MnFe foam metal composite material and preparation method and application thereof
By loading MnFe oxide on the foam metal and combining with the skirting line heater, a self-driven air purification electric heater is formed, which solves the problem of limited removal of complex pollutants in the room and achieves efficient coordinated control of pollutants removal and heating .
Patent Information
- Application Number
- CN202410932741.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art has limited effect in removing complex indoor pollutant gases, and the preparation methods of common air purifiers are cumbersome, making it difficult to effectively solve the problem of indoor pollution in winter.
Using MnFe@ foam metal composite material, the MnFe oxide is loaded on the foam metal, and the chemical bonds and magnetic field anchoring is used to form a self-driven air purification electric heater, and the heating pipe is used to generate Joule heat to provide catalysis. Reaction temperature to achieve the removal of indoor organic pollutants.
It has achieved efficient removal of key indoor pollutants, improved the coordinated control of indoor heating and air pollution in winter, and provided a simple and effective preparation method.
Smart Images

Figure CN118904351A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a MnFe@foam metal composite material and a preparation method and application thereof. Background Art
[0002] In winter, people usually close doors and windows to reduce indoor heat loss. However, this will lead to a large accumulation of indoor air pollutants. Indoor pollution has become a major threat to people's healthy home life. The purification principle of common air purifiers is to remove PM2.5 and germs through adsorption filtration, and to remove formaldehyde through photocatalyst technology. However, these two methods are very limited in their effectiveness in removing complex indoor pollutant gases.
[0003] Patent CN 101298024 B provides a catalyst for purifying volatile organic pollutants and ozone in the air at room temperature, and its preparation method and application. Ozone is catalytically decomposed at room temperature to generate highly active oxygen atoms that further oxidize volatile organic pollutants in the air, and finally generate carbon dioxide and water. The catalyst uses three-dimensional porous metal as a carrier, activated carbon, silicon oxide, aluminum oxide and their composite materials as a coating, and transition metal oxides of Mn, Cu, Fe, Ni, and Co as active components. Even if the invention can remove organic pollutants and ozone at room temperature at the same time without heating, the method for preparing the catalyst is too complicated and still needs to be improved.
[0004] The art is in urgent need of a composite material that has a simple preparation method and can be used to remove indoor pollutants in winter. Summary of the invention
[0005] The purpose of the present invention is to provide a MnFe@foam metal composite material and a preparation method and application thereof, so as to improve the problem of coordinated control of indoor heating and indoor air pollution in winter.
[0006] One of the technical solutions provided by the present invention:
[0007] A MnFe@ foam metal composite material, manganese and iron elements in the form of MnFe oxide (MnFeO x ) in the form of being loaded on the foam metal, wherein the molar ratio of the manganese element to the iron element is 5:1, and the MnFeO in the MnFe@ foam metal composite material x The loading amount is 0.1-0.5wt%.
[0008] The second technical solution provided by the present invention is:
[0009] A preparation method of the above-mentioned MnFe@foam metal composite material comprises the following steps: using an acidic solution of hydrogen peroxide as solution A and a mixed aqueous solution of KMnO4 and Fe(NO3)3 as solution B, adding the solution A dropwise into the solution B, filtering and washing to obtain a MnFe suspension, soaking a foamed metal in the MnFe suspension, taking it out, drying it, and calcining it to obtain the MnFe@foam metal composite material.
[0010] Preferably, the foam metal is selected from foam aluminum, foam stainless steel or foam copper, preferably foam nickel.
[0011] Taking nickel foam as an example, the MnFe suspension is adsorbed on the surface of nickel foam under the capillary action of the main structure of nickel foam, and the MnFe suspension is calcined to form MnFeO X (MnFe oxide) and form Mn-O-Ni bond or Fe-O-Ni bond with the carrier nickel foam to anchor on the nickel foam carrier. In addition, the calcined MFeO x It can also be anchored on a nickel foam carrier through a magnetic field.
[0012] Preferably, the molar ratio of KMnO4 to Fe(NO3)3 in the B solution is 5:1.
[0013] Preferably, the acid in solution A includes HNO3, H2SO4, H3PO4 or HClO4.
[0014] More preferably, the mass concentration of H2O2 in the A solution is 2.9wt.%, and the mass concentration of acid is 0.42-0.67wt.%.
[0015] The reaction process and product equations of KMnO4, Fe(NO3)3 and hydrogen peroxide acid solution are shown in equations (1)-(3):
[0016]
[0017] When every 20g KMnO4 participates in the reaction, if the concentration of hydrogen peroxide in solution A is lower than 2.9wt.% or the concentration of nitric acid is lower than 0.67wt.%, the reaction equation shown in formula (1) will not proceed sufficiently, the amount of MnO2 generated will be insufficient, and finally the molar ratio of Mn:Fe will be less than 5:1. MnFeO x In the reaction, Mn serves as the reaction site for adsorbing and activating organic pollutants, while Fe serves as the active site for adsorbing and activating oxygen. When the molar ratio of Mn:Fe is less than 5:1, there are fewer active sites for adsorbing and activating organic pollutants, and the reaction rate decreases; when the molar ratio of Mn:Fe is greater than 5:1, there are fewer active sites for adsorbing and activating oxygen, and the reaction rate decreases.
[0018] Preferably, the soaking temperature is 25°C and the soaking time is 1-5 min.
[0019] Preferably, the drying temperature is 30-150° C. and the drying time is 1-24 h.
[0020] More preferably, the drying temperature is 100° C. and the drying time is 12 hours.
[0021] Preferably, the calcination temperature is 200-600° C. and the calcination time is 1-24 h.
[0022] More preferably, the calcination temperature is 400° C. and the calcination time is 2.5 h.
[0023] The third technical solution provided by the present invention is:
[0024] An application of the MnFe@foam metal composite material in removing indoor organic pollutants, wherein the indoor organic pollutants include toluene, formaldehyde, xylene and ethylbenzene.
[0025] The fourth technical solution provided by the present invention is:
[0026] A self-driven air-purifying electric heater is prepared by combining a skirting heater and the above-mentioned MnFe@foam metal composite material, wherein the MnFe@foam metal composite material is located above the heating tube of the skirting heater.
[0027] Preferably, the skirting heater is selected from a small sun heater, an oil-filled heater, a fan heater or a radiator.
[0028] The fifth technical solution provided by the present invention is:
[0029] An application of the self-driven air-purifying electric heater in removing indoor organic pollutants, wherein the volatile organic pollutants include toluene, formaldehyde, xylene and ethylbenzene.
[0030] Technical principle of the present invention:
[0031] In the field of gas phase organic pollutant removal, manganese-based materials are increasingly attracting attention due to their unique physical and chemical properties. Layered manganese dioxide (i.e. birnessite) has excellent performance in catalytic oxidation of organic matter and is a very promising purification material for removing indoor organic pollutants. The MnFe copolymerization precipitation method can achieve the increase of lattice defects, oxygen vacancies and specific surface area on the surface of birnessite. 3+ With the increase of the content, there are a large number of unsaturated oxygen atoms and manganese atoms on the catalyst surface, which is conducive to the adsorption and activation of organic pollutant molecules and oxygen molecules on the surface. xProviding the temperature required for catalytic reaction and removing indoor organic pollutants. The heating tube inside the skirting heater has a large resistance, and a large amount of Joule heat is generated after the current passes through. The fins connected to the heating tube play a role in enhancing heat transfer, which provides the temperature required for the catalytic reaction of the MnFe catalyst. At the same time, after being heated, the cold air around the heating tube and the fins becomes less dense and tends to move vertically upward, which provides a mass transfer driving force for the air purification unit.
[0032] Compared with the prior art, the present invention has the following advantages and technical effects:
[0033] The present invention provides a method for preparing a MnFe@foam metal composite material, in which MnFe oxide is loaded on a foam metal through chemical bonds and magnetic field anchoring. The composite material, as a new type of integral catalyst, has excellent low-temperature catalytic activity and stability. The present invention combines the new type of integral catalyst with a skirting heater to obtain a self-driven air purification type electric heater. During the heating and heat dissipation process, the current passes through the heating tube to generate a large amount of Joule heat. The fins connected to the heating tube play a role in enhancing heat transfer, providing the temperature required for the catalytic reaction for the MnFe@foam metal composite material, thereby achieving the removal of indoor pollutants in winter and improving the coordinated control of indoor heating and indoor air pollution in winter. The present invention can achieve MnFeO X It has high efficiency and uniform loading and excellent performance in removing key indoor pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0035] Figure 1 This is a schematic diagram of the reaction principle for preparing the MnFe@foam metal composite material according to the present invention;
[0036] Figure 2 is a scanning electron microscope image of the blank nickel foam in Example 1;
[0037] Figure 3 This is a scanning electron microscope image of the MnFe@nickel foam composite material prepared in Example 1;
[0038] Figure 4 This is the Raman spectrum of the MnFe@nickel foam composite material prepared in Example 1;
[0039] Figure 5Schematic diagram of the structure of the self-driven air-purifying electric heater of Example 1, wherein 1 is a protective cover, 2 is a metal shell, 3 is a MnFe@nickel foam monolithic catalyst, 4 is a heating fin, 5 is a heating tube, and 6 is a support leg;
[0040] Figure 6 This is a 60-hour toluene degradation stability diagram of the self-driven air-purifying electric heater of Example 1 in a pilot scenario;
[0041] Figure 7 This is a diagram showing the degradation effects of formaldehyde, benzene, toluene, xylene and ethylbenzene in the pilot scenario for 300 hours for the self-driven air-purifying electric heater of Example 1;
[0042] Figure 8 This is a graph showing the degradation effects of toluene, formaldehyde, xylene and ethylbenzene in the pilot scenario for 300 hours for the self-driven air purification electric heater of Comparative Example 2;
[0043] Fig. 9 This is a diagram showing the degradation effects of benzene, toluene, formaldehyde, xylene and ethylbenzene in the pilot scenario for 300 hours using the self-driven air-purifying electric heater of Example 2. DETAILED DESCRIPTION
[0044] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0045] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0046] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0047] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0048] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0049] The embodiment of the present invention provides a preparation method of a MnFe@nickel foam composite material, comprising the following steps: S10. adding an appropriate amount of acid to diluted H2O2, and then dripping it dropwise into a mixed solution of KMnO4 and Fe(NO3)3 to obtain a MnFe suspension; S20. the MnFe suspension is filtered and washed several times and then dispersed into deionized water, and then the foam metal is immersed in the MnFe suspension and taken out after being fully absorbed; S30. the nickel foam fully absorbed by the MnFe suspension is dried and calcined in an air atmosphere to obtain the MnFe@nickel foam composite material. Figure 1 This is a schematic diagram of the reaction principle for preparing the MnFe@foam metal composite material of the present invention.
[0050] In the embodiment of the present invention, the acid in S10 is selected from one or more of HNO3, H2SO4, H3PO4 or HClO4.
[0051] In the embodiment of the present invention, the drying temperature in S30 is 30-150°C, the drying time is 1-24h, the calcination temperature is 200-600°C, and the calcination time is 1-24h. In some preferred embodiments, the drying temperature is 100°C, the drying time is 12h, the calcination temperature is 400°C, and the calcination time is 2.5h.
[0052] The embodiment of the present invention also provides a self-driven air purification electric heater, which is prepared by combining a skirting heater and the above-mentioned MnFe@nickel foam composite material, wherein the MnFe@nickel foam composite material is located above the heating pipe of the skirting heater. Preferably, the skirting heater is selected from a small sun heater, an oil-filled heater, a heater or a radiator.
[0053] Example 1 Preparation method of MnFe@nickel foam composite material
[0054] S1. First, 64.6 g of 30 wt.% H2O2 solution was diluted in 600 mL of deionized water, and then 3.2 mL of 65 wt.% HNO3 was added, stirred and recorded as solution A (i.e., the mass concentration of H2O2 in solution A was 2.9 wt.%, and the mass concentration of HNO3 was 0.67 wt.%); 20 g (0.126 mol) of KMnO4 and 10.2 g (0.025 mol) of Fe(NO3)3·9H2O were dissolved in 600 mL of deionized water, recorded as solution B;
[0055] S2. Add solution A drop by drop into solution B, stir vigorously, react for 6 hours, filter and wash the obtained suspension with deionized water three times to prepare MnFe oxide, disperse MnFe oxide in 500mL deionized water to obtain suspension of MnFe oxide, immerse 50g carrier blank nickel foam in the suspension, dry at 100℃ for 12h, and calcine at 400℃ for 2.5h to obtain MnFe@nickel foam composite material. The ratio of the number of Mn and Fe atoms in the composite material is 5:1, and the loading amount of MnFe oxide (MnFeOx) is about 0.5wt.% (loading amount = (mass of MnFe@nickel foam composite material - mass of blank nickel foam) / mass of blank nickel foam * 100).
[0056] Figure 2 is a scanning electron microscope image of the blank nickel foam of this embodiment, Figure 2 It can be seen that its surface is relatively flat. Figure 3 This is a scanning electron microscope image of the MnFe@nickel foam composite material prepared in this example. It can be seen that the surface of the nickel foam carrier is loaded with a catalyst.
[0057] The MnFe@nickel foam composite material prepared in Example 1 was subjected to Raman spectroscopy, and the structure was determined as shown in FIG. Figure 4 The characterization results show that the MnFe@nickel foam composite material is loaded with MnFe oxide (MnFeO x ), instead of MnO2 and Fe2O3.
[0058] The MnFe@nickel foam composite material prepared in Example 1 is placed on the fins of the skirting heater to obtain a self-driven air purification electric heater, the structural schematic diagram of which is shown in FIG. Figure 5 As shown, 1 is a protective cover, 2 is a metal shell, 3 is a MnFe@nickel foam monolithic catalyst, 4 is a heating fin, 5 is a heating tube, and 6 is a support leg. The self-driven air purification electric heater is used for the coordinated control of indoor air pollutants and indoor temperature in winter, so as to achieve the removal of indoor organic pollutants.
[0059] The self-driven air purification electric heater prepared in this embodiment was tested for its pilot activity: the self-driven air purification electric heater prepared in this embodiment and a separate baseboard heater were used to evaluate the removal of organic pollutants in a room that had been newly renovated for three months. The evaluation results are as follows: Figure 6 The 60h toluene degradation stability of the self-driven air purification electric heater of Example 1 in the pilot scenario is shown in the figure. Figure 6 It can be seen that when the self-driven air purification electric heater prepared in this embodiment is used, after 60 hours of heating, the indoor toluene reaches the national standard of 200 μg / m 3 , proving that the MnFe@nickel foam composite material has good toluene removal performance (i.e. Figure 6 In the non-heating state, even if the self-driven air purification electric heater is combined with MnFe@ nickel foam composite material, after 60 hours, toluene cannot reach the recommended value of less than 200ug / m in the national standard "Indoor Air Quality Standard" (GB / T18883-2022). 3 (Right now Figure 6 When a separate baseboard heater is used, the indoor toluene concentration cannot reach the recommended value of less than 200ug / m in the national standard "Indoor Air Quality Standard" (GB / T18883-2022) after 60 hours under heating. 3 (Right now Figure 6 No catalyst was added).
[0060] Figure 7 The degradation effect diagram of the self-driven air purification electric heater of Example 1 on formaldehyde, benzene, toluene, xylene and ethylbenzene in the pilot scene for 60 hours is shown in FIG. Figure 7 It can be seen that when the catalyst is added to the baseboard heater, after 60 hours of removal, formaldehyde and toluene will reach a level suitable for human habitation. After 300 hours of removal, the total amount of xylene and ethylbenzene will also reach an acceptable level for the human body, but due to its relatively stable structure, the concentration of benzene in the air is still high after 300 hours, and it still takes longer to remove.
[0061] Example 2 Preparation method of MnFe@nickel foam composite material
[0062] S1. Dilute 64.6 g of 30 wt.% H2O2 in 600 mL of deionized water, add 1.4 mL of 98 wt.% H2SO4 (the mass concentration of H2O2 is 2.9 wt.%, and the mass concentration of H2SO4 is 0.42 wt.%), stir evenly and record it as solution A, dissolve 20 g (0.126 mol) of KMnO4 and 10.2 g (0.025 mol) of Fe(NO3)3·9H2O in 600 mL of deionized water and record it as solution B;
[0063] S2. Solution A was dripped into solution B drop by drop, and stirred vigorously. The reaction was carried out for 12 hours. The obtained suspension was filtered and washed three times with deionized water to prepare MnFe oxide. The MnFe oxide was then dispersed in deionized water to obtain a suspension. Then 50g of carrier blank nickel foam was immersed in the suspension, dried at 150°C for 8 hours and then calcined at 360°C for 5 hours to obtain a MnFe@nickel foam composite material. The ratio of the number of Mn and Fe atoms in the composite material was 5:1, and the loading amount of MnFe oxide was about 0.1wt.%. It can be seen that changing the type of acid used, the calcination temperature and the calcination time will not change the ratio of the number of Mn and Fe atoms. The reason is that the self-driven redox reaction is mainly subject to the influence of KMnO4, H2O2 and H + The amount of addition does not depend on the calcination time.
[0064] The self-driven air purification electric heater prepared in this embodiment was tested for its pilot activity: The self-driven air purification electric heater prepared in this embodiment was used to evaluate the removal of organic pollutants in a room that had been newly renovated for three months. The evaluation results are as follows: Fig. 9 The degradation stability diagram of benzene, toluene, xylene and ethylbenzene for 60 hours in the pilot scene of the self-driven air purification electric heater prepared in Example 2 is shown in FIG. Fig. 9 It can be seen that: compared with Example 1, although the MnFe oxide loading in the product prepared in this example is less, it still shows a good catalytic purification effect. This can be attributed to the excessive loading of MnFe oxide in Example 1, and the organic pollutants in the air can only diffuse to the surface of the catalyst layer.
[0065] Comparative Example 1
[0066] S1. First, 64.6g of 30wt.% H2O2 solution was diluted in 600mL of deionized water, and then 0mL65wt.% HNO3 was added, stirred and recorded as solution A (the mass concentration of H2O2 was 2.9wt.%); 20g (0.126mol) KMnO4 and 10.2g (0.025mol) Fe(NO3)3·9H2O were dissolved in 600mL of deionized water, recorded as solution B;
[0067] S2. Add solution A drop by drop into solution B, stir vigorously, react for 6 hours, filter and wash the obtained suspension three times with deionized water, and then disperse it in 500mL deionized water to obtain MnFe suspension, then immerse 50g of carrier blank nickel foam in the suspension, dry it at 100℃ for 12h, and then calcine it at 400℃ for 2.5h to obtain MnFe@nickel foam composite material. The ratio of Mn to Fe atoms in the composite material is 3:1, and the loading amount of MnFe oxide (MnFeOx) is about 0.4wt.%, which shows that when nitric acid is not added to solution A, the ratio of Mn to Fe atoms in the composite material will be changed. The reason is that 0.025mlFe 3+ The H+ produced by hydrolysis is not enough to provide the H required for the reaction of KMnO4 and H2O2. + , so that when the Mn:Fe atomic ratio reaches 3:1, it cannot proceed.
[0068] Comparative Example 2
[0069] S1. First, 64.6 g of 30 wt.% H2O2 was diluted in 600 mL of deionized water, stirred and recorded as solution A (the mass concentration of H2O2 was 2.9 wt.%), and 20 g (0.126 mol) of KMnO4 and 10.2 g (0.025 mol) of Fe(NO3)3·9H2O were dissolved in 600 mL of deionized water, recorded as solution B;
[0070] S2. Solution A was dripped into solution B drop by drop, and stirred vigorously, and the reaction was carried out for 12 hours. The obtained suspension was filtered and washed three times with deionized water, and then dispersed in 500 mL of deionized water to obtain a suspension. Then 50 g of carrier blank nickel foam was immersed in the suspension, dried at 80° C. for 24 h, and then calcined at 600° C. for 1 h to obtain a MnFe@nickel foam composite material. The ratio of the number of Mn and Fe atoms in the composite material was 3:1, and the loading amount of MnFe oxide was about 0.6 wt.%. The difference between Comparative Example 2 and Comparative Example 1 is that the calcination temperature is different, which proves that increasing the calcination temperature will increase the loading amount of MnFe oxide.
[0071] The self-driven air purification electric heater prepared in this comparative example was tested for its pilot activity: The self-driven air purification electric heater prepared in this comparative example was used to evaluate the removal of organic pollutants in a room that had been newly renovated for three months. The evaluation results are as follows: Figure 8 The self-driven air purification electric heater prepared in Comparative Example 2 has a 60h degradation stability of benzene, toluene, xylene and ethylbenzene in the pilot scenario. Figure 8It can be seen that due to the decrease in the Mn:Fe atomic ratio, even though the loading amount was increased from 0.5% to 0.6%, the activity of MnFe@nickel foam was lower than that of Example 1, which was attributed to the reduction in the number of Mn atoms, resulting in a decrease in the catalytic active sites for toluene.
[0072] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A MnFe@ foam metal composite material, characterized in that: Manganese and iron are present as MnFe oxide MnFeO x The MnFe@foam metal composite material is loaded on the foam metal in the form of x The loading amount is 0.1-0.5wt%.
2. A method for preparing the MnFe@ foam metal composite material according to claim 1, characterized in that: The following steps are involved: An acidic solution of hydrogen peroxide is used as solution A, and a mixed aqueous solution of KMnO4 and Fe(NO3)3 is used as solution B. The solution A is added dropwise into the solution B, and a MnFe suspension is obtained after filtration and washing. The foamed metal is immersed in the MnFe suspension, taken out, dried, and calcined to obtain the MnFe@foamed metal composite material.
3. The method for preparing the MnFe@ foam metal composite material according to claim 2, characterized in that: The molar ratio of KMnO4 to Fe(NO3)3 in the B solution is 5:
1.
4. The method for preparing the MnFe@ foam metal composite material according to claim 2, characterized in that: The acid in the solution A includes HNO3, H2SO4, H3PO4 or HClO4.
5. The method for preparing the MnFe@ foam metal composite material according to claim 4, characterized in that: The mass concentration of H2O2 in the solution A is 2.9wt.%, and the mass concentration of acid is 0.42-0.67wt.%.
6. The method for preparing the MnFe@ foam metal composite material according to claim 2, characterized in that: The drying temperature is 30-150° C. and the drying time is 1-24 hours.
7. The method for preparing the MnFe@ foam metal composite material according to claim 2, characterized in that: The calcination temperature is 200-600° C. and the calcination time is 1-24 hours.
8. Use of the MnFe@ foam metal composite material according to claim 1 in removing indoor organic pollutants, characterized in that: The indoor organic pollutants include one or more of toluene, formaldehyde, xylene and ethylbenzene.
9. A self-driven air-purifying electric heater, characterized in that: The baseboard heater is prepared by combining a baseboard heater and the MnFe@foam metal composite material according to claim 1, wherein the MnFe@foam metal composite material is located above the heating pipe of the baseboard heater.
10. Use of the self-driven air-purifying electric heater according to claim 9 in removing indoor organic pollutants, characterized in that: The indoor organic pollutants include one or more of toluene, formaldehyde, xylene and ethylbenzene.
Citation Information
Patent Citations
Catalyst for purifying volatile organic pollutant and ozone in air under normal temperature as well as preparation and use thereof
CN101298024A
Ozonolysis catalyst and preparation method thereof
CN101757933A
Manganese-iron composite oxide supported catalyst for removing ozone in indoor air
CN103084184A
Bimetallic oxide prepared through redox-hydrolysis coupling reaction and used for low-temperature catalytic combustion reaction of VOCs
CN107999085A
Preparation method and application of bimetallic oxide modified foamed nickel composite electrode
CN113060800A