Advanced Pd-based heterostructure formic acid dehydrogenation catalyst and preparation method thereof

The preparation of Pd-based heterostructure catalysts with high specific surface area and rich pore size structures by solvothermal method solves the problems of insufficient activity of existing catalysts and complex preparation processes, and significantly improves the performance and stability of formic acid dehydrogenation reaction.

CN118904329APending Publication Date: 2024-11-08JILIN UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410970780.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing Pd-based heterostructure catalysts have problems of insufficient activity and inactivation caused by nanoparticle agglomeration in the formic acid dehydrogenation reaction, and the preparation process is complex and difficult to control, resulting in a small specific surface area and low capacitance, which limits the catalytic performance.

Method used

Using solvothermal synthesis method, soluble zirconium salt and 2-aminoterephthalic acid react in dicarboxamide, followed by centrifugation, drying, grinding, and annealing in a nitrogen atmosphere, and finally palladium salt and NaBH4 were added to prepare Pd-based heterostructure catalyst with high specific surface area and rich pore size structure.

Benefits of technology

The surface permeability and active sites of the catalyst are improved, the performance and stability of formic acid dehydrogenation are significantly improved, and the specific surface area and better catalytic activity are provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904329A_ABST
    Figure CN118904329A_ABST
Patent Text Reader

Abstract

The invention discloses an advanced Pd-based heterostructure formic acid dehydrogenation catalyst and a preparation method thereof, and belongs to the technical field of formic acid dehydrogenation, and the preparation method comprises the following preparation steps: dissolving soluble zircon salt, 2-aminoterephthalic acid and concentrated hydrochloric acid in a dicarboxamide solvent to obtain a mixed solution; filling the mixed solution into a reaction kettle for solvothermal reaction; centrifuging, drying and grinding in sequence to obtain a powder sample; annealing and grinding the powder sample to obtain a precursor; adding palladium salt and NaBH4 into the precursor, uniformly stirring, and sequentially centrifuging, drying and grinding to obtain the advanced Pd-based heterostructure formic acid dehydrogenation catalyst. The prepared advanced Pd-based heterostructure formic acid dehydrogenation catalyst has a specific surface area of 330m < 2 > / g-480m < 2 > / g and a rich aperture structure, has better surface permeability and more active sites compared with electrode materials prepared by other methods, and improves the formic acid dehydrogenation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of formic acid dehydrogenation, and specifically relates to an advanced Pd-based heterostructure formic acid dehydrogenation catalyst and a preparation method thereof. Background Art

[0002] In recent years, formic acid has stood out among many hydrogen storage materials and attracted much attention due to its easy availability, convenient storage and transportation conditions, high hydrogen volume density and non-toxic properties. As the mainstream heterogeneous catalyst for the decomposition of formic acid, palladium-based supported catalysts are widely used, but they still face the challenges of insufficient activity and further deactivation due to easy agglomeration of nanoparticles. To solve this problem, the introduction of catalyst carriers is considered an effective way. However, in order to make such catalysts closer to practical applications, there is still room for optimization of the porous carriers currently used to support palladium nanoparticles. Specifically, the ideal catalyst carrier should have a high specific surface area to achieve efficient dispersion and loading of palladium nanoparticles; at the same time, the surface of the carrier should be rich in evenly dispersed heteroatoms to stabilize the loaded palladium nanoparticles and prevent them from agglomerating, thereby further improving the overall performance and stability of the catalyst.

[0003] The methods for preparing Pd-based heterogeneous structure catalysts in the prior art mainly include hydrothermal method, stepwise annealing method, etc. For example, the document "Designing a Robust Palladium Catalyst for Formic Acid Dehydrogenation" reports the synthesis of Pd-based catalysts by stepwise annealing method. First, melamine (10 mmol) and isocyanuric acid (10 mmol) are dissolved in 85°C distilled water (100 cm 3 ) to form solution A and solution B. Solution B was then added to solution A and stirred at 85°C for 4 hours. The white solid complex obtained by centrifugation was collected and dried at 85°C overnight. Finally, under a nitrogen atmosphere, the complex was calcined at 600°C (heating rate 5°C / min) for 4 hours to obtain PCN. PdCl2 was then dissolved in 0.5M hydrochloric acid, and then PCN (500mg) was added. The suspension was ultrasonically treated for 1 hour, stirred at room temperature for 6 hours, then rotary evaporated to remove moisture, and finally dried at 85°C overnight. After grinding, the brown powder was treated at 300°C for 5 hours (heating rate 5°C / min) under a nitrogen atmosphere. The obtained powder was centrifuged and precipitated with 1M ammonia water (50cm 3 ) was washed three times and then dried at 85° C. overnight. Finally, the powder was calcined again at 300° C. (heating rate 2° C. / min) for 5 hours under nitrogen atmosphere to obtain the final product.

[0004] The materials prepared by this method have extremely high process requirements and strict control of corresponding experimental conditions such as temperature, vacuum and other parameters, which makes it difficult to prepare catalytic materials by this method. In addition, the morphology produced by the preparation has a small specific surface area and low specific capacitance, which hinders its application in high-performance formic acid dehydrogenation catalysis. Summary of the invention

[0005] In view of this, the object of the present invention is to provide an advanced Pd-based heterostructure formic acid dehydrogenation catalyst and a preparation method thereof. The prepared advanced Pd-based heterostructure formic acid dehydrogenation catalyst has a higher specific surface area and a richer pore structure. Compared with catalyst materials prepared by other methods, it has better surface permeability and more active sites, thereby improving the performance of formic acid dehydrogenation.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] According to a first aspect of the present invention, there is provided a method for preparing an advanced Pd-based heterostructure formic acid dehydrogenation catalyst, comprising:

[0008] 1) dissolving a soluble zirconium salt, 2-aminoterephthalic acid and concentrated hydrochloric acid in a diformamide solvent to obtain a mixed solution, wherein the molar ratio of the soluble zirconium salt to the 2-aminoterephthalic acid is 1:1-2;

[0009] 2) The obtained mixed solution is charged into a reaction kettle for solvothermal reaction at a reaction temperature of 120° C. to 160° C. for a reaction time of 24 h to 36 h;

[0010] 3) After the solvothermal reaction, centrifugation, drying, and grinding are performed in sequence to obtain a powder sample;

[0011] 4) annealing the obtained powder sample in a nitrogen atmosphere at a temperature of 700°C to 1100°C for 5h to 7h, a heating rate of 3°C / min to 5°C / min, a cooling rate of 3°C / min to 5°C / min, lowering to room temperature, and grinding to obtain a precursor;

[0012] 5) Add palladium salt and NaBH4 to the obtained precursor, stir evenly, centrifuge, dry and grind in sequence to obtain an advanced Pd-based heterostructure formic acid dehydrogenation catalyst.

[0013] Furthermore, in step 1), the soluble zirconium salt is zirconium chloride, zirconium nitrate or zirconium sulfate.

[0014] According to a specific embodiment of the present invention, the volume of concentrated hydrochloric acid in step 1) is 4 mL to 6 mL.

[0015] According to a specific embodiment of the present invention, in step 3), the drying temperature is 60° C. to 80° C., and the drying time is 12 h to 18 h.

[0016] According to a specific embodiment of the present invention, in step 5), the mass ratio of palladium salt to NaBH4 is 1:1.

[0017] According to a specific embodiment of the present invention, in step 5), the palladium salt is H2PdCl4.

[0018] According to a second aspect of the present invention, there is provided an advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared by the above-mentioned advanced Pd-based heterostructure formic acid dehydrogenation catalyst preparation method, wherein the specific surface area of ​​the advanced Pd-based heterostructure formic acid dehydrogenation catalyst is 330 m 2 / g~480m 2 / g.

[0019] Compared with the prior art, the present invention has the following beneficial effects: the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared by the present invention has a higher specific surface area and a richer pore structure, and has better surface permeability and more active sites than the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared by other methods, thereby improving the performance of formic acid dehydrogenation. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 1 is the X-ray diffraction pattern of Example, Comparative Example 1 and Comparative Example 2;

[0021] Figure 2 1 is a nitrogen adsorption / desorption curve diagram of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example 1 and Comparative Example 1;

[0022] Figure 3 1 is a nitrogen adsorption / desorption curve diagram of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example 1 and Comparative Example 2;

[0023] Figure 4 is a diagram of formic acid decomposition activity of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example and Comparative Example 1;

[0024] Figure 5 is a diagram of formic acid decomposition activity of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example and Comparative Example 2;

[0025] Figure 6 is a graph of conversion frequency-reaction number of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example;

[0026] Figure 7 Graph showing the cyclic stability of formic acid decomposition of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example. DETAILED DESCRIPTION

[0027] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0028] The following reagents and raw materials, unless otherwise specified, are commercially available.

[0029] The present invention has no particular limitation on the mixing method of various drugs, and any mixing method well known to those skilled in the art may be used.

[0030] The present invention does not specifically limit the grinding method, and any grinding method known to those skilled in the art can be selected. The present invention does not specifically limit the grinding degree, and any grinding degree known to those skilled in the art can be selected.

[0031] Example

[0032] ZrCl4 zirconium chloride (1.12g 4.8mmoL) and 2-aminoterephthalic acid (0.87g 4.8mmoL) were added to 160mL of diformamide solvent, and the mixture was stirred for 10min, and concentrated hydrochloric acid (4.8mL) was added to obtain a mixed solution. The mixed solution was then transferred to a Teflon stainless steel autoclave, heated at 120°C for 24h, centrifuged, dried, and ground to obtain a powder sample at a drying temperature of 60°C for 18h. 50mg of the powder sample was placed in a crucible, and the temperature was increased to 800°C at 5°C / min in a nitrogen atmosphere, and maintained at this temperature for 5h, and then cooled to room temperature at 5°C / min to obtain a precursor.

[0033] 100 mg of the precursor was mixed with 10 mL of deionized water, and then dispersed by ultrasonication. 1.5 mL of H2PdCl4 (0.02 M) was added under stirring. After stirring at room temperature for 10 h, NaBH4 sodium borohydride (30 mg) was added and stirred for 1 h. The mixture was centrifuged (8000 r / min, 5 min), washed with water and ethanol for 3 times, and dried at 50°C to obtain the sample of the embodiment.

[0034] Figure 1 is the X-ray diffraction pattern of the sample prepared in Example, Figure 1 It can be seen that the diffraction peaks of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst correspond one to one with the standard card, indicating that no other impurities are produced, indicating that a homogeneous phase with high crystallinity is synthesized.

[0035] Figure 2 is the nitrogen adsorption-desorption curve of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example, Figure 2 It can be seen that the advanced Pd-based heterostructure formic acid dehydrogenation catalyst has a larger specific surface area and more active sites.

[0036] Figure 43 is a diagram of the formic acid decomposition activity of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example 1. It can be seen from the diagram that the material has a high catalytic activity formic acid decomposition.

[0037] Figure 6 3 is a graph of conversion frequency-reaction number of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Example 1. It can be seen from the graph that the material has a higher conversion rate.

[0038] Figure 7 4 is a graph showing the cyclic stability of formic acid decomposition of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in the example. It can be seen from the graph that the material has relatively good cyclic stability.

[0039] Comparative Example 1

[0040] Add ZrCl4 (1.56g) and 2-aminoterephthalic acid (0.99g) to 180mL dimethylformamide solvent. After stirring for 15min, add concentrated hydrochloric acid (6ml) to obtain a mixed solution. Then transfer the obtained mixed solution to a Teflon stainless steel autoclave, heat it at 120℃ for 24h, centrifuge, dry it, grind it in sequence to obtain a powder sample, the drying temperature is 70℃, and the time is 15h; put the above 50mg powder sample into a crucible, heat it to 1100℃ at 4℃ / min in a nitrogen atmosphere, keep it at this temperature for 6h, and then cool it down at 4℃ / min to room temperature to obtain a precursor.

[0041] 100 mg of the precursor was mixed with 10 mL of deionized water, and then ultrasonically dispersed. 2 mL of H2PdCl4 was added under stirring. After stirring at room temperature for 10 h, NaBH4 (40 mg) was added and stirred for 1.5 h. The mixture was centrifuged (7000 r / min, 6 min). The mixture was washed with water and ethanol for 3 times, and dried at 50°C to obtain a comparative example 1 sample.

[0042] Figure 1 is the X-ray diffraction pattern of the sample prepared in comparative example 1, Figure 1 It can be seen that the diffraction peaks of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst correspond one to one with the standard card, indicating that no other impurities are produced, indicating that we have synthesized a relatively high relative proportion of crystallinity.

[0043] Figure 2 is the nitrogen adsorption-desorption curve of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Comparative Example 1, Figure 2 It can be seen that the material has a larger specific surface area and more active sites.

[0044] Figure 4 This is a formic acid decomposition activity diagram of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Comparative Example 1. It can be seen from the diagram that the material has a high formic acid decomposition catalytic activity.

[0045] Comparative Example 2

[0046] Add ZrCl4 (1.74g) and 2-aminoterephthalic acid (1.02g) to 180mL dimethylformamide solvent. After stirring for 15min, add concentrated hydrochloric acid (5.5ml) to obtain a mixed solution. Then transfer the obtained mixed solution to a Teflon stainless steel autoclave, heat it at 140℃ for 30h, centrifuge, dry and grind it in sequence to obtain a powder sample, the drying temperature is 80℃, and the time is 12h. Put 60mg of the above powder sample into a crucible and heat it to 700℃ at 3℃ / min in a nitrogen atmosphere, and keep it at this temperature for 7h, then cool it down at 3℃ / min to room temperature to obtain a precursor.

[0047] 100 mg of the precursor was mixed with 10 mL of deionized water, and then ultrasonically dispersed. 3 mL of H2PdCl4 was added under stirring. After stirring at room temperature for 10 h, NaBH4 (35 mg) was added and stirred for 2 h. The mixture was centrifuged (6000 r / min, 9 min). The mixture was washed with water and ethanol for 3 times, and dried at 50° C. to obtain Comparative Example 2.

[0048] Figure 1 is the X-ray diffraction pattern of the sample prepared in comparative example 2, Figure 1 It can be seen that the diffraction peaks of the advanced Pd-based heterostructure catalyst correspond one to one with the standard card, indicating that no other impurities are produced, indicating that we have synthesized a relatively high relative proportion of crystallinity.

[0049] Figure 3 is the nitrogen adsorption-desorption curve of the advanced Pd-based heterogeneous structure catalyst prepared in comparative example 2, Figure 2 It can be seen that the material has a larger specific surface area and more active sites.

[0050] Figure 5 This is a formic acid decomposition activity diagram of the advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared in Comparative Example 2. It can be seen from the diagram that the material has a high formic acid decomposition catalytic activity.

[0051] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an advanced Pd-based heterostructure formic acid dehydrogenation catalyst, characterized in that: include: 1) dissolving a soluble zirconium salt, 2-aminoterephthalic acid and concentrated hydrochloric acid in a diformamide solvent to obtain a mixed solution, wherein the molar ratio of the soluble zirconium salt to the 2-aminoterephthalic acid is 1:1-2; 2) The obtained mixed solution is charged into a reaction kettle for solvothermal reaction at a reaction temperature of 120° C. to 160° C. for a reaction time of 24 h to 36 h; 3) After the solvothermal reaction, centrifugation, drying, and grinding are performed in sequence to obtain a powder sample; 4) annealing the obtained powder sample in a nitrogen atmosphere at a temperature of 700°C to 1100°C for 5h to 7h, a heating rate of 3°C / min to 5°C / min, a cooling rate of 3°C / min to 5°C / min, lowering to room temperature, and grinding to obtain a precursor; 5) After mixing the obtained precursor with deionized water, palladium salt and NaBH4 are added, stirred evenly, centrifuged, dried, and ground in sequence to obtain an advanced Pd-based heterostructure formic acid dehydrogenation catalyst.

2. The method for preparing an advanced Pd-based heterostructure formic acid dehydrogenation catalyst according to claim 1, characterized in that: In step 1), the soluble zirconium salt is zirconium chloride, zirconium nitrate or zirconium sulfate.

3. The method for preparing an advanced Pd-based heterostructure formic acid dehydrogenation catalyst according to claim 1, characterized in that: In step 1), the volume of concentrated hydrochloric acid is 4 mL to 6 mL.

4. The method for preparing an advanced Pd-based heterostructure formic acid dehydrogenation catalyst according to claim 1, characterized in that: In step 3), the drying temperature is 60° C. to 80° C. and the drying time is 12 h to 18 h.

5. The method for preparing an advanced Pd-based heterostructure formic acid dehydrogenation catalyst according to claim 1, characterized in that: In step 5), the mass ratio of palladium salt to NaBH4 is 1:

1.

6. The method for preparing an advanced Pd-based heterostructure formic acid dehydrogenation catalyst according to claim 1, characterized in that: In step 5), the palladium salt is selected from H2PdCl4.

7. An advanced Pd-based heterostructure formic acid dehydrogenation catalyst prepared by the method for preparing an advanced Pd-based heterostructure formic acid dehydrogenation catalyst according to any one of claims 1 to 6, wherein the specific surface area of ​​the advanced Pd-based heterostructure formic acid dehydrogenation catalyst is 330 m 2 / g~480m 2 / g.

Citation Information

Patent Citations

  • Pd composite nano-catalyst for hydrogen production by formic acid decomposition and preparation method of Pd composite nano-catalyst

    CN110026236A

  • Cr-based MOF carbon material catalyst co-doped with loaded nano-palladium particles, preparation of Cr-based MOF carbon material catalyst and application of catalyst in hydrogen production from formic acid

    CN113731502A

  • Preparation method and application of superfine gold-palladium nanoparticle / nitrogen-doped porous carbon composite material

    CN114471659A

  • MOF-derived porous nitrogen-doped carbon-loaded Pd catalyst as well as preparation method and application thereof

    CN118281245A

  • Porous organometallic framework materials loaded with catalyst metal components

    WO2008129024A1