Diatomite carrier and catalyst prepared from diatomite carrier and used for synthesizing allyl acetate
By using a combination of diatomaceous earth support and inert additives, a high mechanical strength lascini-type support was prepared and a stable palladium-copper catalyst was formed thereon, which solved the unstable catalytic activity and insufficient mechanical strength of the existing support. The problem of this paper improves the selectivity and space-time yield of propylene acetate synthesis, and reduces the pressure drop.
Patent Information
- Application Number
- CN202410961495.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The existing silica support has unstable catalytic activity in the synthesis of propylene acetate, and the support has low mechanical strength, resulting in high bed pressure drop and short catalyst service life.
Using diatomaceous earth as a carrier, a lascini-type carrier with high mechanical strength was prepared by mixing with inert additives and binders and dispersing of silica sols, and metal components such as palladium and copper were impregnated thereon. , forming a stable catalyst.
The selectivity and spatiotemporal yield of propylene acetate synthesis are improved, the pressure drop of the reaction bed is reduced, the service life of the catalyst is extended, and the high catalytic selectivity is maintained.
Smart Images

Figure CN118904322A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fine chemical synthesis, and particularly relates to a diatomaceous earth carrier and a catalyst for synthesizing propylene acetate prepared by using the diatomaceous earth carrier. Background Art
[0002] The synthesis of propylene acetate generally uses propylene, oxygen and acetic acid as raw materials, and an oxidation reaction is carried out in a tubular fixed bed reactor loaded with palladium and copper catalysts at a reaction temperature of 140-200°C and a reaction pressure of 0.75MPa(G) to generate propylene acetate. In order to obtain highly active and highly selective catalysts, researchers have been continuously improving the active component composition, preparation process and even shape of the catalyst. For example, the early preparation method of propylene acetate catalyst is to uniformly impregnate metals such as Pd and Cu into the interior and surface of the carrier, because the reactants are not easy to diffuse to the center or inner area of the porous network of the catalyst. Therefore, the reaction mainly occurs only in the outermost or surface area of the catalyst. The catalyst components in the inner area of the carrier do not play a big role in the progress of the reaction, resulting in a reduction in the catalytic efficiency of the catalyst components per unit weight. The local concentration of precious metals on the surface of the catalyst obtained in this way is low, and the catalytic activity is not high. In order to enhance the utilization rate of precious metals, the earliest method proposed was to first impregnate metal salts and then use alkali or alkaline earth metals to precipitate these metal salts, and fix the active components only on the surface of the carrier. Core-shell catalyst. Some studies have also proposed using a solution containing palladium and copper compounds to impregnate the carrier. The impregnated carrier is contacted with an aqueous solution containing an alkaline compound (such as sodium silicate) to precipitate the aqueous palladium and copper compounds into water-insoluble palladium and copper compounds; then a reducing agent (such as hydrated hydrazine) is used to convert the palladium and copper compounds into a Pd-Cu alloy; finally, the carrier is impregnated with an alkali metal acetate and dried.
[0003] The carriers of supported Pd-Cu catalysts are mainly activated carbon, alumina, silica, etc. The use of activated carbon as a carrier has the following advantages: (1) The carbon matrix itself has strong acid and alkali resistance; (2) The carbon has good temperature resistance and can maintain its structural morphology even at higher temperatures; (3) The high specific surface area and porosity of activated carbon can make the active phase highly dispersed, and the reaction heat can be removed in time to reduce condensation and condensation; (4) Precious metals can be recovered from waste catalysts by burning the activated carbon carrier. 2 O 3 As a support, in addition to Pd-Cu being the active component, γ-Al 2 O 3 Since its acidic sites can also act as a promoter in the esterification reaction, this catalyst has a bifunctional effect. 2 It is a porous substance with good chemical inertness and high adsorption capacity. It is used as an adsorbent in industry, and can also be used as a filler and catalyst carrier.
[0004] Compared with activated carbon and alumina carriers, silica is more widely used as a carrier in the production of vinyl acetate and propylene acetate. For example, a patent document discloses a technology for preparing propylene acetate by using propylene, acetic acid and oxygen, in which the carrier used is SiO 2 or SiO 2 / Al 2 O 3 There are also documents that disclose the use of palladium, potassium acetate, copper loaded with SiO 2 The carrier is then prepared into a catalyst for producing propylene acetate. The carrier for preparing vinyl acetate and propylene acetate is a known inert carrier material, such as a catalyst with a specific surface area of (40 to 350) m 2 ·g -1 The average pore size of this type of carrier measured by BET method is (5-200) nm, especially SiO 2 and SiO 2 / Al 2 O 3 mixture.
[0005] Generally, such catalyst supports show high activity. Unfortunately, the catalytic activity of palladium copper catalysts using silica has been unstable. This variability is partly related to the distribution and contour of the catalyst components deposited on and associated with the support. In order to increase the selectivity of acetylation of propylene to produce propylene acetate, the SiO2 can be treated by chemical pore expansion and hydrothermal treatment. 2 The carrier is expanded to increase the volume. At present, the shape of the catalyst carrier used in the production of propylene acetate by propylene method in China is basically spherical. One is pressed and elliptical; the other carrier is rolled and completely spherical, with an average particle size of 5 to 6 mm. According to relevant data, the bed void ratio of spherical objects is the smallest, and the bed pressure drop is inversely proportional to the cube of the void ratio. This means that under the condition of increasing the feed space velocity, the bed pressure drop of spherical objects will greatly increase, which will have an adverse effect on mass transfer and heat transfer. In the reaction of synthesizing propylene acetate by propylene method, in order to significantly increase the output, a more feasible method is to increase the feed space velocity, thereby increasing the absolute oxygen supply of the reaction. Therefore, it is of great significance to develop a catalyst that can increase the feed space velocity for the synthesis of propylene acetate. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a diatomaceous earth carrier and a catalyst for synthesizing propylene acetate prepared using the diatomaceous earth carrier. The diatomaceous earth carrier prepared by the present invention can effectively improve the selectivity and time-space yield of propylene acetate produced by acetylation of propylene and reduce the pressure drop.
[0007] The invention provides a method for preparing a diatomaceous earth carrier.
[0008] Specifically, a method for preparing a diatomaceous earth carrier comprises the following steps:
[0009] Mix diatomaceous earth, inert auxiliary agent and adhesive; then add silica sol, stir and knead, and place in a sealed container for 20 to 60 hours to disperse the silica sol between the microparticles of diatomaceous earth; make Raschig rings after stirring and kneading, and place at 5 to 35°C for 20 to 60 hours to dry in the shade; finally, calcine the dried Raschig rings to obtain a diatomaceous earth carrier.
[0010] Preferably, the amount of the binder added is 1% to 20% of the mass of the diatomite; further preferably, the amount of the binder added is 3% to 15% of the mass of the diatomite; more preferably, the amount of the binder added is 3% to 10% of the mass of the diatomite.
[0011] Preferably, the adhesive comprises a first polymer and a second polymer, wherein the first polymer comprises polyacrylamide and / or polyvinyl alcohol, and the second polymer comprises cellulose and / or modified starch. The cellulose is preferably hydroxymethyl cellulose. In some embodiments, the first polymer is polyvinyl alcohol, and the second polymer is a hydroxymethyl cellulose solution. The first polymer and the second polymer are substantially free of residue after calcination.
[0012] Preferably, the mass ratio of the first polymer to the second polymer is (0.5-2):1; further preferably, the mass ratio of the first polymer to the second polymer is (0.8-1.5):1.
[0013] Preferably, the first polymer is added in the form of a first polymer solution, and the mass concentration of the first polymer solution is 1.0% to 10.0%; further preferably, the mass concentration of the first polymer solution is 3.0% to 8.0%.
[0014] Preferably, the second polymer is added in the form of solid powder.
[0015] When the diatomite is mixed with the first polymer and the second polymer in the adhesive, the second polymer added in solid form is distributed between the diatomite particles to play a bonding role; while the first polymer added in solution form will penetrate into the micropores in the diatomite particles and fully interact with the micropores. The two work together to make the pores of the final diatomite carrier evenly distributed, without affecting the pore structure of the carrier itself, and can improve the mechanical strength of the carrier.
[0016] Preferably, the particle diameter of the diatomaceous earth is less than 44 μm.
[0017] Preferably, the specific surface area of the diatomaceous earth is 20 to 60 m / g.
[0018] Preferably, the inert additive comprises quartz powder and / or short glass fibers. The inert additive has high temperature resistance and a small thermal expansion coefficient, so it can reduce the deformation of the catalyst due to stress, resulting in crushing and powdering during the exothermic process of propylene acetate synthesis.
[0019] Preferably, the mass of the inert auxiliary agent is 1% to 12% of the mass of the diatomaceous earth; further preferably, the mass of the inert auxiliary agent is 5% to 10% of the mass of the diatomaceous earth.
[0020] Preferably, the sealed placement time is 30 to 50 hours.
[0021] Preferably, the Na content in the silica sol is less than 0.1%.
[0022] Preferably, the average diameter of the silica sol particles is 10 to 30 nm.
[0023] Preferably, the mass concentration of the silica sol is 20% to 40%; further preferably, the mass concentration of the silica sol is 20% to 30%.
[0024] Preferably, the amount of the silica sol added is 15% to 60% of the mass of the diatomite; further preferably, the amount of the silica sol added is 15% to 40% of the mass of the diatomite.
[0025] Preferably, the process of drying in the shade is to place the mixture in the shade at 5 to 30° C. for 30 to 50 hours.
[0026] Preferably, the calcination process is performed at 500-900°C for 2-4 hours; further preferably, the calcination process is performed at 700-850°C for 2-4 hours; more preferably, the calcination process is performed at 7500-850°C for 2-4 hours.
[0027] The invention also provides a diatomaceous earth carrier.
[0028] A diatomaceous earth carrier is prepared by the above-mentioned preparation method, and the diatomaceous earth carrier is in the shape of Raschig ring.
[0029] Preferably, the diatomaceous earth carrier has an inner diameter of 1 to 3 mm, an outer diameter of 5 to 8 mm, and a height of 4 to 8 mm.
[0030] The invention also provides a catalyst for synthesizing propylene acetate.
[0031] Specifically, a catalyst for synthesizing propylene acetate comprises the diatomaceous earth carrier, and palladium and copper loaded on the diatomaceous earth carrier.
[0032] Preferably, the loading amount of palladium is 0.01% to 1%.
[0033] Preferably, the copper loading is 0.01% to 1%.
[0034] Preferably, the catalyst further comprises potassium, and the potassium is loaded on the diatomaceous earth carrier, and the loading amount of the potassium is 1% to 10%.
[0035] The invention also provides a method for preparing the catalyst.
[0036] Specifically, the preparation method of the above catalyst comprises the following steps:
[0037] The diatomaceous earth carrier is impregnated with a water-soluble salt solution containing palladium and copper; then an alkali solution is added to the diatomaceous earth carrier to convert copper ions and palladium ions into insoluble palladium and copper compounds; then a reducing agent is added to reduce the palladium and copper compounds into palladium and copper, and finally, the catalyst is impregnated with a potassium salt solution and dried to obtain the catalyst.
[0038] Preferably, the water-soluble salt solution includes one of acetate solution, sulfate solution, nitrate solution, and chloride solution. That is, palladium acetate solution, palladium sulfate solution, palladium nitrate solution, palladium chloride solution, cupric chloride solution, cupric acetate solution, cupric nitrate solution, or cupric sulfate solution. Further preferably, the water-soluble salt solution is a nitrate solution. When palladium nitrate and cupric acetate are used as metal sources, the washing step can be omitted (such as washing to remove chloride ions when chloride salts are used), and the preparation process is simple; and the hidden danger of copper poisoning by chlorine is avoided; in addition, it can also avoid that chloride ions will form a low melting point and highly mobile CuCl substance with copper, and Cu and Cl will combine to generate a large amount of heat, which will accelerate the sintering of metallic copper and sharply reduce the catalytic activity. Using palladium nitrate and cupric acetate as metal sources can further improve the stability of the catalyst and avoid the decrease in the catalytic selectivity of the catalyst after long-term use.
[0039] Preferably, the water-soluble salt solution comprises a solvent, and the solvent comprises water, carboxylic acid, alcohol or benzene; further preferably, the solvent is water or acetic acid.
[0040] Preferably, the impregnation amount of the water-soluble salt solution containing palladium and copper is 95% to 100% of the water absorption value of the diatomaceous earth carrier.
[0041] Preferably, the alkali solution includes sodium silicate, ammonia water, sodium hydroxide, sodium carbonate or potassium hydroxide; further preferably, the alkali solution is sodium silicate.
[0042] Preferably, the reducing agent includes hydrazine hydrate, sodium borohydride or glucose; more preferably, the reducing agent is hydrazine hydrate. The amount of the reducing agent is 5 to 20 times the reaction equivalent required to completely convert the palladium and copper compounds into palladium and copper metals.
[0043] Preferably, the potassium salt solution is a potassium acetate solution, and the mass percentage of the potassium acetate solution is 5%-15%.
[0044] Preferably, the drying method includes vacuum drying or freeze drying, preferably vacuum drying.
[0045] Diatomaceous earth is a diatomaceous silicon oxide with amorphous silicon dioxide as the main catalyst particle, which can withstand the acidic atmosphere in the synthesis of propylene acetate. Compared with fumed silica raw materials, diatomaceous earth is cheap and has a large output. It contains abundant micropores inside, has a large specific surface area, light weight, and good water absorption performance.
[0046] In the prior art, although the silica content of the diatomite carrier can reach more than 90%, the specific surface area and the pore size are large, the prepared carrier usually has low mechanical strength, and is fragile and easy to pulverize, which will cause the bed pressure drop to be high and the flow to be biased, thereby greatly reducing the processing capacity of the catalyst and greatly shortening the service life of the catalyst. The carrier is prepared into a Raschig ring type, and its mechanical strength is weaker than that of a strip catalyst due to its hollow structure. The present invention is aimed at this problem and provides a Raschig ring diatomite carrier with high mechanical strength. The palladium copper catalyst prepared by the carrier can effectively improve the selectivity and space-time yield of propylene acetylation to produce propylene acetate and reduce the pressure drop. Especially after 1000 hours of reaction, it can still maintain high catalytic selectivity while improving the space-time yield and reducing the pressure drop.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] The present invention uses diatomite and an inert auxiliary agent as raw materials, and controls the preparation process to prepare a Raschig ring diatomite carrier with high mechanical strength. The catalyst prepared by using the Raschig ring diatomite provided by the present invention can not only improve the reaction activity and selectivity due to its hollow structure, but also improve the mass transfer and heat transfer conditions of the reaction bed, increase the contact area of the reactants, and reduce the pressure drop of the catalyst bed. After the reaction is 1000 hours, it can still maintain high catalytic selectivity, and can also significantly improve the time-space yield and reduce the pressure drop. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is a schematic diagram of the structure of the diatomaceous earth carrier prepared in Example 2. DETAILED DESCRIPTION
[0050] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0051] Unless otherwise specified, the raw materials, reagents or devices used in the following examples and comparative examples can be obtained from conventional commercial sources or by existing known methods.
[0052] Example 1
[0053] A method for preparing a diatomaceous earth carrier comprises the following steps:
[0054] Weigh 1000g of diatomite raw material, 90g of quartz powder and 35g of hydroxymethyl cellulose, add them into a mixer equipped with a pressure nozzle, close the material port, and start stirring. Use a plunger pump to spray 650g of polyvinyl alcohol solution (mass concentration is 5.3wt%), then spray 200g of silica sol (30wt%), and place it in a sealed container for 30h. After fully stirring again, knead quickly and squeeze out Raschig rings (outer diameter is 6mm, inner diameter is 2mm, height is 6mm); after extruding the strips, place them at room temperature for 72h to dry in the shade, and finally roast them at 700℃ for 2h to obtain the diatomite carrier.
[0055] Example 2
[0056] A method for preparing a diatomaceous earth carrier comprises the following steps:
[0057] Weigh 1000g of diatomite raw material, 90g of quartz powder and 35g of hydroxymethyl cellulose, add them to a mixer equipped with a pressure nozzle, close the material port, and start stirring. Use a plunger pump to spray 650g of polyvinyl alcohol solution (mass concentration is 5.3wt%), then spray 200g of silica sol (30wt%), and place it in a sealed container for 30h. After fully stirring again, quickly knead and squeeze out Raschig rings (outer diameter 6mm; inner diameter 2mm; height 6mm; as shown in Figure 2). Figure 1 After extrusion, the strips were placed at room temperature for 72 hours to dry in the shade, and finally calcined at 800°C for 2 hours to obtain a diatomaceous earth carrier.
[0058] Comparative Example 1
[0059] A method for preparing a diatomaceous earth carrier comprises the following steps:
[0060] Weigh 1000g of diatomite raw material, 90g of quartz powder and 35g of hydroxymethyl cellulose, add them into a mixer equipped with a pressure nozzle, close the material port, and start stirring. Use a plunger pump to spray 650g of polyvinyl alcohol solution (mass concentration is 5.3wt%), then spray 200g of silica sol (30wt%), and place it in a sealed container for 30h. After fully stirring again, knead quickly and extrude strips (diameter is 6mm); after extruding the strips, place them at room temperature for 72h to dry in the shade, and finally roast them at 800℃ for 2h to obtain the diatomite carrier.
[0061] Comparative Example 2
[0062] A method for preparing a diatomaceous earth carrier comprises the following steps:
[0063] Weigh 1000g of diatomite raw material, 90g of quartz powder and 35g of hydroxymethyl cellulose, add them into a mixer equipped with a pressure nozzle, close the material port, and start stirring. Use a plunger pump to spray 650g of polyvinyl alcohol solution (mass concentration is 5.3wt%), then spray 200g of silica sol (30wt%), quickly knead and squeeze out Raschig rings (outer diameter is 6mm; inner diameter is 2mm; height is 6mm); after extrusion, place it at room temperature for 72h to dry in the shade, and finally roast it at 800℃ for 2h to obtain a diatomite carrier.
[0064] Comparative Example 3
[0065] A method for preparing a diatomaceous earth carrier comprises the following steps:
[0066] Weigh 1000g of diatomite raw material, 90g of quartz powder and 35g of hydroxymethyl cellulose, add them into a mixer equipped with a pressure nozzle, close the material port, and start stirring. Use a plunger pump to spray 650g of polyvinyl alcohol solution (mass concentration is 5.3wt%), then spray 200g of silica sol (30wt%), and place it in a sealed container for 30h. After fully stirring again, knead quickly and squeeze out Raschig rings (outer diameter is 6mm; inner diameter is 2mm; height is 6mm); after extruding the strips, immediately put them into an oven for drying at 120℃, and finally roast them at 800℃ for 2h to obtain the diatomite carrier.
[0067] Comparative Example 4
[0068] A method for preparing a diatomaceous earth carrier comprises the following steps:
[0069] Weigh 1000g of diatomite raw material and 35g of hydroxymethyl cellulose, add them into a mixer equipped with a pressure nozzle, close the material port, and start stirring. Use a plunger pump to spray 650g of polyvinyl alcohol solution (mass concentration is 5.3wt%), then spray 200g of silica sol (30wt%), and place it in a sealed container for 30h. After fully stirring again, knead quickly and squeeze out Raschig rings (outer diameter is 6mm; inner diameter is 2mm, height is 6mm); after extruding the strips, place them at room temperature for 72h to dry in the shade, and finally roast them at 800℃ for 2h to obtain the diatomite carrier.
[0070] Application Example 1
[0071] A method for preparing a catalyst for synthesizing propylene acetate comprises the following steps:
[0072] Weigh 1000g of the Raschig ring carrier prepared in Example 2 above, prepare 200g of palladium nitrate solution containing palladium (containing 0.03wt% Pd), weigh 10g of copper nitrate trihydrate, dilute to 1600ml with deionized water, and soak at room temperature for 1 hour to prepare a catalyst precursor. 31.6g of sodium silicate pentahydrate is prepared into 160mL of aqueous solution and added to the above catalyst precursor, shaken several times to avoid caking, and then allowed to stand for 5 hours. The catalyst precursor is impregnated with 30ml of hydrated hydrazine with a concentration of 85wt% for reduction, the impregnation time is 12 hours, and then dried at 60°C. The catalyst precursor is impregnated with 250mL of aqueous solution containing 27g of potassium acetate, and after impregnation for 5 hours, it is dried at 60°C to obtain a finished catalyst.
[0073] Application Example 2
[0074] A method for preparing a catalyst for synthesizing propylene acetate comprises the following steps:
[0075] Weigh 1000g of the Raschig ring carrier prepared in Example 2 above, prepare 200g of palladium chloride (containing 0.03wt% Pd) solution, weigh 10g of copper nitrate trihydrate, dilute to 1600ml with deionized water, and soak at room temperature for 1 hour to prepare a catalyst precursor. 31.6g of sodium silicate pentahydrate is prepared into 160mL of aqueous solution and added to the above catalyst precursor, shaken several times to avoid caking, and then allowed to stand for 5 hours. The catalyst precursor is impregnated with 30ml of hydrated hydrazine with a concentration of 85wt% for reduction, and the impregnation time is 12 hours. Wash the beads ten times with about 50ml of water, decant after each washing, until the chloride ion of the eluate is negative when tested with silver nitrate solution, and then dried at 60°C. The catalyst precursor is impregnated with 250mL of aqueous solution containing 27g of potassium acetate, and after impregnation for 5 hours, it is dried at 60°C to obtain the finished catalyst.
[0076] Application Example 3
[0077] Weigh 1000g of the Raschig ring carrier prepared in Example 1 above, prepare 200g of palladium nitrate solution containing palladium (containing 0.03wt% Pd), weigh 10g of copper nitrate trihydrate, dilute to 1600ml with deionized water, and soak at room temperature for 1 hour to prepare a catalyst precursor. 31.6g of sodium silicate pentahydrate is prepared into 160mL of aqueous solution and added to the above catalyst precursor, shaken several times to avoid caking, and then allowed to stand for 5 hours. The catalyst precursor is impregnated with 30ml of hydrated hydrazine with a concentration of 85wt% for reduction, the impregnation time is 12 hours, and then dried at 60°C. The catalyst precursor is impregnated with 250mL of aqueous solution containing 27g of potassium acetate, and after impregnation for 5 hours, it is dried at 60°C to obtain a finished catalyst.
[0078] Comparative application example 1
[0079] A method for preparing a catalyst for synthesizing propylene acetate comprises the following steps:
[0080] Weigh 1000g of the strip carrier prepared in the above comparative example 1, prepare 200g of palladium nitrate solution containing palladium (containing 0.03wt% Pd), weigh 10g of copper nitrate trihydrate, dilute to 1600ml with deionized water, and soak at room temperature for 1 hour to prepare a catalyst precursor. 31.6g of sodium silicate pentahydrate is prepared into 160ml of aqueous solution and added to the above catalyst precursor, shaken several times to avoid caking, and then allowed to stand for 5 hours. The catalyst precursor is impregnated with 30ml of hydrated hydrazine with a concentration of 85wt% for reduction, the impregnation time is 12 hours, and then dried at 60°C. The catalyst precursor is impregnated with 250ml of aqueous solution containing 27g of potassium acetate, and after impregnation for 5 hours, it is dried at 60°C to obtain a finished catalyst.
[0081] Comparative Application Example 2
[0082] A method for preparing a catalyst for synthesizing propylene acetate comprises the following steps:
[0083] Weigh 1000g of commercially purchased carrier KA160-ex silica carrier, prepare 200g of palladium nitrate solution (containing 0.03wt% Pd), weigh 10g of copper nitrate trihydrate, dilute to 1600ml with deionized water, and soak at room temperature for 1 hour to prepare a catalyst precursor. 31.6g of sodium silicate pentahydrate is prepared into 160mL of aqueous solution and added to the above catalyst precursor, shaken several times to avoid caking, and then allowed to stand for 5 hours. The catalyst precursor is impregnated with 30ml of hydrated hydrazine with a concentration of 85wt% for reduction, the impregnation time is 12 hours, and then dried at 60°C. The catalyst precursor is impregnated with 250mL of aqueous solution containing 27g of potassium acetate, and after impregnation for 5 hours, it is dried at 60°C to obtain the finished catalyst.
[0084] Comparative Application Example 3
[0085] A method for preparing a catalyst for synthesizing propylene acetate comprises the following steps:
[0086] Weigh 1000g of the Raschig ring carrier prepared in Comparative Example 4, prepare 200g of palladium nitrate solution containing palladium (containing 0.03wt% Pd), weigh 10g of copper nitrate trihydrate, dilute to 1600ml with deionized water, and soak at room temperature for 1 hour to prepare a catalyst precursor. 31.6g of sodium silicate pentahydrate is prepared into 160mL of aqueous solution and added to the above catalyst precursor, shaken several times to avoid caking, and then allowed to stand for 5 hours. The catalyst precursor is impregnated with 30ml of hydrated hydrazine with a concentration of 85wt% for reduction, the impregnation time is 12 hours, and then dried at 60°C. The catalyst precursor is impregnated with 250mL of aqueous solution containing 27g of potassium acetate, and after impregnation for 5 hours, it is dried at 60°C to obtain a finished catalyst.
[0087] Product effect testing
[0088] 1. The physicochemical indices of the carriers prepared in Examples 1 to 2 and Comparative Examples 1 to 4 were tested.
[0089] Because the carrier in the embodiment of the present invention has a macroporous structure, the specific surface area, pore volume and pore size are all measured by mercury intrusion. Catalyst strength determination method: See ASTM D4179-01 (Single particle crushing strength of shaped catalysts and catalyst carriers) to cover the compression "side compression strength" (SCS) of single particles measured in a regular form (such as a sphere, a short cylinder or a tablet). Apply pressure to the catalyst particles at a uniform rate until they are crushed or collapsed, and record the maximum crushing strength (at the time of initial collapse). The measurement results are shown in Table 1.
[0090] Table 1 Physical and chemical indicators of carriers (reduced state) prepared in various embodiments and comparative examples
[0091]
[0092] As is well known, the mechanical strength of silica carriers is not as high as that of alumina, especially when made into non-solid carriers such as Raschig rings. The difficulty in developing Raschig ring carriers lies mainly in the control of side strength. In the present invention, polymers such as hydroxymethyl cellulose and polyvinyl alcohol with a certain viscosity are first added to the diatomaceous earth raw material in different forms and mixed and stirred. Most of the adhesive will penetrate into the pores of the diatomaceous earth to fill the gaps, and the colloidal particles of silica sol added later are mainly dispersed between the diatomaceous earth particles for bonding to improve the mechanical strength. This addition method can avoid the addition of silica sol and affect the pore structure of the carrier itself. By comparing Example 1 and Example 2, it is found that increasing the calcination temperature of the carrier helps to improve the mechanical strength of the carrier. By comparing Comparative Example 4, it can be seen that the added quartz powder additive will block part of the pores of the diatomaceous earth, and the specific surface area, pore volume and pore size are reduced. The corresponding influence will be comprehensively discussed in conjunction with the catalytic activity below. It can be seen from Comparative Example 2 that the adhesive requires a certain amount of sealing time to diffuse into the internal structure of the diatomaceous earth raw material, and uniform dispersion also helps to improve the mechanical strength of the carrier. In Comparative Example 3, too fast drying and too fast evaporation of water will also affect the strength of the carrier.
[0093] 2. Catalyst performance evaluation
[0094] 700 mL of catalyst was loaded into the fixed bed reactor. The nitrogen pressure test was performed first. After confirming that there was no leakage, propylene was introduced until the nitrogen was completely replaced. Then the reactor inlet pressure was adjusted to 7 ktg / cm 2 The reactor bed temperature was adjusted to 138-145°C, and the reaction gas included 41 mol% propylene, 43 mol% nitrogen, 10 mol% acetic acid and 6 mol% oxygen.
[0095] Propylene, nitrogen, acetic acid and oxygen are mixed in a preheater and then fed. The acetic acid pump is adjusted to control its flow rate, and the propylene and oxygen flows are both controlled by mass flow rate controllers. The reaction gas is discharged after condensation in a condenser. The reaction product propylene acetate and unreacted acetic acid in the reaction liquid, as well as the side reaction product carbon dioxide, uncondensed propylene acetate and unreacted oxygen, nitrogen and propylene in the tail gas are analyzed. The evaluation results of the catalysts of each embodiment and comparative example are shown in Table 2. The calculation formulas for the activity and selectivity of the catalysts are as follows:
[0096]
[0097]
[0098] The activity evaluation results of the catalysts prepared in various examples and comparative examples are shown in Table 2.
[0099] Table 2 Evaluation results of catalyst activity prepared in various examples and comparative examples
[0100]
[0101] It can be seen from the activity evaluation data of the examples and comparative examples that the catalyst prepared using a diatomaceous earth carrier in the examples of the present invention can stably exert a catalytic effect under long-term high acid value reaction conditions, and the catalyst has excellent corrosion resistance and will not cause problems such as pulverization and increased pressure drop.
[0102] By comparing Application Example 1 with Comparative Application Examples 1 and 2, it can be found that the pressure drop of the Raschig ring carrier used in Application Example 1 of the present invention is smaller than that of the strip carrier used in Comparative Application Example 1, which can improve the mass transfer and heat transfer of the reaction bed, increase the contact area of the reactants, and help improve the space-time yield. Comparing Application Example 1 with Application Example 3, it can be found that the strength of the carrier will affect the pressure drop of the catalyst operation, and the weak strength of the carrier is likely to cause the pressure drop to rise due to crushing in the later stage of the catalyst operation. In the synthesis reaction of propylene acetate, temperature fluctuations can easily cause the catalytic reaction rate to be unstable, and it is an exothermic reaction, which is difficult to control the balance, causing intense local reactions, temperature rise, causing catalyst coking and shortening the service life of the catalyst. By analyzing Application Example 1 and Comparative Application Example 3, it can be found that the addition of quartz powder can enhance the thermal stability of the catalyst, because it has high temperature resistance and a small thermal expansion coefficient, so it can avoid the deactivation of the catalyst due to local overheating during the exothermic process of propylene acetate synthesis, and can effectively improve the space-time yield. By comparing Application Example 1 and Application Example 2, it can be found that the selectivity of the catalyst using palladium chloride as the palladium source decreases after the acclimation period. It is speculated that chloride ions will react with copper to form a CuCl substance with a low melting point and high mobility. At the same time, the combination of Cu and Cl generates a large amount of heat, which will accelerate the sintering of metallic copper and lead to a decrease in catalytic selectivity.
[0103] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a diatomaceous earth carrier, characterized in that: The following steps are involved: Mix diatomaceous earth, inert auxiliary agent and adhesive; then add silica sol, stir and knead, and place in a sealed container for 20 to 60 hours to disperse the silica sol between the microparticles of diatomaceous earth; make Raschig rings after stirring and kneading, and place at 5 to 35°C for 20 to 60 hours to dry in the shade; finally, calcine the dried Raschig rings to obtain a diatomaceous earth carrier.
2. The preparation method according to claim 1, characterized in that: The amount of the binder added is 1% to 20% of the mass of the diatomite; preferably, the amount of the binder added is 3% to 15% of the mass of the diatomite.
3. The preparation method according to claim 1 or 2, characterized in that: The adhesive comprises a first polymer and a second polymer, wherein the first polymer comprises polyacrylamide and / or polyvinyl alcohol, and the second polymer comprises cellulose and / or modified starch.
4. The preparation method according to claim 1 or 2, characterized in that: The inert auxiliary agent comprises quartz powder and / or short glass fibers; the mass of the inert auxiliary agent is 1% to 12% of the mass of the diatomaceous earth.
5. A diatomaceous earth carrier, characterized in that: The diatomaceous earth carrier is prepared by the preparation method described in any one of claims 1 to 4, and is in the shape of a Raschig ring; the inner diameter of the diatomaceous earth carrier is 1 to 3 mm, the outer diameter is 5 to 8 mm, and the height is 4 to 8 mm.
6. A catalyst for synthesizing propylene acetate, characterized in that: The invention comprises the diatomaceous earth carrier according to claim 5, and palladium and copper supported on the diatomaceous earth carrier.
7. The catalyst according to claim 6, characterized in that The loading amount of the palladium is 0.01% to 1%; the loading amount of the copper is 0.01% to 1%.
8. The catalyst according to claim 6 or 7, characterized in that The catalyst also includes potassium, which is loaded on the diatomaceous earth carrier; the loading amount of the potassium is 1% to 10%.
9. The method for preparing a catalyst according to any one of claims 6 to 8, characterized in that: The following steps are involved: The diatomaceous earth carrier is impregnated with a water-soluble salt solution containing palladium and copper; then an alkali solution is added to the diatomaceous earth carrier to convert copper ions and palladium ions into insoluble palladium and copper compounds; then a reducing agent is added to reduce the palladium and copper compounds into palladium and copper, and finally, the catalyst is impregnated with a potassium salt solution and dried to obtain the catalyst.
10. The preparation method according to claim 9, characterized in that: The reducing agent includes hydrazine hydrate, sodium borohydride or glucose.
Citation Information
Patent Citations
A preparation method of acetate propylene ester synthesis catalysts
CN101157030A
Low-temperature smoke denitration SCR (silicon controlled rectifier) catalyst and preparation method
CN102114424A
Catalyst for synthesizing isopropenyl acetate and preparation method thereof
CN102463139A
Preparation method of catalyst for synthesizing allyl acetate
CN103878022A
Preparation method of diatomite support with high mechanical strength
CN105126929A