Preparation method and application of Al-based catalyst
By controlling the preparation process of Al-based catalysts, catalysts rich in AlF2(OH) phase were prepared, solving the problem of difficulty in controlling the strength of Lewis acid sites and achieving high efficiency, stability and low carbon deposition characteristics in the R152a defluorination reaction.
Patent Information
- Application Number
- CN202410914166.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing Al-based catalysts used in the catalytic defluorination of R152a, the strength of the Lewis acid sites is difficult to control, leading to carbon deposition and catalyst deactivation, which affects the reaction efficiency.
An Al-based catalyst rich in AlF2(OH) phase was prepared by mixing an aluminum precursor and an alkaline precipitant to control the pH value, and then reacting it with hydrofluoric acid. The catalyst with moderate Lewis acid strength was obtained by filtration, washing and calcination.
The prepared Al-based catalyst exhibits moderate Lewis acid strength, reduced carbon deposition rate, improved stability, and a large number of active sites, avoiding acetylene byproducts and enhancing the activity and stability of the R152a defluorination reaction.
Smart Images

Figure CN118904365A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fluorine chemical industry, and specifically relates to the technology of industrial production of polyvinylidene fluoride. Background Art
[0002] Polyvinylidene fluoride has a wide range of applications in building materials, chemical equipment, computers, and aerospace. It is mainly produced by the polymerization of vinyl fluoride (VF). At present, the main technical routes for the industrial production of polyvinylidene fluoride (PVF) include the reaction of acetylene with hydrogen fluoride and the dehydrofluorination reaction of 1,1-difluoroethane (R152a). Among them, R152a is mainly involved in the fields of refrigerants and foaming agents. In recent years, its production capacity has increased rapidly, resulting in market supply significantly exceeding demand. In addition, due to the high greenhouse effect potential (GWP) of R152a, this substance is listed as one of the gases that should be controlled in the Kyoto Protocol. Therefore, the technical route of producing VF by dehydrofluorination of R152a has become a highly-regarded alternative. This method can not only reduce the demand for R152a, but also help reduce greenhouse gas emissions, thereby mitigating adverse effects on the environment.
[0003] The mainstream catalysts for this reaction are Al-based, Cr-based, and Mg-based. Among them, Al-based catalysts have been widely studied for their relatively low cost, good stability, and high catalytic activity. In addition, compared with the sintering deactivation of Mg-based catalysts, Al-based catalysts are mainly affected by carbon deposition deactivation, so they can be restored to activity by air roasting, which is conducive to the recycling of catalysts. Studies have pointed out that the Lewis acid sites in Al-based catalysts are the main active sites. The strength of the Lewis acid sites is positively correlated with the activity of the catalyst, but acid sites with too high strength may lead to the production of by-products such as acetylene and promote the formation of carbon deposits. Therefore, the rational control of the Lewis acid sites of Al-based catalysts is crucial to ensure the efficient progress of the reaction. Summary of the invention
[0004] In view of the defects of the prior art, the present invention provides a method for preparing an Al-based catalyst to solve the problem of how to reasonably control the Lewis acid sites of the Al-based catalyst.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A method for preparing an Al-based catalyst comprises the following steps:
[0007] Step 1: mixing an aluminum precursor solution and an alkaline precipitant solution and stirring them to react, controlling the pH value of the mixed solution to be constant at alkaline during the reaction, and reacting to obtain an aluminum-containing precipitate; aging for a set time after the reaction is completed, and then filtering, washing, drying, and roasting to obtain a solid product;
[0008] Step 2: The solid product obtained in step 1 is subjected to a liquid-solid mixed reaction with hydrofluoric acid, and the mixture is allowed to stand for a set time to obtain a precipitate. The obtained precipitate is filtered, washed, dried, and calcined to obtain the final product, an aluminum-based catalyst.
[0009] Preferably, the aluminum precursor is any one of Al(NO3)2·9H2O, AlCl3·6H2O, and Al2(SO4)3·18H2O.
[0010] Preferably, the alkaline precipitant is one of ammonia water, Na2CO3, and NaOH, or a mixture of any two or more thereof.
[0011] Preferably, during the reaction process of step 1, the pH value of the mixed solution is controlled in the range of 9 to 11.
[0012] Preferably, the calcination temperature in step 1 is 100-800° C., and the calcination atmosphere is air or nitrogen.
[0013] Preferably, the calcination temperature in step 2 is 400-700° C., the calcination atmosphere is air or nitrogen, and the calcination time is 2-24 hours.
[0014] Preferably, the mass concentration of hydrofluoric acid in step 2 is 10-50wt%.
[0015] Preferably, the aluminum-based catalyst produced in step 2 is AlF2(OH).
[0016] Preferably, in step 2, the yield of AlF2(OH) is controlled by changing the amount of hydrofluoric acid used.
[0017] The present invention also provides an Al-based catalyst application method, wherein the Al-based catalyst prepared by the Al-based catalyst preparation method is used as a catalyst for preparing VF by dehydrofluorination reaction of R152a.
[0018] The present invention adopts the above technical solution and has the following beneficial effects:
[0019] In step 1, an aluminum precursor solution and an alkaline precipitant solution are mixed and reacted, and then filtered, washed, dried, and calcined to obtain a solid product. In step 2, the solid product obtained in step 1 is mixed and reacted with hydrofluoric acid in a liquid-solid manner, and then filtered, washed, dried, and calcined to obtain a final product, an aluminum-based catalyst. In the prepared Al-based catalyst, one -F is replaced by -OH, so that its Lewis acid strength is moderate, mainly weak acid and medium acid, which greatly reduces the rate of catalyst carbon deposition, thereby enhancing the stability of the catalyst.
[0020] Since the Al-based catalyst rich in AlF2(OH) phase has a higher specific surface area, the high specific surface area of the Al-based catalyst also makes it have a large number of active sites.
[0021] Since the Al-based catalyst is prepared by a precipitation method and has no by-products, it has the characteristics of simple operation, low cost and environmental friendliness.
[0022] Since the Al-based catalyst has moderate Lewis acid strength and a large number of active sites, it has excellent activity and stability in catalyzing the dehydrofluorination of 1,1-difluoroethane (R152a) to prepare vinyl fluoride (VF), avoiding the production of by-products such as acetylene and promoting the formation of carbon deposits.
[0023] The specific technical solutions and beneficial effects of the present invention will be described in detail in the following specific embodiments in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments:
[0025] Figure 1 XRD spectrum of the catalyst of the embodiment of the present invention;
[0026] Figure 2 NH3-TPD characterization diagram of the catalyst of the embodiment of the present invention;
[0027] Figure 3 Lifetime diagram of the reaction of producing VF by dehydrofluorination of R152a catalyzed by the catalyst of the embodiment of the present invention. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] Those skilled in the art will appreciate that, in the absence of conflict, the features in the following embodiments and implementations may be combined with each other.
[0030] The present invention relates to a method for preparing an Al-based catalyst rich in AlF2(OH) phase and application thereof, wherein the method for preparing an Al-based catalyst comprises the following steps:
[0031] Step 1: mixing an aluminum precursor solution and an alkaline precipitant solution and stirring them to react, controlling the pH value of the mixed solution to be constant at alkaline during the reaction, and reacting to obtain an aluminum-containing precipitate; aging for a set time after the reaction is completed, and then filtering, washing, drying, and roasting to obtain a solid product;
[0032] Step 2: The solid product obtained in step 1 is subjected to a liquid-solid mixed reaction with hydrofluoric acid, and the mixture is allowed to stand for a set time to obtain a precipitate. The obtained precipitate is filtered, washed, dried, and calcined to obtain the final product, an aluminum-based catalyst.
[0033] In the Al-based catalyst prepared by the above method, one -F is replaced by -OH, so its Lewis acid strength is moderate, mainly weak acid and medium acid, which greatly reduces the rate of catalyst carbon deposition, thereby enhancing the stability of the catalyst.
[0034] Since the Al-based catalyst rich in AlF2(OH) phase has a higher specific surface area, the high specific surface area of the Al-based catalyst also makes it have a large number of active sites.
[0035] Since the Al-based catalyst is prepared by a precipitation method and has no by-products, it has the characteristics of simple operation, low cost and environmental friendliness.
[0036] Preferably, the aluminum precursor is any one of Al(NO3)2·9H2O, AlCl3·6H2O, and Al2(SO4)3·18H2O. The alkaline precipitant is one of ammonia water, Na2CO3, and NaOH, or a mixture of any two or more thereof. Of course, other aluminum precursors and alkaline precipitants are not excluded.
[0037] During the reaction of step 1, the pH value of the mixed solution is controlled to be in the range of 9 to 11, for example, 9, 10, 11. This is conducive to controlling the reaction process and obtaining an aluminum-containing precipitate. The calcination temperature of step 1 is 100 to 800°C, for example, 400°C, 500°C, 700°C, and the calcination atmosphere is air or nitrogen. The calcination temperature of step 2 is 400 to 700°C, for example, 400°C, 500°C, 700°C, and the calcination atmosphere is air or nitrogen, and the calcination time is 2 to 24 hours.
[0038] In addition, the mass concentration of hydrofluoric acid in step 2 is 10-50 wt%. The aluminum-based catalyst produced in step 2 is AlF2(OH). It is understood that the yield of AlF2(OH) can be controlled by changing the amount of hydrofluoric acid used.
[0039] An Al-based catalyst application method is disclosed, wherein the Al-based catalyst prepared by the Al-based catalyst preparation method is used as a catalyst for preparing VF by dehydrofluorination reaction of R152a.
[0040] Since the Al-based catalyst has moderate Lewis acid strength and a large number of active sites, the Al-based catalyst has excellent activity and stability in catalyzing the dehydrofluorination of 1,1-difluoroethane (R152a) to prepare vinyl fluoride (VF), avoiding the generation of by-products such as acetylene and promoting the formation of carbon deposits.
[0041] The technical solution of the present invention is described below in conjunction with specific embodiments.
[0042] Example 1
[0043] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M ammonia water as solution B. Solution A and solution B are precipitated in a three-necked flask by co-dropping method, with magnetic stirring speed of 800r / min, and pH is controlled by pH meter to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the end, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid.
[0044] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 7.7g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 400°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0045] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 93.7% and the selectivity of VF was 98.3%.
[0046] Example 2
[0047] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M ammonia water as solution B. Solution A and solution B are precipitated in a three-necked flask by co-dropping method, with magnetic stirring speed of 800r / min, and pH is controlled by pH meter to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the end, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid.
[0048] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 7.7g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0049] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 94.9% and the selectivity of VF was 99.0%.
[0050] Example 3
[0051] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M ammonia water as solution B. Solution A and solution B are precipitated in a three-necked flask by co-dropping method, with magnetic stirring speed of 800r / min, and pH is controlled by pH meter to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the end, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid.
[0052] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 7.7g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 600°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0053] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 88.6% and the selectivity of VF was 98.9%.
[0054] Example 4
[0055] 17.4g aluminum chloride hexahydrate (AlCl3·6H2O) was dissolved in 100mL water and recorded as solution A. 1M ammonia water was prepared and recorded as solution B. Solution A and solution B were precipitated by co-dropping in a three-necked flask. The magnetic stirring speed was 800r / min. The pH was controlled to be constant at 9.5 by a pH meter during the process. After the addition was completed, stirring was continued for 30min, and then aging was performed for 24h. After completion, the precipitated solid was obtained by filtering, washing and drying in an oven at 120℃.
[0056] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 7.7g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0057] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 93.6%, and the selectivity of VF was 98.5%.
[0058] Example 5
[0059] Dissolve 66.6g of aluminum sulfate 18hydrate (Al2(SO4)3·18H2O) in 100mL of water as solution A, and prepare 1M ammonia water as solution B. Solution A and solution B are precipitated by co-dropping in a three-necked flask, with a magnetic stirring speed of 800r / min, and a pH meter is used to control the pH to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the addition, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid.
[0060] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 11.8g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0061] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 84.5%, and the selectivity of VF was 98.1%.
[0062] Example 6
[0063] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M ammonia water as solution B. Solution A and solution B were precipitated by co-dropping in a three-necked flask, with a magnetic stirring speed of 800r / min, and a pH meter was used to control the pH to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the addition, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid, which was then air-roasted in a muffle furnace at 500℃ for 8h.
[0064] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 11.8g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0065] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 94.5%, and the selectivity of VF was 97.8%.
[0066] Example 7
[0067] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M ammonia water as solution B. Solution A and solution B are precipitated by co-dropping in a three-necked flask, with a magnetic stirring speed of 800r / min, and a pH meter is used to control the pH to be constant at 10.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the addition, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid.
[0068] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 7.7g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0069] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 95.1%, and the selectivity of VF was 98.9%.
[0070] Example 8
[0071] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M NaOH solution as solution B. Solution A and solution B are precipitated in a three-necked flask by co-dropping method, with magnetic stirring speed of 800r / min, and pH is controlled by pH meter to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the end, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid.
[0072] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 7.7g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0073] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 90.5%, and the selectivity of VF was 98.2%.
[0074] Example 9
[0075] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M sodium carbonate solution (Na2CO3) as solution B. Solution A and solution B are precipitated by co-dropping in a three-necked flask, with a magnetic stirring speed of 800r / min, and a pH meter is used to control the pH to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the addition, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid.
[0076] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 7.7g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0077] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 92.8%, and the selectivity of VF was 98.4%.
[0078] Example 10
[0079] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M NaOH solution as solution B. Solution A and solution B were precipitated by co-dropping in a three-necked flask, with a magnetic stirring speed of 800r / min, and a pH meter was used to control the pH to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the addition, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid, which was then calcined in a muffle furnace at 500℃ for 8h.
[0080] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 11.8g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0081] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 84.6% and the selectivity of VF was 98.3%.
[0082] Embodiment 11
[0083] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M ammonia water as solution B. Solution A and solution B were precipitated by co-dropping in a three-necked flask, with a magnetic stirring speed of 800r / min, and a pH meter was used to control the pH to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the addition, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid, which was then air-roasted in a muffle furnace at 900℃ for 8h.
[0084] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 11.8g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in a muffle furnace under nitrogen atmosphere, and obtain an aluminum-based catalyst after cooling.
[0085] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 79.7% and the selectivity of VF was 98.9%.
[0086] Example 12
[0087] Dissolve 37.5g of aluminum nitrate nonahydrate (Al(NO3)3·6H2O) in 100mL of water as solution A, and prepare 1M ammonia water as solution B. Solution A and solution B were precipitated by co-dropping in a three-necked flask, with a magnetic stirring speed of 800r / min, and a pH meter was used to control the pH to be constant at 9.5 during the process. Continue stirring for 30min after the addition, and then age for 24h. After the addition, filter, wash and dry in an oven at 120℃ to obtain a precipitated solid, which was then calcined in a muffle furnace at 500℃ for 8h.
[0088] Take 5.0g of the above precipitated solid and put it in a plastic beaker, add 11.8g of hydrofluoric acid (50wt%) solution dropwise into the plastic beaker, filter and wash after the fluorination is completed, and calcine at 500°C for 4h in an air atmosphere in a muffle furnace, and obtain an aluminum-based catalyst after cooling.
[0089] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 85.2% and the selectivity of VF was 98.5%.
[0090] Comparative Example 13
[0091] A commercial aluminum fluoride catalyst was purchased, calcined at 500°C for 4 h in a nitrogen atmosphere in a muffle furnace, and then cooled to obtain an aluminum-based catalyst.
[0092] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 85.7% and the selectivity of VF was 96.7%.
[0093] Comparative Example 14
[0094] A commercial gamma alumina catalyst was purchased, calcined at 500°C for 4 h in a nitrogen atmosphere in a muffle furnace, and then cooled to obtain an aluminum-based catalyst.
[0095] The aluminum-based catalyst prepared as above was applied to the reaction of removing HF from R152a to produce VF, and the conversion rate of R152a was 93.9% and the selectivity of VF was 96.5%.
[0096] Figure 1 The XRD characterization diagrams of the catalysts of some embodiments of the present invention show that the Al-based catalyst contains AlF3 crystal phase and AlF2(OH) crystal phase, and has different contents of AlF2(OH) crystal phase under different synthesis conditions.
[0097] Figure 2 This is the NH3-TPD characterization diagram of the catalyst of Example 2 of the present invention. From the data in the figure, it can be seen that the Lewis acid strength is 194.4°C and 163.9°C, which corresponds to Lewis weak acid and Lewis medium acid, respectively. Studies have shown that Lewis strong acid sites are the center of catalyst carbon deposition. Compared with the traditional aluminum fluoride catalyst with Lewis strong acid sites, the catalyst of the embodiment of the present invention reduces the catalyst carbon deposition efficiency and slows down the catalyst deactivation rate. The catalyst of the embodiment of the present invention has better stability.
[0098] Figure 3 This is a life experiment diagram of the catalyst of Example 2 of the present invention in the reaction of removing HF from R152a to produce VF. The reaction conditions are: 20 ml of a catalyst with a mesh size of 20-40 is loaded into a fixed bed reaction tube, the flow rate of R152a gas is set to 6000 mL / h and diluted with nitrogen, the temperature is set to 300°C, and the relationship between the R152a conversion rate and the reaction time is explored. It can be seen from the figure that the catalyst of Example 2 of the present invention has not been deactivated for 1500 hours in the life experiment, indicating that the catalyst has good stability.
[0099] Table 1 Example Catalyst R152a Dehydrofluorination to VF Reaction Activity Table
[0100]
[0101] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.
Claims
1. A method for preparing an Al-based catalyst, characterized in that: The steps include: Step 1: mixing an aluminum precursor solution and an alkaline precipitant solution and stirring them to react, controlling the pH value of the mixed solution to be constant at alkaline during the reaction, and reacting to obtain an aluminum-containing precipitate; aging for a set time after the reaction is completed, and then filtering, washing, drying, and roasting to obtain a solid product; Step 2: The solid product obtained in step 1 is subjected to a liquid-solid mixed reaction with hydrofluoric acid, and the mixture is allowed to stand for a set time to obtain a precipitate. The obtained precipitate is filtered, washed, dried, and calcined to obtain the final product, an aluminum-based catalyst.
2. The method for preparing an Al-based catalyst according to claim 1, characterized in that: The aluminum precursor is any one of Al(NO3)2·9H2O, AlCl3·6H2O, and Al2(SO4)3·18H2O.
3. The method for preparing an Al-based catalyst according to claim 1, characterized in that: The alkaline precipitant is one of ammonia water, Na2CO3, and NaOH, or a mixture of any two or more thereof.
4. The method for preparing an Al-based catalyst according to claim 1, characterized in that: In step 1, during the reaction process, the pH value of the mixed solution is controlled to be in the range of 9 to 11.
5. The method for preparing an Al-based catalyst according to claim 1, characterized in that: Step 1: The calcination temperature is 100-800° C., and the calcination atmosphere is air or nitrogen.
6. The method for preparing an Al-based catalyst according to claim 1, characterized in that: Step 2: The calcination temperature is 400-700° C., the calcination atmosphere is air or nitrogen, and the calcination time is 2-24 hours.
7. The method for preparing an Al-based catalyst according to claim 1, characterized in that: In step 2, the mass concentration of hydrofluoric acid is 10-50wt%.
8. The method for preparing an Al-based catalyst according to claim 7, characterized in that: The aluminum-based catalyst produced in step 2 is AlF2(OH).
9. The method for preparing an Al-based catalyst according to claim 8, characterized in that: In step 2, the yield of AlF2(OH) is controlled by changing the amount of hydrofluoric acid.
10. A method for applying an AL-based catalyst, characterized in that: The Al-based catalyst prepared by the Al-based catalyst preparation method according to any one of claims 1 to 9 is used as a catalyst for preparing VF by dehydrofluorination reaction of R152a.
Citation Information
Patent Citations
High pore volume gamma-aluminium oxide and preparation method therefor
CN105060323A
Preparation method of nanometer aluminum fluoride-based catalyst
CN105597795A
Catalyst for generating trifluoroethylene from 1, 1, 1, 2-tetrafluoroethane by means of catalytic pyrolysis and in-situ regeneration method
CN106000428A
Aluminum fluorosulfate catalyst as well as preparation method and application thereof
CN113385201A
Defective AlF3 catalyst as well as preparation method and application thereof