Dampness-removing aldehyde-removing odor-removing particles, and preparation method and application thereof
The preparation of doped Er3+:TiO2 nanopowder by sol-gel method and wrapped on the composite matrix is solved, and the problem of poor adsorption effect of pure TiO2 is achieved efficiently remove formaldehyde and improve hygroscopicity. It is suitable for air purification, and the particles are in the sunlight. Reusable to meet environmental protection needs.
Patent Information
- Application Number
- CN202411342416.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The photocatalytic efficiency of existing adsorption materials such as pure TiO2 is low, resulting in poor adsorption effect, and the adsorbent is easily saturated, requiring desorption or renewal, which cannot effectively meet the indoor formaldehyde removal needs.
Doped Er3+:TiO2 nanopowder is prepared by sol-gel method and wrapped it on the activated carbon fiber and concave and concave rock stone composite matrix to form a high-performance adsorbent, which has physical adsorption and chemical decomposition functions to prepare efficient wetting and removal Aldehyde odor granules.
The photocatalytic activity and quantum efficiency of the adsorbent material are significantly improved, and the formaldehyde removal is achieved efficiently. The particles have high strength and good hygroscopicity. They are suitable for air purification and can be reused under sunlight, which is environmentally friendly and pollution-free.
Smart Images

Figure CN118904314A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic functional materials, and in particular to dehumidifying, dealdehyde-removing and odor-removing particles, a preparation method and applications thereof. Background Art
[0002] In family life, home decoration pollution is increasingly being taken seriously. Due to the use of some inferior paints and adhesives in the decoration process, these materials contain a large amount of organic matter. Pollutants such as formaldehyde, benzene, TVOC, etc. will threaten our health. Most of them are clear first-class carcinogens. Living in such an environment for a long time is not good for the body. Currently, the available indoor formaldehyde control technologies include adsorption, thermal destruction, absorption, photocatalysis, photochemical oxidation, etc. Among them, the adsorption method is the most widely used due to its relatively low cost and simple operation. Traditional adsorption materials often add titanium oxide photocatalysts as adsorbents, but pure TiO 2 The photocatalytic efficiency of formaldehyde adsorbents is not enough to meet the actual needs, because of its wide band gap and fast recombination rate of photoinduced electron pairs, which leads to considerable energy consumption, poor visible light catalytic activity and low quantum efficiency. Therefore, ordinary adsorbents have poor adsorption effect in practical applications, and adsorbent saturation requires desorption or renewal. Therefore, the development and application of new high-efficiency formaldehyde adsorption materials and the solution of adsorbent saturation problem in technology have become the focus of current research on indoor formaldehyde treatment. Summary of the invention
[0003] In view of the deficiencies in the prior art, the present invention proposes a dehumidifying, dealdehyde-removing and deodorizing particle, a preparation method and an application thereof.
[0004] A method for preparing dehumidifying, dealdehyde-removing and deodorizing particles comprises the following steps:
[0005] (1) dropping butyl titanate into anhydrous ethanol, adding an inhibitor, stirring, and mixing to obtain solution A; mixing anhydrous ethanol and deionized water, dropping acetic acid to adjust the pH, and stirring to obtain solution B;
[0006] (2) Add solution B to solution A and dropwise add Er(NO 3 ) 3 ·5H 2 O solution is stirred to form Er doped 3+ :TiO 2 Sol; add ammonia water to the sol, adjust the pH, ultrasonically mix, stand for aging, cool, wash with deionized water, dry, and calcine to obtain surface-encapsulated doped Er 3+ :TiO 2 Nano powder;
[0007] (3) Add deionized water to the activated carbon fiber powder, then add acrylic emulsion, stir, maintain the system temperature, add attapulgite and mix, add the surface-coated doped Er 3+ :TiO 2 The nano powder is stirred, filtered and dried to form the surface adsorbed Er doped 3+ :TiO 2 Composite matrix adsorbent of nano powder;
[0008] (4) Adsorbing and doping Er on the surface 3+ :TiO 2 The activated carbon fiber powder of the nano powder is rotated, and the methylcellulose is added and mixed to form spherical particles.
[0009] Preferably, the inhibitor comprises acetylacetone.
[0010] Preferably, the pH in step (1) is 2-3, and the pH in step (2) is 9-10.
[0011] Preferably, the calcination temperature is 400-500° C. and the calcination time is 1 hour.
[0012] Preferably, the temperature of the maintenance system is 50-55°C.
[0013] Preferably, the drying temperature is 80°C.
[0014] Preferably, the concentration of the lock methyl cellulose is 20%.
[0015] Preferably, the rotation speed is 50 to 100 r.min -1 , time is 2 to 4 hours.
[0016] The dehumidifying, formaldehyde-removing and odor-removing particles prepared by the above preparation method.
[0017] The above-mentioned dehumidifying, formaldehyde-removing and odor-removing particles are used in the production of adsorption materials.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] The present invention prepares a kind of black particles for dehumidification, dealdehyde removal and odor removal, and uses sol-gel to prepare a high-activity titanium-based photocatalytic material. 2 Nanopowder doped with rare earth element Er 3+, reducing the energy band gap of Ti ions, promoting the migration and separation of photogenerated carriers, forming a large number of oxygen vacancies, and on the porous adsorption matrix material, this application uses an aqueous acrylic emulsion wrapped on the surface of activated carbon fiber, which has active functional groups such as hydroxyl groups, and is made into a composite matrix adsorbent with attapulgite. The titanium-based photocatalytic material is adsorbed on the surface to prepare a high-performance adsorption material with physical adsorption and chemical decomposition functions, achieving the effects of formaldehyde removal and deodorization in the air, and using an adhesive to form high-strength, high-hygroscopic spherical particles under the molding equipment, which are pollution-free and corrosion-free to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0021] Figure 1 This is a picture of the dehumidifying, formaldehyde-removing and odor-removing particles.
[0022] Figure 2 This is the SEM image of the internal morphology of the dehumidifying, formaldehyde-removing and odor-removing particles.
[0023] Figure 3 No water-based acrylic emulsion is added in the preparation process, and Er is not doped on the surface. 3+ :TiO 2 SEM image of the internal morphology of nanopowder particles. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1:
[0026] A method for preparing black particles for dehumidification, dealdehyde removal and odor removal comprises the following steps:
[0027] Step 1, slowly drip 50 ml of butyl titanate into 100 ml of anhydrous ethanol, add 20 ml of acetylacetone as an inhibitor, and then stir for 30 minutes, mix evenly to obtain solution A for standby use; mix 100 ml of anhydrous ethanol and 20 ml of deionized water, drip glacial acetic acid to adjust the pH to 3, and stir evenly at room temperature to obtain solution B;
[0028] Step 2: Place solution A in a 70°C thermostat, slowly add solution B into solution A, and gradually drop 20 ml of Er(NO 3 ) 3 ·5H 2 O solution is stirred evenly to form doped Er 3+ :TiO 2 Sol; add ammonia water to the prepared sol, adjust the system to pH 9, ultrasonically mix at 50°C for 30 minutes, then stand at 60°C for aging for 12 hours, cool to room temperature, wash with deionized water 3 times, and dry in a vacuum drying oven at 80°C for 24 hours; calcine in the atmosphere at 400°C for 1 hour to obtain surface-encapsulated doped Er 3+ :TiO 2 Nano powder;
[0029] Step 3: Place 10g of activated carbon fiber powder in a beaker, then add 200ml of deionized water and 5ml of acrylic emulsion, stir in a constant temperature water bath, and keep the speed at 350r.min. -1 , maintain the system temperature at 55°C, stir for 1 to 2 hours, add 20 g of attapulgite into the system, continue stirring for 2 to 4 hours; slowly add the doped Er prepared in step 2 into the system 3+ :TiO 2 The nano powder was stirred for 30 minutes at a speed of 150 r.min. -1 After filtration, the solid powder was dried at 80℃ to obtain the surface adsorbed Er doped 3+ :TiO 2 Nano powder adsorbent powder.
[0030] Step 4: Rotate the adsorbent powder on a 50° turntable, spray 20% methylcellulose into the mixture, and mix at a turntable speed of 50 r.min. -1 Spherical particles are formed by rotating for 4 hours.
[0031] Embodiment 2:
[0032] A method for preparing black particles for dehumidification, dealdehyde removal and odor removal comprises the following steps:
[0033] Step 1: slowly drip 70 ml of butyl titanate into 150 ml of anhydrous ethanol, add 15 ml of acetylacetone as an inhibitor, and then stir for 30 minutes. After mixing evenly, a solution A is obtained for standby use; 150 ml of anhydrous ethanol and 20 ml of deionized water are mixed, glacial acetic acid is dripped into the mixture to adjust the pH to 2, and the solution B is obtained by stirring evenly at room temperature;
[0034] Step 2: Place solution A in a 70°C thermostat, slowly add solution B into solution A, and gradually drop 25 ml of Er(NO3 ) 3 ·5H 2 O solution is stirred evenly to form doped Er 3+ :TiO 2 Sol; add ammonia water to the prepared sol, adjust the system to pH 10, ultrasonically mix at 50°C for 30 minutes, then stand at 60°C for aging for 12 hours, cool to room temperature, wash with deionized water 5 times, and dry in a vacuum drying oven at 80°C for 24 hours; calcine in the atmosphere at 500°C for 1 hour to obtain surface-encapsulated doped Er 3+ :TiO 2 Nano powder;
[0035] Step 3: Place 12g of activated carbon fiber powder in a beaker, then add 220ml of deionized water and 10ml of acrylic emulsion, stir in a constant temperature water bath, and keep the speed at 500r.min. -1 , maintain the system temperature at 50°C, stir for 1 to 2 hours, add 25g of attapulgite into the system, continue stirring for 2 to 4 hours; slowly add the doped Er prepared in step 2 into the system 3+ :TiO 2 The nano powder was stirred for 30 min at a speed of 200 r.min. -1 After filtration, the solid powder was dried at 80℃ to obtain the surface adsorbed Er doped 3+ :TiO 2 Nano powder adsorbent powder.
[0036] Step 4: Rotate the adsorbent powder on a 60° turntable, spray 20% methylcellulose into the mixture, and rotate the turntable at 100 rpm. -1 Spherical particles are formed under rotation for 2 hours.
[0037] Comparative Example 3:
[0038] A method for preparing particles comprises the following steps:
[0039] Step 1: Place 10g of activated carbon fiber powder in a beaker, then add 200ml of deionized water and stir in a constant temperature water bath at a speed of 350r.min. -1 The system temperature was maintained at 55°C, and after stirring for 1 to 2 hours, 20 g of attapulgite was added to the system, and stirring was continued for 2 to 4 hours. After filtering, the solid powder was dried at 80°C to obtain the adsorbent powder.
[0040] Step 2: Rotate the adsorbent powder on a 50° turntable, spray 20% methylcellulose into the mixture, and mix at a turntable speed of 50 r.min. -1 Spherical particles are formed by rotating for 4 hours.
[0041] The dehumidifying, dealdehyde-removing and odor-removing black particles prepared in Example 1 are Figure 1 As shown, the particle size is about 1.5 to 2.5 mm, the size is relatively uniform, and the internal morphology is as follows Figure 2 As shown, the rod-like crystals of attapulgite are arranged neatly and orderly, and tiny adsorbed particles can be seen on the surface. The specific surface area is large and can be effectively adsorbed. The samples were entrusted to Nanjing Mineral Resources Supervision and Inspection Center for performance testing. According to DZG93-06 standard, the results show that the particles prepared by the present invention have excellent dryness. Under the conditions of air humidity of 66% and temperature of 22°C, the moisture absorption rate reaches 39.8%, the moisture content is lower than 5.3%, and the pH value is 7.37. The particles have good strength under the action of carboxymethyl cellulose adhesive, which can reach 4.1Mpa. The structure is stable. The particles do not fall apart after being soaked in water for 7 days. The weighed moisture absorption rate reaches more than 57%, which has good water absorption. The particles have a good air purification effect. After 24 hours, the air formaldehyde purification rate reaches more than 95%, which can effectively remove odor in the air environment without any chemical fungicide addition, reduce pollution, meet the deodorization and deodorization needs of confined spaces, physically adsorb formaldehyde to remove odor and moisture, and can be used again after sunlight exposure, which is more ecological and environmentally friendly.
[0042] As a performance comparison, in Comparative Example 3, the internal morphology is as follows Figure 3 As shown in the figure, most of the attapulgite crystals are in the state of aggregates, with coarse crystals, small specific surface area, and low adsorption. No water-based acrylic emulsion is added in the sample preparation process, and the surface is not doped with Er. 3+ :TiO 2 Nano powder has certain moisture absorption and formaldehyde removal functions, but its performance indicators are relatively low. Under the conditions of air humidity of 66% and temperature of 22°C, the moisture absorption rate is 18.67%. After 24 hours, the air formaldehyde purification rate reaches more than 42%.
[0043] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0044] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for preparing dehumidifying, dealdehyde-removing and deodorizing particles, It is characterized in that The following steps are involved: (1) dropping butyl titanate into anhydrous ethanol, adding an inhibitor, stirring, and mixing to obtain solution A; mixing anhydrous ethanol and deionized water, dropping acetic acid to adjust the pH, and stirring to obtain solution B; (2) Add solution B to solution A and dropwise add Er(NO 3 ) 3 ·5H 2 O solution is stirred to form Er doped 3+ :TiO 2 Sol; add ammonia water to the sol, adjust the pH, ultrasonically mix, stand for aging, cool, wash with deionized water, dry, and calcine to obtain surface-encapsulated doped Er 3+ :TiO 2 Nano powder; (3) Add deionized water to the activated carbon fiber powder, then add acrylic emulsion, stir, maintain the system temperature, add attapulgite and mix, add the surface-coated doped Er 3+ :TiO 2 The nano powder is stirred, filtered and dried to form the surface adsorbed Er doped 3+ :TiO 2 Composite matrix adsorbent of nano powder; (4) Adsorbing and doping Er on the surface 3+ :TiO 2 The activated carbon fiber powder of the nano powder is rotated, and the methylcellulose is added and mixed to form spherical particles.
2. The method for preparing the dehumidifying, dealdehyde-removing and deodorizing particles according to claim 1, It is characterized in that The inhibitor includes acetylacetone.
3. The method for preparing the dehumidifying, dealdehyde-removing and deodorizing particles according to claim 1, It is characterized in that The pH in step (1) is 2-3, and the pH in step (2) is 9-10.
4. The method for preparing the dehumidifying, dealdehyde-removing and deodorizing particles according to claim 1, It is characterized in that The calcination temperature is 400-500° C. and the calcination time is 1 hour.
5. The method for preparing the dehumidifying, dealdehyde-removing and deodorizing particles according to claim 1, It is characterized in that The temperature of the maintenance system is 50-55°C.
6. The method for preparing the dehumidifying, dealdehyde-removing and deodorizing particles according to claim 1, It is characterized in that The drying temperature is 80°C.
7. The method for preparing the dehumidifying, dealdehyde-removing and deodorizing particles according to claim 1, It is characterized in that The concentration of the lock methyl cellulose is 20%.
8. The method for preparing the dehumidifying, dealdehyde-removing and deodorizing particles according to claim 1, It is characterized in that The rotation speed is 50-100 r.min -1 , time is 2 to 4 hours.
9. The dehumidifying, dealdehyde-removing and odor-removing granules obtained by the preparation method according to any one of claims 1 to 8.