismuth-modified beech wood biochar was loaded with modified baddeleyite to prepare nano-mineral activated carbon.

2. The method for preparing nano mineral activated carbon according to claim 1, characterized in that: The specific steps of modifying baddeleyite with sodium alginate are: The baddeleyite concentrate is washed with deionized water, calcium oxide powder is added, ground for 60 minutes at 40°C and then dried; the mixed powder of baddeleyite and calcium oxide is mixed with sodium alginate, Dolapix-CE-64 dispersant and deionized water, and ultrasonic dispersion is performed at 20kHz in a mode of ultrasonic treatment for 10 seconds and then paused for 50 seconds. After circulating for 20 minutes, the solution is degassed in a vacuum furnace at 25°C and 0.2 bar for 1-2 minutes, and then added dropwise to a 2% calcium chloride suspension, filtered after standing for 10 minutes, washed with distilled water and dried at room temperature for 24 hours, and sintered in a muffle furnace at an air atmosphere of 1000-1300°C at a heating rate of 5°C / min for 1 hour to obtain modified baddeleyite.

3. The method for preparing nano mineral activated carbon according to claim 2, characterized in that: The mass ratio of the mixed powder of baddeleyite and calcium oxide, sodium alginate and Dolapix-CE-64 dispersant is 1:1.5-2:0.05-0.

09.

4. The method for preparing nano mineral activated carbon according to claim 1, characterized in that: The specific operation for preparing bismuth-modified beech wood biochar is as follows: The beech wood raw material was heated at 500°C at a rate of 5°C / min for 5 hours to prepare biochar, which was passed through a 30-mesh sieve for later use; Bismuth nitrate pentahydrate was dissolved in 1 mol / L nitric acid solution and diluted with deionized water. The beech wood biochar was mixed with 5 mmol / L bismuth nitrate pentahydrate and ultrasonically dispersed for 60 minutes. The mixture was vigorously stirred at 25°C for 4 hours, and then rinsed with deionized water until the pH value was neutral. The mixture was then dried at 105°C to obtain bismuth-modified beech wood biochar.

5. The method for preparing nano mineral activated carbon according to claim 1, characterized in that: The specific operation of loading the bismuth-modified beech wood biochar with modified baddeleyite is as follows: The bismuth-modified beech wood biochar was ground at room temperature, passed through a 100-mesh sieve, mixed with modified baddeleyite, transferred to a ball mill and worked at a rotation speed of 400 rpm for 12 hours, with the rotation direction changed every 1 hour, to obtain nano mineral activated carbon.

6. The method for preparing nano mineral activated carbon according to claim 5, characterized in that: The mass ratio of bismuth-modified beech wood biochar to modified baddeleyite was 1:2-3.