Preparation method of modified titanium-based metal oxide and application of modified titanium-based metal oxide as catalyst for removing CVOCs at low temperature

By doping ruthenium and transition metals with titanium-based metal oxide catalyst, the problem of insufficient removal efficiency and stability against chlorine poisoning in low temperature CVOCs is solved, and efficient catalytic oxidation performance and long-term stability are achieved, which is suitable for the treatment of CVOCs. .

CN118904335APending Publication Date: 2024-11-08ZHEJIANG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410972205.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove chlorine-containing volatile organic compounds (CVOCs) under low temperature conditions, and the catalyst is prone to inactivate due to chlorine poisoning, resulting in insufficient catalytic oxidation activity and anti-chlorine poisoning stability.

Method used

Using a modified titanium-based metal oxide catalyst, ruthenium is doped with transition metals (such as chromium, manganese, cobalt, and nickel) through the preparation method to form a catalyst with rich oxygen vacancies and excellent redox properties, which is used to remove CVOCs at low temperatures. The method includes mixing acetic acid, ethanol and tetrabutyl titanate at room temperature, adding transition metal nitrate to form a transparent gel, followed by calcining in an air atmosphere and treating with NaBH4 to improve catalyst performance.

Benefits of technology

The chlorobenzene removal efficiency of 90% at about 200°C and the stable catalytic oxidation conversion rate was maintained for a long time at 255°C, which significantly improved the anti-chlorination stability and low-temperature oxidation activity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904335A_ABST
    Figure CN118904335A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a modified titanium-based metal oxide and application of the modified titanium-based metal oxide as a catalyst for removing CVOCs at low temperature, a solution is heated and stirred under a water bath condition until transparent gel is formed, the transparent gel is transferred into a drying oven to be dried overnight, an obtained solid is transferred into a muffle furnace and calcined in an air atmosphere, and the modified titanium-based metal oxide is obtained. The transition metal doped titanium-based catalyst is obtained. Weighing RuCl3, dissolving the RuCl3 in water, and recording the solution as a solution D; and weighing a transition metal doped titanium catalyst, dispersing the transition metal doped titanium catalyst in the solution D, and stirring at room temperature. NaBH4 is weighed and dissolved in water, and a solution E is marked; under the stirring condition, the solution E is dropwise added into the solution D, stirring reaction is conducted at the room temperature, suction filtration and washing are conducted, an obtained solid is dried, and the modified titanium-based catalyst is obtained. The modified titanium-based catalyst has abundant oxygen vacancies and excellent oxidation-reduction performance, shows excellent catalytic performance in the process of treating CVOCs, and has wide application prospects in the field of CVOCs catalytic oxidation application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of CVOCs catalysts, and in particular to a preparation method of a modified titanium-based metal oxide and an application of the modified titanium-based metal oxide as a catalyst for removing CVOCs at low temperature. Background Art

[0002] Chlorinated Volatile Organic Compounds (CVOCs) refer to volatile organic compounds containing chlorine atoms, which easily evaporate into the air at room temperature. Common CVOCs include chlorobenzene, dichloromethane, vinyl chloride and chloroform. These compounds are widely used in industrial cleaning agents, solvents, refrigerants and chemical raw materials. Their high volatility and toxicity pose a serious threat to the environment and human health. CVOCs are persistent and bioaccumulative, and can easily exist in the environment for a long time and enter the body through water, soil and air. Exposure to CVOCs may lead to a variety of health problems.

[0003] For CVOCs catalytic oxidation technology, two aspects need to be considered: the low-temperature oxidation activity of the catalyst and the stability against chlorine poisoning. Titanium-based catalysts can dechlorinate through HCl by combining with dissociated chlorine in CVOCs through surface hydroxyl groups, thereby slowing down the phenomenon of catalyst deactivation due to chlorine poisoning and reducing the formation of chlorinated byproducts. Ruthenium, as a precious metal that is inexpensive compared to gold, platinum and palladium, has excellent low-temperature catalytic oxidation activity for CVOCs, and ruthenium has been shown to be dechlorinated through the Deacon reaction, which makes it stable against chlorine poisoning. Transition metals have variable valence states and good redox properties, which are very beneficial to the deep oxidation of CVOCs and can improve the selectivity of CO2. Modifying titanium-based catalysts with ruthenium and transition metals is expected to achieve both low-temperature oxidation activity and stability against chlorine poisoning in CVOCs treatment. Summary of the invention

[0004] The present invention provides a preparation method of a modified titanium-based metal oxide and its application as a catalyst for removing CVOCs at low temperature, which can be used as a high-performance modified titanium-based metal oxide catalyst for removing CVOCs at low temperature. The modified titanium-based catalyst has abundant oxygen vacancies and excellent redox properties, and exhibits excellent catalytic performance in the process of treating CVOCs (in 500ppm chlorobenzene, 10000mL g -1 h -1 Under the condition of , the catalyst can achieve a removal efficiency of 90% at about 200°C). In addition, the catalyst can maintain a stable chlorine-resistant catalyst oxidation conversion rate for a long time at 255°C, and has broad application prospects in the field of CVOCs catalytic oxidation applications.

[0005] The purpose of the present invention is to provide a preparation method and application of a modified titanium-based metal oxide catalyst for removing CVOCs at low temperature.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing a modified titanium-based metal oxide catalyst for removing CVOCs at low temperature comprises the following steps:

[0008] 1) Weigh acetic acid, ethanol and tetrabutyl titanate, mix them evenly, adjust the pH of the solution with nitric acid, record it as solution A, and adjust the pH of solution A with nitric acid; weigh ethanol, water and transition metal nitrate and mix them evenly to form solution B; slowly drop solution B into solution A, stir at room temperature for 1 hour to form solution C;

[0009] 2) Heat and stir solution C in a water bath at 70-90° C. (more preferably 80° C.) until a transparent gel is formed, transfer the solution to a drying oven and dry overnight, transfer the obtained solid to a muffle furnace, and calcine it in an air atmosphere for 4 hours to obtain a transition metal-doped titanium-based catalyst.

[0010] 3) Weigh RuCl3 and dissolve it in water, which is called solution D. Weigh a certain amount of transition metal-doped titanium catalyst and disperse it in solution D, and stir it at room temperature for 18 to 30 hours (more preferably 24 hours).

[0011] 4) Weigh NaBH4 and dissolve it in water, which is called solution E. Add solution E dropwise into solution D under stirring, and stir the mixture at room temperature for 2 to 4 hours (preferably 3 hours). Filter and wash the obtained solid, and dry it at 50 to 70°C (preferably 60°C). A modified titanium-based catalyst is obtained.

[0012] In step 1), the ratio of the amount of acetic acid, ethanol and tetrabutyl titanate is 1-3 ml: 23-43 ml: 0.012-0.036 mol. More preferably, the amount of acetic acid, ethanol and tetrabutyl titanate is 2 ml, 33 ml and 0.024 mol respectively.

[0013] In step 1), the pH of the solution is adjusted to 2 to 3 with nitric acid. The pH of the solution is adjusted to about 2.5 with nitric acid.

[0014] In step 2), the calcination conditions in air atmosphere are: calcination at a temperature of 450-550° C. at a heating rate of 1-5° C. / min in air atmosphere. More preferably, calcination at a temperature of 500° C. at a heating rate of 2° C. / min in air atmosphere in a muffle furnace.

[0015] In step 1), the molar ratio of metal nitrate to tetrabutyl titanate is 1:1-9.

[0016] In step 1), the molar ratio of transition metal nitrate to tetrabutyl titanate in the solution C is 1:1 to 9. The transition metal nitrate includes one of iron nitrate, cobalt nitrate, chromium nitrate, nickel nitrate and manganese nitrate.

[0017] In step 3), the mass ratio of Ru element to transition metal-doped titanium catalyst is 0.5 to 3:100 (more preferably 1:100).

[0018] In step 4), the ratio of the amount of NaBH4 to water is 0.1-0.5 g: 5-15 mL, and more preferably, the amount of NaBH4 to water is 0.25 g and 10 ml, respectively.

[0019] The modified titanium-based metal oxide low-temperature CVOCs removal catalyst prepared by the preparation method is used in removing CVOCs in tail gas from pharmaceutical, chemical and metal manufacturing industries.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] 1. This preparation method is a universal modified titanium-based preparation method, which can be used to prepare catalysts such as Ru / TiCo, Ru / TiMn and Ru / TiNi.

[0022] 2. The modified titanium-based metal oxide catalyst prepared by this method has the advantages of abundant oxygen vacancies and uniform dispersion of metal elements, thus showing excellent low-temperature CVOCs catalytic oxidation activity; in addition, the catalyst prepared by this method has good stability against chlorine poisoning. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 XRD results of chromium-modified titanium-based catalyst.

[0024] Figure 2 TEM image of chromium-modified titanium-based catalyst.

[0025] Figure 3 Mapping results for chromium-modified titanium-based catalysts.

[0026] Figure 4 These are the EPR results of chromium-modified titanium-based catalysts.

[0027] Figure 5 The results of catalytic oxidation of CVOCs on titanium-based catalysts modified with ruthenium and different proportions of chromium.

[0028] Figure 6 The results of catalytic oxidation of CVOCs by ruthenium and different transition metal doped modified titanium-based catalysts.

[0029] Figure 7These are the test results of the stability of Ru / Cr2Ti8 catalyst in catalytic oxidation of CVOCs against chlorine. DETAILED DESCRIPTION

[0030] Example 1. Preparation of Ru / Cr1Ti9 catalyst

[0031] Take 2ml acetic acid, 33ml ethanol and 0.024mol tetrabutyl titanate, mix them evenly, adjust the pH of the solution to 2.5 with nitric acid, and record it as solution A; take 16ml ethanol, 2ml water and 0.00027mol Cr(NO3)3·9H2O and mix them evenly to form solution B; slowly add solution B to solution A and stir at room temperature for 1 hour to form solution C; heat and stir solution C in a water bath at 80℃ until a transparent gel is formed, transfer it to a drying oven and dry it overnight, move the obtained solid to a muffle furnace, and heat it to 500℃ in an air atmosphere at a heating rate of 2℃ / min for 4 hours to obtain a chromium-doped titanium-based catalyst. Weigh RuCl3 (the loading amount of Ru element is 1wt / %) and dissolve it in water, record it as solution D. Weigh 0.7g chromium-doped titanium catalyst and disperse it in solution D, and stir it at room temperature for 24h. Weigh 0.25g NaBH4 and dissolve it in 10ml water, record it as solution E. Under stirring conditions, solution E was added dropwise to solution D, and the mixture was stirred at room temperature for 3 h. The solid obtained by suction filtration and washing was dried at 60°C to obtain a Ru / Cr1Ti9 catalyst.

[0032] Example 2. Preparation of Ru / Cr2Ti8 catalyst

[0033] Take 2ml acetic acid, 33ml ethanol and 0.024mol tetrabutyl titanate, mix them evenly, adjust the pH of the solution to 2.5 with nitric acid, and record it as solution A; take 16ml ethanol, 2ml water and 0.006mol Cr(NO3)3·9H2O and mix them evenly to form solution B; slowly add solution B to solution A and stir at room temperature for 1 hour to form solution C; heat and stir solution C in a water bath at 80℃ until a transparent gel is formed, transfer it to a drying oven and dry it overnight, move the obtained solid to a muffle furnace, and heat it to 500℃ at a heating rate of 2℃ / min in an air atmosphere and calcine it for 4 hours to obtain a chromium-doped titanium-based catalyst. Weigh RuCl3 (the loading amount of Ru element is 1wt / %) and dissolve it in water, record it as solution D. Weigh 0.7g chromium-doped titanium catalyst and disperse it in solution D, and stir it at room temperature for 24h. Weigh 0.25g NaBH4 and dissolve it in 10ml water, record it as solution E. Under stirring conditions, solution E was added dropwise to solution D, and the mixture was stirred at room temperature for 3 h. The solid obtained by suction filtration and washing was dried at 60° C. A Ru / Cr2Ti8 catalyst was obtained.

[0034] Example 3. Preparation of Ru / Cr4Ti6 Catalyst

[0035] Take 2ml acetic acid, 33ml ethanol and 0.024mol tetrabutyl titanate, mix them evenly, adjust the pH of the solution to 2.5 with nitric acid, and record it as solution A; take 16ml ethanol, 2ml water and 0.016mol Cr(NO3)3·9H2O and mix them evenly to form solution B; slowly add solution B to solution A and stir at room temperature for 1 hour to form solution C; heat and stir solution C in a water bath at 80℃ until a transparent gel is formed, transfer it to a drying oven and dry it overnight, move the obtained solid to a muffle furnace, and heat it to 500℃ in an air atmosphere at a heating rate of 2℃ / min for 4 hours to obtain a chromium-doped titanium-based catalyst. Weigh RuCl3 (the loading amount of Ru element is 1wt / %) and dissolve it in water, record it as solution D. Weigh 0.7g chromium-doped titanium catalyst and disperse it in solution D, and stir it at room temperature for 24h. Weigh 0.25g NaBH4 and dissolve it in 10ml water, record it as solution E. Under stirring conditions, solution E was added dropwise to solution D, and the mixture was stirred at room temperature for 3 h. The solid obtained by suction filtration and washing was dried at 60°C to obtain a Ru / Cr4Ti6 catalyst.

[0036] Example 4. Preparation of Ru / Mn1Ti9 Catalyst

[0037] The chromium nitrate nonahydrate weighed in Example 1 was replaced by 0.0027 mol of manganese nitrate tetrahydrate, and the other conditions remained unchanged to obtain a Ru / Mn1Ti9 sample.

[0038] Example 5. Preparation of Ru / Co1Ti9 Catalyst

[0039] The chromium nitrate nonahydrate weighed in Example 1 was replaced by 0.0027 mol of cobalt nitrate hexahydrate, and the other conditions remained unchanged to obtain a Ru / Co1Ti9 sample.

[0040] Example 6. Preparation of Ru / Ni1Ti9 Catalyst

[0041] The chromium nitrate nonahydrate weighed in Example 1 was replaced by 0.0027 mol of nickel nitrate hexahydrate, and the other conditions remained unchanged to obtain a Ru / Ni1Ti9 sample.

[0042] Example 7. Preparation of Ru / Fe1Ti9 Catalyst

[0043] The chromium nitrate nonahydrate weighed in Example 1 was replaced by 0.0027 mol of ferric nitrate nonahydrate, and the other conditions remained unchanged to obtain a Ru / Fe1Ti9 sample.

[0044] In Examples 1, 2 and 3, the XRD results of the ruthenium-chromium modified titanium-based catalysts are as follows: Figure 1As shown, the synthesized catalyst contains diffraction peaks of rutile phase titanium dioxide and chromium oxide. As the chromium doping amount increases, the intensity of the catalyst characteristic diffraction peak decreases.

[0045] In Example 2, the TEM results of the ruthenium-chromium modified titanium-based catalyst are as follows: Figure 2 As shown, the synthesized catalyst presents a sheet-like structure of stacked nanoparticles.

[0046] In Example 2, the EDS results of the ruthenium-chromium modified titanium-based catalyst are as follows: Figure 3 As shown in the figure, it can be seen that the three metal elements Cr, Ru and Ti of the catalyst are evenly dispersed, which is conducive to the synergistic effect between the metals.

[0047] In Example 2, the ruthenium-chromium modified titanium-based catalyst EPR is as follows Figure 4 As shown in the figure, it can be seen that the oxygen vacancy concentration of the catalyst is significantly increased after Ru loading and Cr doping modification.

[0048] Example 8: Evaluation of the performance of modified titanium-based catalysts in catalyzing CVOCs

[0049] The catalysts prepared in Examples 1, 2, 3, 4, 5, 6, and 7 were applied to the catalytic oxidation reaction of CVOCs, and all showed good catalytic activity. The chlorobenzene removal efficiency of the catalysts prepared in Examples 1, 2, and 3 was as follows: Figure 5 As shown, the chlorobenzene removal efficiency of the catalysts prepared in Examples 4, 5, 6, and 7 is as follows Figure 6 As shown, the stability test of the catalyst prepared in Example 2 is as follows Figure 6 As shown. The reaction was carried out on a CVOCs catalytic oxidation evaluation device. The catalyst evaluation device mainly consists of four parts: gas pipeline, fixed bed reactor, flow control system and gas detection system. During the experiment, a mass flow meter was used to achieve precise control of each gas. A quartz tube with an outer diameter of 10 mm and an inner diameter of 6 mm was used as a catalytic reactor. The reactor was heated by a resistance furnace, and the temperature in the reactor was monitored by a K-type thermocouple. The total flow rate of the mixed gas was 50 mL·min-1, of which the volume fraction of O2 was 21%. During the experiment, the catalyst loading was 300 mg, the particle size was 40-60 mesh, and the corresponding mass space velocity (WHSV) was 10000 mL·(g·h) -1 .

Claims

1. A method for preparing a modified titanium-based metal oxide, characterized in that: The following steps are involved: 1) Weigh acetic acid, ethanol and tetrabutyl titanate, mix them evenly, and adjust the pH of the solution with nitric acid, which is recorded as solution A; Weigh ethanol, water and transition metal nitrate and mix them evenly to form solution B; Add solution B dropwise to solution A and stir to form solution C; 2) heating and stirring the solution C in a water bath at 70-90° C. until a transparent gel is formed, drying to obtain a solid, and calcining the solid in an air atmosphere to obtain a transition metal-doped titanium-based catalyst; 3) Weigh RuCl3 and dissolve it in water, record it as solution D, weigh the transition metal-doped titanium-based catalyst and disperse it in solution D, stir for 18 to 30 hours, and obtain a stirred solution D; 4) Weigh NaBH4 and dissolve it in water, record it as solution E, add solution E dropwise into the stirred solution D under stirring, stir and react for 2 to 4 hours, filter and wash the obtained solid, and dry it at 50 to 70° C. to obtain a modified titanium-based metal oxide.

2. The method for preparing the modified titanium-based metal oxide according to claim 1, characterized in that: In step 1), the ratio of the amount of acetic acid, ethanol and tetrabutyl titanate is 1-3 ml: 23-43 ml: 0.012-0.036 mol.

3. The method for preparing the modified titanium-based metal oxide according to claim 1, characterized in that: In step 1), the pH of the solution is adjusted to 2-3 with nitric acid.

4. The method for preparing the modified titanium-based metal oxide according to claim 1, characterized in that: In step 2), the calcination conditions in air atmosphere are: heating the temperature to 450-550° C. at a heating rate of 1-5° C. / min in air atmosphere.

5. The method for preparing the modified titanium-based metal oxide according to claim 1, characterized in that: In step 1), the molar ratio of transition metal nitrate to tetrabutyl titanate in the solution C is 1:1-9.

6. The method for preparing the modified titanium-based metal oxide according to claim 1, characterized in that: In step 1), the transition metal nitrate is one or more of iron nitrate, cobalt nitrate, chromium nitrate, nickel nitrate and manganese nitrate.

7. The method for preparing the modified titanium-based metal oxide according to claim 1, characterized in that: In step 3), the mass ratio of Ru element to transition metal-doped titanium-based catalyst is 0.5 to 3:

100.

8. The method for preparing the modified titanium-based metal oxide according to claim 1, characterized in that: In step 4), the ratio of the amount of NaBH4 to water is 0.1-0.5 g: 5-15 mL.

9. Use of the modified titanium-based metal oxide prepared by the preparation method according to any one of claims 1 to 8 as a catalyst for removing CVOCs at low temperature.

10. The use according to claim 9, characterized in that Specifically include: Modified titanium-based metal oxides are used as low-temperature CVOCs removal catalysts for CVOCs catalytic oxidation reactions to remove CVOCs from tail gases in pharmaceutical, chemical, and metal manufacturing industries.

Citation Information

Patent Citations

  • Third main group element modified ruthenium titanium compound oxide and preparation method and application thereof

    CN109939677A

  • Supported titanium-based metal oxide catalyst as well as preparation method and application thereof

    CN117431580A

  • Preparation method and application of Ru monatomic noble metal type catalyst RuCeTi

    CN118179502A